A multifunctional polyester fiber based on modified bamboo charcoal and preparation method thereof

By surface modification and treatment of nano bamboo charcoal, multifunctional bamboo charcoal and polyester material blended into a blended wire, solving the problems of poor compatibility and flammability of nanoceramic powder and polyester fiber, improving far-infrared, anti-static and Flame retardant properties have expanded the application of fiber in fillers and indoor home furnishings.

CN118600584BActive Publication Date: 2024-11-29江苏海科纤维有限公司
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410768796.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-11-29
Estimated Expiration
2044-06-14

AI Technical Summary

Technical Problem

The poor compatibility of nanoceramic powders and polyester in existing far-infrared antistatic fiber materials leads to difficulties in spinning, and the polyester fibers are flammable and have insufficient flame retardant properties, limiting their application in fillers and indoor home furnishings.

Method used

The nano bamboo charcoal was surface modified by in-situ polymerization method, and treated with phosphorus oxychloride, para-hydroxyphenylethanol and methanol to form multifunctional bamboo charcoal, and then melt blended with polyester material, and prepared based on modification Multifunctional polyester fiber of bamboo charcoal.

Benefits of technology

It improves the far-infrared emission, antistatic properties and flame retardant properties of the fiber, and enhances the application potential of fiber in the fields of fillers and indoor homes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118600584B_ABST
    Figure CN118600584B_ABST
Patent Text Reader

Abstract

The invention relates to a multifunctional polyester fiber based on modified bamboo charcoal and a preparation method thereof, and belongs to the technical field of functional fibers. The preparation method of the invention comprises the following steps: S1, under the action of a catalyst, nano bamboo charcoal, aniline and polyaniline dopant react in water to obtain polyaniline modified bamboo charcoal; S2, polyaniline modified bamboo charcoal is dispersed in a solvent, phosphorus oxychloride, p-hydroxyphenylethanol and methanol are successively added to react to obtain multifunctional bamboo charcoal; S3, multifunctional bamboo charcoal and polyester powder are granulated to obtain multifunctional polyester masterbatch; S4, multifunctional polyester masterbatch and polyester slice are spun to obtain the multifunctional polyester fiber based on modified bamboo charcoal, which has high far-infrared emission performance, far-infrared radiation heating performance, antistatic performance and flame retardant performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional fibers, and in particular relates to a multifunctional polyester fiber based on modified bamboo charcoal and a preparation method thereof. Background Art

[0002] With the rapid improvement of living standards, people have higher and higher requirements for safety, environmental protection and health care. Far-infrared antistatic polyester fiber has good thermal insulation and health care functions, which meets people's needs. At present, far-infrared antistatic fibers are often prepared using nano-ceramic powders, graphene and other materials as functional additives. However, nano-powders have high surface energy and poor compatibility with polyester. They are easy to agglomerate in polyester fibers, resulting in difficulties in spinning and even damage to spinning equipment. In addition, polyester fibers are extremely flammable, and the droplet phenomenon is serious during the combustion process, which seriously limits their application in fillings, indoor furniture and other fields.

[0003] References (Sun Haibo, Wang Shuangcheng, Ma Junqiang, et al. Preparation and properties of biomass graphene modified regenerated polyester fiber [J]. Cotton Textile Technology, 2019, 47(12): 6-8; Wang Shuangcheng, Ma Junqiang. Preparation and application of biomass graphene inner warm fleece [C]. / / "Hengtian Lixin Cup" 29th (2016) National Knitting Dyeing and Finishing Academic Seminar Proceedings. 2016: 4-6.) Graphene-modified regenerated polyester fiber was prepared by polymer melt blending spinning method, which improved the antibacterial and far-infrared properties of polyester fiber; however, the cost of graphene is extremely high, and there are still major problems in the mass production of graphene. Its products are mainly based on graphite flakes, and graphene is very easy to agglomerate due to its special hierarchical structure, resulting in uneven dispersion in the fiber, which limits the application of graphene in polyester fibers.

