High-performance corrugated paperboard with double corrugated paper core and production method thereof

By using a double-corrugated core structure and modified adhesive system, combined with composite particles of mesoporous cerium oxide and nickel-doped carbon dots, the mechanical strength, flame retardancy, and oxidation resistance of corrugated cardboard are improved, solving the problems of easy breakage and insufficient flame retardancy of traditional corrugated cardboard, extending its service life and providing a freshness preservation effect.

CN118600779BActive Publication Date: 2024-11-08JIANGSU SHENGSHENG PACKAGING CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410772993.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-11-08
Estimated Expiration
2044-06-17

AI Technical Summary

Technical Problem

Traditional corrugated cardboard is easily damaged during high-intensity transportation and use, has poor resistance to deformation, and lacks sufficient flame retardancy and oxidation resistance, resulting in a shortened service life.

Method used

The paperboard adopts a double corrugated core structure and uses modified adhesives and composite modified particles to enhance the interlayer bonding of the paperboard. The mechanical strength and flame retardant properties are improved by grafting mesoporous cerium oxide and nickel-doped carbon dots onto graphene oxide composite particles, and the dispersibility and antioxidant capacity are improved by silane coupling agent modification.

Benefits of technology

It significantly improves the mechanical strength and flame retardant properties of corrugated cardboard, extends its service life, and has antioxidant capabilities, making it suitable for packaging products that require preservation, such as fruits and vegetables.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118600779B_ABST
    Figure CN118600779B_ABST
Patent Text Reader

Abstract

The invention discloses a high-performance corrugated paperboard with a double corrugated paper core and a production method thereof, wherein the corrugated paperboard comprises a first surface paper layer, a first corrugated paper core layer, an intermediate paper layer, a second corrugated paper core layer and a second surface paper layer which are stacked in sequence, and adjacent layers are bonded by a modified adhesive; the modified adhesive comprises the following raw material components in parts by weight: 35-65 parts of bisphenol A epoxy resin, 13-42 parts of polyurethane acrylate oligomer, 4-17 parts of tackifying resin, 7.5-28 parts of composite modified particles, 0.6-2 parts of curing agent, and 14-50 parts of solvent. The corrugated paperboard prepared by the invention has high bursting strength, edge compression strength and bonding strength, excellent mechanical strength, and obvious flame retardant properties, and also has excellent antioxidant ability and ethylene removal ability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of corrugated paper, in particular to a high-performance corrugated paperboard with a double corrugated paper core and a production method thereof. Background Art

[0002] Corrugated cardboard is a multi-layer adhesive body, which consists of at least one layer of corrugated core paper (commonly known as "corrugated paper", "corrugated core paper") and one layer of cardboard (also known as "boxboard", "boxboard"). At present, packaging boxes made of corrugated cardboard have been widely used in the packaging and transportation of various items. They have the advantages of light weight, foldability, and shock resistance.

[0003] However, during high-intensity transportation and use, the traditional corrugated paperboard used as the outer packaging of articles is not elastic, strong and impact-resistant enough, and is easily damaged, and has poor anti-deformation effect, and cannot provide good protection for the packaged articles. The above problems can be solved to a certain extent by improving the layered structure of the corrugated paperboard, such as the high-strength and impact-resistant composite corrugated paper and its preparation method disclosed in patent CN111907181B or the high-elasticity double-corrugated paper core corrugated paperboard disclosed in patent CN111959085A.

[0004] Since the main component of corrugated paperboard is plant cellulose, the oxygen index of traditional corrugated paperboard at room temperature is only about 15%, which is flammable and has the defect of poor flame retardancy, resulting in safety hazards when used. Patent CN110306380B discloses a waterproof flame retardant coating for corrugated paperboard and a preparation method thereof, which improves its flame retardancy by coating the waterproof flame retardant coating on the corrugated paperboard, but the improvement effect on the mechanical strength of the corrugated paperboard is insufficient.

[0005] Cellulose is one of the main components of corrugated paperboard. Under oxidation, cellulose will decompose, resulting in a decrease in the toughness of the paper and a phenomenon of "becoming brittle". At the same time, the organic glue used for the bonding structure between the layers of corrugated paperboard will also be destroyed by the polymer molecular chain under the action of oxygen, resulting in a decrease in the interfacial bonding strength and poor flexibility, which will eventually lead to a significant decrease in the overall performance of the corrugated paperboard and a significant shortening of its service life. Therefore, improving the anti-oxidation and aging ability of corrugated paperboard will be able to extend its service life and improve its use effect, but there is a lack of reliable solutions in the existing technology.

[0006] Therefore, it is necessary to improve the existing technology to provide a more reliable solution. Summary of the invention

[0007] The technical problem to be solved by the present invention is to provide a high-performance corrugated paperboard with a double corrugated paper core and a production method thereof in view of the deficiencies in the above-mentioned prior art.