[0004] Nano bamboo charcoal is a porous material formed by high-temperature carbonization of native bamboo. It has a hard texture, fine and porous texture, and strong adsorption capacity. Nano bamboo charcoal has good antibacterial properties and far-infrared temperature regulation properties. The raw materials are easily available and inexpensive, and it has also been widely used in the field of textiles. References (Zhuang Rong. Preparation and capacitance energy storage performance of manganese oxide aerogel composites [D]. Beijing: Beijing University of Chemical Technology, 2020.) Bamboo-based activated carbon was modified by in-situ polymerization in an ice-water bath to prepare bamboo-based activated carbon / polyaniline composites. References (Sun Kang, Jiang Jianchun, Lu Xincheng, et al. Preparation of surface nitrogen-doped activated carbon and study on its formaldehyde adsorption performance [J]. Chemistry and Industry of Forest Products, 2014, 34 (4): 77-82.) Aniline was used as a nitrogen source, and nitrogen-doped activated carbon was prepared by in-situ polymerization and carbonization on the surface of activated carbon, which improved the adsorption performance of activated carbon for formaldehyde. However, polyaniline-modified activated carbon still has poor compatibility with polyester fibers and cannot be directly used for melt-addition modification of polyester fibers; and polyaniline-modified activated carbon has poor flame retardant properties and cannot effectively improve the flame retardant and anti-melt dripping properties of polyester fabrics.

[0005] Based on the above background, the development of multifunctional polyester fiber based on bamboo charcoal has great market prospects. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides a multifunctional polyester fiber based on modified bamboo charcoal and a preparation method thereof, firstly, the surface of nano bamboo charcoal is modified by in-situ polymerization using polyaniline, then the modified bamboo charcoal is treated with phosphorus oxychloride, p-hydroxyphenylethanol and methanol in sequence to obtain multifunctional bamboo charcoal. Finally, the multifunctional bamboo charcoal and polyester material are granulated by melt blending and spun by melt spinning to prepare multifunctional polyester fiber based on modified bamboo charcoal.

[0007] The first object of the present invention is to provide a method for preparing a multifunctional polyester fiber based on modified bamboo charcoal, comprising the following steps:

[0008] S1. Under the action of a catalyst, nano bamboo charcoal, aniline and polyaniline dopant react in water to obtain polyaniline modified bamboo charcoal;

[0009] S2, dispersing the polyaniline modified bamboo charcoal described in S1 in a solvent, and successively adding phosphorus oxychloride, p-hydroxyphenylethanol and methanol to react to obtain multifunctional bamboo charcoal;

[0010] S3, granulating the multifunctional bamboo charcoal and polyester powder described in S2 to obtain multifunctional polyester masterbatch;

[0011] S4, spinning the multifunctional polyester masterbatch and polyester chips described in S3 to obtain the multifunctional polyester fiber based on modified bamboo charcoal.

[0012] In one embodiment of the present invention, in S1, the catalyst is selected from ammonium persulfate and / or sodium periodate; and the polyaniline dopant is selected from phosphoric acid.

[0013] In one embodiment of the present invention, in S1, the mass ratio of the nano bamboo charcoal to aniline is 4-5:1, the molar ratio of aniline to aniline dopant is 7-10:1, and the molar ratio of aniline to catalyst is 1:1-1.2.

[0014] In one embodiment of the present invention, in S1, the reaction temperature is 10°C-35°C, the reaction time is 3h-5h, if the reaction time is too short, the modification is incomplete, and if the reaction time is too long, it is wasted. Within the provided time range, polyaniline can be generated on the surface of nano bamboo charcoal; polyaniline modification can increase the content of active amino groups on the surface of nano bamboo charcoal, improve the reaction performance, conductivity and antistatic properties of the material.

[0015] In one embodiment of the present invention, in S2, the molar ratio of the polyaniline-modified bamboo charcoal, phosphorus oxychloride, p-hydroxyphenylethanol and methanol is 3-3.5:1:2-2.2:0.5-1.

[0016] In one embodiment of the present invention, in S2, the reaction temperature after adding phosphorus oxychloride is 10°C-20°C, the reaction time is 4h-5h, and the amino group rich on the surface of polyaniline-modified nano bamboo charcoal can undergo nucleophilic substitution reaction with the active chlorine of phosphorus oxychloride, so that the first active chlorine of phosphorus oxychloride participates in the reaction; the reaction temperature after adding p-hydroxyphenylethanol is 35°C-40°C, and the reaction time is 3h-4h. Theoretically, two moles of p-hydroxyphenylethanol react with one mole of the remaining active chlorine of phosphorus oxychloride. The aliphatic terminal hydroxyl group of p-hydroxyphenylethanol has high reactivity with phosphorus oxychloride and small steric hindrance, and preferentially reacts with the active chlorine of phosphorus oxychloride; methanol is added to continue the reaction for 1h-2h to cap the active chlorine that does not participate in the reaction.

[0017] In one embodiment of the present invention, in S2, the solvent is selected from one or more of chloroform, dichloromethane and tetrahydrofuran.

[0018] Furthermore, in S2, the solvent is chloroform.

[0019] In one embodiment of the present invention, before S3, the step of drying the multifunctional bamboo charcoal and the polyester powder is also included, the drying temperature of the multifunctional bamboo charcoal is 60°C-80°C, for example, it can be 60°C, 61°C, 62°C, 63°C, 64°C, 65°C, 66°C, 67°C, 68°C, 69°C, 70°C, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C, 80°C; the drying time is 7h-9h, for example, it can be 7h, 8h, 9h; the drying temperature of the polyester powder is 120°C-130°C, for example, it can be 120°C, 121°C, 122°C, 123°C, 124°C, 125°C, 126°C, 127°C, 128°C, 129°C, 130°C; the time is 10h-12h, for example, it can be 10h, 11h, 12h.

[0020] In one embodiment of the present invention, in S3, the granulation is performed by melt blending, extrusion molding, cooling and pelletizing through a twin-screw extruder; the granulation temperature is 255°C-270°C; if the processing temperature is too low, the multifunctional bamboo charcoal and polyester powder cannot be mixed evenly, which is not conducive to granulation, and if the temperature is too high, it will cause energy waste.

[0021] In one embodiment of the present invention, in S3, the mass fraction of the multifunctional bamboo charcoal in the multifunctional polyester masterbatch is 25%-30%, for example, it can be 25%, 26%, 27%, 28%, 29%, or 30%.

[0022] In one embodiment of the present invention, before S4, it also includes a step of drying the multifunctional polyester masterbatch and polyester chips, wherein the drying is performed by pre-crystallization at 90°C-110°C for 3h-4h, and then drying at 120°C-140°C for 10h-15h to ensure that the final moisture content of the multifunctional polyester masterbatch and polyester chips is less than 100ppm.

[0023] In one embodiment of the present invention, in S4, the spinning is performed by a melt spinning machine, followed by oiling, pre-stretching, winding, and stretching; the spinning process parameters are: a speed of 2500m / min-2800m / min, a temperature of 280℃-290℃, and a pulling ratio of 1.5-2.

[0024] In one embodiment of the present invention, in S4, the mass fraction of the multifunctional polyester masterbatch in the multifunctional polyester fiber based on modified bamboo charcoal is 15%-20%, for example, it can be 15%, 16%, 17%, 18%, 19%, or 20%.

[0025] The second object of the present invention is to provide a multifunctional polyester fiber based on modified bamboo charcoal prepared by the method described above.

[0026] In one embodiment of the present invention, the far-infrared normal emissivity of the multifunctional polyester fiber based on modified bamboo charcoal is 0.91-0.93, the far-infrared radiation temperature rise is 2.5°C-3.2°C, the surface temperature rise is 20.5°C-23.9°C higher than that of ordinary fibers, the antistatic property reaches Class A, the limiting oxygen index is 29.2%-32.3%, and the breaking strength is 3.2cN / detx-3.4cN / detx.

[0027] The technical solution of the present invention has the following advantages over the prior art:

[0028] (1) The preparation method of the present invention uses polyaniline to modify the surface of nano bamboo charcoal particles through an in-situ polymerization method, so that the surface of the nano bamboo charcoal is rich in amino groups. The surface of the modified nano bamboo charcoal is rough, which helps to enhance the far-infrared emission performance of the nano bamboo charcoal. The polyaniline structure has strong conductive properties, so the modified nano bamboo charcoal has excellent far-infrared performance and antistatic properties.

[0029] (2) The three active chlorines of phosphorus oxychloride used in the preparation method of the present invention have different reaction temperatures, and the ratio between the reactants and the reaction temperature are controlled so that phosphorus oxychloride is grafted on the polyaniline-modified nano bamboo charcoal, and then p-hydroxyphenylethanol and methanol are used in sequence for grafting reaction; in addition to the above-mentioned covalent bond binding, p-hydroxyphenylethanol can also be combined with the polyaniline on the surface of the nano bamboo charcoal through π-π stacking, so the phosphate structure, p-hydroxyphenylethanol and polyaniline-modified nano bamboo charcoal have excellent binding ability, so as to be coated on the surface of the nano bamboo charcoal, and the outer layer of p-hydroxyphenylethanol has good compatibility with polyester and is evenly dispersed in the polyester fiber, which not only has high functionality, but also has less damage to the strength performance of the polyester fiber.

[0030] (3) The phosphate ester structure in the multifunctional bamboo charcoal prepared by the method of the present invention and the doped phosphoric acid of polyaniline can act as an acid source, the polyaniline rich in nitrogen can act as a gas source, the polyaniline and p-hydroxyphenylethanol rich in aromatic structure and the nano bamboo charcoal can act as a carbon source, so the components in the multifunctional bamboo charcoal can synergistically construct an intumescent flame retardant system with high flame retardant efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:

[0032] Figure 1 This is a schematic diagram of the structure of the multifunctional bamboo charcoal according to Example 1 of the present invention;

[0033] Figure 2 This is a temperature difference curve of the near-infrared heat storage test of the modified polyester fiber and the unmodified polyester fiber in Test Example 1 of the present invention. DETAILED DESCRIPTION

[0034] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. It should be understood that the specific embodiments are only used to explain the present invention, but the embodiments are not intended to limit the present invention.

[0035] In the present invention, unless otherwise explained, technical and scientific terms used in the present invention have the same meanings as commonly understood by those skilled in the art to which the present invention belongs.

[0036] In the present invention, unless otherwise stated, the term "and / or" used in the present invention includes any and all combinations of one or more of the associated listed items.

[0037] In the present invention, unless otherwise stated, the experimental methods used in the embodiments of the present invention are conventional methods unless otherwise stated, and the materials, reagents, etc. used are all commercially available unless otherwise stated.

[0038] In the present invention, unless otherwise specified, the nano bamboo charcoal used in the embodiments of the present invention is purchased from Hunan Chuangchun New Materials Co., Ltd., and the particle size is 100nm-300nm.

[0039] Example 1

[0040] The multifunctional polyester fiber based on modified bamboo charcoal and the preparation method thereof of this embodiment specifically include the following steps:

[0041] S1. Adding nano bamboo charcoal to an aqueous solution containing aniline and phosphoric acid, ultrasonically dispersing for 1.5 hours, then adding ammonium persulfate to react at 25° C. for 4 hours, centrifuging, washing with water and ethanol three times in sequence, and drying to obtain polyaniline modified bamboo charcoal powder; wherein the mass ratio of nano bamboo charcoal to aniline is 4.5:1, the molar ratio of aniline to aniline dopant is 9:1, and the molar ratio of aniline to catalyst is 1:1.1;

[0042] S2, polyaniline modified bamboo charcoal powder and chloroform were mixed at a mass ratio of 1:35, chloroform solution of phosphorus oxychloride (the mass ratio of phosphorus oxychloride to chloroform was 1:8) was added dropwise, and the mixture was reacted at 15°C for 4.5h, and then p-hydroxyphenylethanol ether solution (the mass ratio of p-hydroxyphenylethanol to ether was 1:25) was added and the mixture was reacted at 38°C for 3.5h; finally, methanol was added and the reaction was continued for 1.5h, and the multifunctional bamboo charcoal powder ( Figure 1 ); wherein the molar ratio of polyaniline-modified bamboo charcoal, phosphorus oxychloride, p-hydroxyphenylethanol and methanol is 3.3:1:2.1:0.8;

[0043] S3, the multifunctional bamboo charcoal powder was vacuum dried at 70°C for 8h; the polyester powder was vacuum dried at 125°C for 11h, and after mixing, melt blending, extrusion molding, cooling and pelletizing were carried out by a twin-screw extruder, and the temperature of the twin-screw extruder was 265°C to obtain a multifunctional polyester masterbatch with a mass fraction of 28% of the multifunctional bamboo charcoal powder;

[0044] S4, the multifunctional polyester masterbatch and the polyester chips were pre-crystallized in a 100°C blast oven for 3.5 hours, and then dried at 130°C for 12 hours to make the final moisture content of the multifunctional polyester masterbatch and the polyester chips less than 100 ppm. After mixing, they were spun in a melt spinning machine, cooled and oiled, pre-stretched, wound and stretched. The speed of the melt spinning machine was 2650 m / min, the temperature was 285°C, and the pulling ratio was 1.8, to obtain a multifunctional polyester fiber based on modified bamboo charcoal with a mass fraction of 18% of the multifunctional polyester masterbatch.

[0045] Example 2

[0046] The multifunctional polyester fiber based on modified bamboo charcoal and the preparation method thereof of this embodiment specifically include the following steps:

[0047] S1. Adding nano bamboo charcoal to an aqueous solution containing aniline and phosphoric acid, ultrasonically dispersing for 1 hour, then adding sodium periodate to react at 10° C. for 5 hours, centrifuging, washing with water and ethanol three times in sequence, and drying to obtain polyaniline modified bamboo charcoal powder; wherein the mass ratio of nano bamboo charcoal to aniline is 4:1, the molar ratio of aniline to aniline dopant is 7:1, and the molar ratio of aniline to catalyst is 1:1;

[0048] S2, the polyaniline modified bamboo charcoal powder and chloroform are mixed in a mass ratio of 1:30, and a chloroform solution of phosphorus oxychloride (the mass ratio of phosphorus oxychloride to chloroform is 1:5) is added dropwise to react at 10°C for 5h, and then a p-hydroxyphenylethanol ether solution (the mass ratio of p-hydroxyphenylethanol to ether is 1:20) is added to react at 35°C for 4h; finally, methanol is added to continue the reaction for 2h, and the multifunctional bamboo charcoal powder is obtained by centrifugation, washing with ethanol and distilled water, and drying at 60°C for 6h; wherein the molar ratio of polyaniline modified bamboo charcoal, phosphorus oxychloride, p-hydroxyphenylethanol and methanol is 3:1:2:0.5;

[0049] S3, the multifunctional bamboo charcoal powder is vacuum dried at 60°C for 9h; the polyester powder is vacuum dried at 120°C for 12h, and after mixing, it is melt blended, extruded, cooled and pelletized by a twin-screw extruder, and the temperature of the twin-screw extruder is 255°C to obtain a multifunctional polyester masterbatch with a mass fraction of 25% of the multifunctional bamboo charcoal powder;

[0050] S4, the multifunctional polyester masterbatch and the polyester chips were pre-crystallized in a 90°C blast oven for 4 hours, and then continued to be dried at 120°C for 15 hours, so that the final moisture content of the multifunctional polyester masterbatch and the polyester chips was less than 100 ppm. After mixing, they were spun through a melt spinning machine, cooled and oiled, pre-stretched, wound, and stretched. The speed of the melt spinning machine was 2500 m / min, the temperature was 280°C, and the traction ratio was 1.5, to obtain a multifunctional polyester fiber based on modified bamboo charcoal with a mass fraction of 15% of the multifunctional polyester masterbatch.

[0051] Example 3

[0052] The multifunctional polyester fiber based on modified bamboo charcoal and the preparation method thereof of this embodiment specifically include the following steps:

[0053] S1. Adding nano bamboo charcoal to an aqueous solution containing aniline and phosphoric acid, ultrasonically dispersing for 2 hours, then adding ammonium persulfate to react at 35° C. for 3 hours, centrifuging, washing with water and ethanol three times in sequence, and drying to obtain polyaniline modified bamboo charcoal powder; wherein the mass ratio of nano bamboo charcoal to aniline is 5:1, the molar ratio of aniline to aniline dopant is 10:1, and the molar ratio of aniline to catalyst is 1:1.2;

[0054] S2, the polyaniline modified bamboo charcoal powder and chloroform are mixed in a mass ratio of 1:40, and a chloroform solution of phosphorus oxychloride (the mass ratio of phosphorus oxychloride to chloroform is 1:10) is added dropwise to react at 20°C for 4h, and then a p-hydroxyphenylethanol ether solution (the mass ratio of p-hydroxyphenylethanol to ether is 1:30) is added to react at 40°C for 3h; finally, methanol is added to continue the reaction for 1h, and the multifunctional bamboo charcoal powder is obtained by centrifugation, washing with ethanol and distilled water, and drying at 70°C for 5h; wherein the molar ratio of polyaniline modified bamboo charcoal, phosphorus oxychloride, p-hydroxyphenylethanol and methanol is 3.5:1:2.2:1;

[0055] S3, the multifunctional bamboo charcoal powder is vacuum dried at 80°C for 7h; the polyester powder is vacuum dried at 130°C for 10h, and after mixing, it is melt blended, extruded, cooled and pelletized by a twin-screw extruder, and the temperature of the twin-screw extruder is 270°C to obtain a multifunctional polyester masterbatch with a mass fraction of 30% of the multifunctional bamboo charcoal powder;

[0056] S4, the multifunctional polyester masterbatch and the polyester chips are pre-crystallized in a 110°C blast oven for 3 hours, and then dried at 140°C for 10 hours to make the final moisture content of the multifunctional polyester masterbatch and the polyester chips less than 100 ppm. After mixing, they are spun through a melt spinning machine, cooled and oiled, pre-stretched, wound, and stretched. The speed of the melt spinning machine is 2800 m / min, the temperature is 290°C, and the pulling ratio is 2, so as to obtain a multifunctional polyester fiber based on modified bamboo charcoal with a mass fraction of 20% of the multifunctional polyester masterbatch.

[0057] Comparative Example 1

[0058] The method is basically the same as Example 1, except that nano bamboo charcoal is directly used for granulation and spinning.

[0059] Comparative Example 2

[0060] The method is basically the same as Example 1, except that phosphoric acid is replaced by sulfuric acid when modifying the nano bamboo charcoal.

[0061] Comparative Example 3

[0062] The method is basically the same as Example 1, except that polyaniline-modified bamboo charcoal is directly used for granulation and spinning.

[0063] Comparative Example 4

[0064] The method is basically the same as Example 1, except that phosphorus oxychloride is directly used when treating the polyaniline-modified bamboo charcoal.

[0065] Comparative Example 5

[0066] The method is basically the same as Example 1, except that phosphorus oxychloride is replaced by phosphoric acid when treating the polyaniline-modified bamboo charcoal.

[0067] Test Example 1

[0068] The flame retardant properties of the multifunctional polyester fibers (modified polyester fibers) based on modified bamboo charcoal prepared in Examples 1-3 and Comparative Examples 1-5 were tested:

[0069] Far infrared performance: Refer to GB / T 30127-2013 "Testing and evaluation of far infrared performance of textiles" to test the far infrared emissivity and heating performance of modified polyester fiber;

[0070] Photothermal performance: Refer to GB / T 18319-2019 "Test method for photothermal performance of textiles" to test the photothermal performance of thermal insulation flame-retardant polyester fiber, with an irradiance of 150W / m 2 ;

[0071] Antistatic performance: Refer to GB / T 14342-2015 "Test method for specific electrical resistance of chemical staple fibers" to test the antistatic performance of modified polyester fibers;

[0072] Flame retardant properties: Refer to FZ / T 50017-2011 "Test method for flame retardant properties of polyester fibers - oxygen index method" to test the limiting oxygen index of the fiber;

[0073] Physical properties: Refer to GB / T 14344-2022 "Test method for tensile properties of chemical fiber filaments" to test the breaking strength of modified polyester fiber;

[0074] Figure 2 It is a near infrared light heat storage test curve diagram of the unmodified polyester fiber and the modified polyester fiber of Example 1;

[0075] Table 1 shows the relevant properties of the unmodified polyester fiber and the modified polyester fiber finally measured:

[0076] Table 1

[0077]

[0078] From Table 1 and Figure 2 It can be seen that the modified polyester fiber has higher far-infrared emission performance, far-infrared radiation heating performance, antistatic performance and flame retardant performance.

[0079] Compared with Comparative Example 1, the nano-bamboo charcoal-modified polyester fiber has better far-infrared and antistatic properties, but poor flame retardant properties and great damage to mechanical properties. This is because the nano-bamboo charcoal has poor compatibility with polyester fiber and does not have flame retardant function.

[0080] Compared with Comparative Example 2, by using sulfuric acid as the polyaniline dopant, the far-infrared emission performance, heating performance and antistatic performance of the modified polyester fiber are all good, but its flame retardant performance is reduced, which is because the flame retardant performance of the sulfuric acid dopant is not good;

[0081] Compared with Comparative Example 3, the far infrared and antistatic properties of the polyester fiber modified with polyaniline-modified nano-bamboo charcoal are better, but the flame retardant properties are poor and the mechanical properties are greatly damaged, because the polyaniline-modified nano-bamboo charcoal is not evenly dispersed in the polyester fiber and the flame retardant properties of polyaniline are not good;

[0082] Compared with Comparative Example 4, the modified nano bamboo charcoal was treated with phosphorus oxychloride only, and the flame retardant property of the modified polyester fiber was good, but the modified nano bamboo charcoal had poor compatibility with the polyester fiber and was unevenly dispersed, resulting in a decrease in its strength performance;

[0083] Compared with Comparative Example 5, phosphoric acid is used for modification and then p-hydroxyphenylethanol is used for treatment. Phosphoric acid and p-hydroxyphenylethanol cannot react with each other. Therefore, phosphoric acid, p-hydroxyphenylethanol and polyaniline modified bamboo charcoal are simply blended and combined, and have poor compatibility with polyester fibers and poor dispersibility in polyester fibers, resulting in reduced performance and serious damage to mechanical properties.

[0084] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.

Claims

1. A method for preparing multifunctional polyester fiber based on modified bamboo charcoal, characterized in that: The following steps are involved: S1. Under the action of a catalyst, nano bamboo charcoal, aniline and polyaniline dopant react in water to obtain polyaniline modified bamboo charcoal; The polyaniline dopant is selected from phosphoric acid; S2, dispersing the polyaniline modified bamboo charcoal described in S1 in a solvent, and successively adding phosphorus oxychloride, p-hydroxyphenylethanol and methanol to react to obtain multifunctional bamboo charcoal; wherein the reaction temperature after adding phosphorus oxychloride is 10°C-20°C, and the reaction time is 4h-5h; the reaction temperature after adding p-hydroxyphenylethanol is 35°C-40°C, and the reaction time is 3h-4h; finally, methanol is added to continue the reaction for 1h-2h; the molar ratio of the polyaniline modified bamboo charcoal, phosphorus oxychloride, p-hydroxyphenylethanol and methanol is 3-3.5:1:2-2.2:0.5-1; S3, granulating the multifunctional bamboo charcoal and polyester powder described in S2 to obtain multifunctional polyester masterbatch; S4, spinning the multifunctional polyester masterbatch and polyester chips described in S3 to obtain the multifunctional polyester fiber based on modified bamboo charcoal.

2. The method for preparing multifunctional polyester fiber based on modified bamboo charcoal according to claim 1, characterized in that: In S1, the catalyst is selected from ammonium persulfate and / or sodium periodate.

3. The method for preparing multifunctional polyester fiber based on modified bamboo charcoal according to claim 1, characterized in that: In S1, the mass ratio of the nano bamboo charcoal to aniline is 4-5:1, the molar ratio of aniline to aniline dopant is 7-10:1, and the molar ratio of aniline to catalyst is 1:1-1.

2.

4. The method for preparing multifunctional polyester fiber based on modified bamboo charcoal according to claim 1, characterized in that: In S1, the reaction temperature is 10°C-35°C, and the reaction time is 3h-5h.

5. The method for preparing multifunctional polyester fiber based on modified bamboo charcoal according to claim 1, characterized in that: In S3, the granulation is performed by melt blending, extrusion molding, cooling and pelletizing through a twin-screw extruder; the granulation temperature is 255°C-270°C.

6. The method for preparing multifunctional polyester fiber based on modified bamboo charcoal according to claim 1, characterized in that: In S3, the mass fraction of the multifunctional bamboo charcoal in the multifunctional polyester masterbatch is 25%-30%.

7. The method for preparing multifunctional polyester fiber based on modified bamboo charcoal according to claim 1, characterized in that: In S4, the spinning is carried out by a melt spinning machine, followed by oiling after cooling, pre-stretching, winding, and stretching; the spinning process parameters are: speed of 2500m / min-2800m / min, temperature of 280℃-290℃, and traction ratio of 1.5-2.

8. The method for preparing multifunctional polyester fiber based on modified bamboo charcoal according to claim 1, characterized in that: In S4, the mass fraction of the multifunctional polyester masterbatch in the multifunctional polyester fiber based on modified bamboo charcoal is 15%-20%.

9. A multifunctional polyester fiber based on modified bamboo charcoal prepared by the method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Method for preparing bamboo charcoal / polyaniline composite material by adopting bamboo charcoal

    CN102134318A

  • Method for preparing bamboo charcoal and polyamide composite fibers by in situ polymerization

    CN102409424A

  • BC-PANI composite adsorbent for treating azo dye wastewater, and preparation method and applications thereof

    CN103007903A

  • Preparation method of polyaniline / active carbon fiber compound electrode material capable of being used as anode and cathode of capacitor simultaneously