[0008] In order to solve the above technical problems, the technical solution adopted by the present invention is: a high-performance corrugated paperboard with a double corrugated paper core, which includes a first face paper layer, a first corrugated paper core layer, an intermediate paper layer, a second corrugated paper core layer and a second face paper layer stacked in sequence, and adjacent layers are bonded by a modified adhesive;

[0009] The modified adhesive comprises the following raw material components in parts by weight:

[0010] 35-65 parts of bisphenol A epoxy resin, 13-42 parts of polyurethane acrylate oligomer, 4-17 parts of tackifying resin, 7.5-28 parts of composite modified particles, 0.6-2 parts of curing agent, and 14-50 parts of solvent;

[0011] The modified adhesive is prepared by the following method:

[0012] According to the weight ratio, bisphenol A epoxy resin, polyurethane acrylate oligomer, tackifying resin and composite modified particles are added to the solvent, stirred, and then a curing agent is added and stirred evenly to obtain the modified adhesive.

[0013] Preferably, the composite modified particles are prepared by the following method:

[0014] S1, grafting mesoporous cerium oxide onto graphene oxide to obtain CeO2-Go mesoporous composite nanomaterials;

[0015] S2, modifying nickel-doped carbon dots on CeO2-Go mesoporous composite nanomaterials to obtain CeO2-Go@Ni-CDs composite particles;

[0016] S3, modifying the CeO2-Go@Ni-CDs composite particles with a silane coupling agent to obtain surface-modified CeO2-Go@Ni-CDs composite particles;

[0017] S4. Loading a flame retardant on the surface-modified CeO2-Go@Ni-CDs composite particles by an impregnation method to obtain the composite modified particles.

[0018] Preferably, step S1 specifically includes:

[0019] S1-1, take 2.5-10g of graphene oxide, add it into a mixed acid consisting of 25-100mL of 30% hydrogen peroxide and 75-300mL of 95% concentrated sulfuric acid, stir and reflux at 60-80°C for 3-12h, wash with deionized water until neutral, and dry at 80-100°C for 4-24h to obtain pretreated graphene oxide;

[0020] S1-2, add 1-4 g of pretreated graphene oxide to 100-350 mL of deionized water, ultrasonically disperse for 15-60 min, then add 1.63-6.54 g of cerium nitrate to the obtained dispersion, stir for 5-30 min, and obtain mixture A; add 0.75-3 g of P123 and 0.9-3.6 g of urea to 50-200 mL of deionized water, stir for 5-20 min, and obtain mixture B;

[0021] S1-3, adding mixture B to mixture A under stirring, transferring the resulting mixture to a polytetrafluoroethylene-lined reactor, and reacting at 120-140° C. for 3-8 hours;

[0022] S1-4. After the reaction is completed, cool to room temperature, filter, wash the solid product with deionized water, and then dry it at 100-120°C for 0.5-3h, and then calcine it at 400-500°C in an air atmosphere for 3-8h, grind it, and obtain CeO2-Go mesoporous composite nanomaterials.

[0023] Preferably, step S2 specifically includes:

[0024] S2-1, take 0.5-2g CeO2-Go mesoporous composite nanomaterials and 0.183-0.732g nickel nitrate, add them into 50-160mL deionized water, and ultrasonically disperse for 30-60min;

[0025] S2-2, add 0.088-0.352 g of ascorbic acid, 0.15-0.6 g of tartaric acid, 0.06-0.24 g of ethylenediamine, and 0.054-0.216 g of o-phenylenediamine to an ethanol aqueous solution consisting of 15-60 mL of ethanol and 35-140 mL of deionized water, and stir for 5-30 min. Add the resulting mixed solution to the dispersion obtained in step S2-1, and ultrasonically disperse for 15-60 min to obtain a precursor solution;

[0026] S2-3. Add the precursor solution into a polytetrafluoroethylene-based reactor, react at 165-185°C for 4-16 hours, cool to room temperature after the reaction, filter, wash the solid product with ethanol, vacuum dry at 60-80°C for 2.5-10 hours, and grind to obtain CeO2-Go@Ni-CDs composite particles.

[0027] Preferably, step S3 specifically includes:

[0028] Take 0.5-2g CeO2-Go@Ni-CDs composite particles and add them to 50-200mL acetone, then add 0.075-0.3g silane coupling agent A-172, stir at 50-60℃ for 0.5-2h, cool, filter, wash the solid product with ethanol, and then vacuum dry at 55-70℃ for 3-12h to obtain surface modified CeO2-Go@Ni-CDs composite particles.

[0029] Preferably, step S4 specifically includes:

[0030] Take 1-4g of surface modified CeO2-Go@Ni-CDs composite particles and add them to 50-200mL of 8-12% mass fraction of tricresyl phosphate ethanol solution, shake on a shaker at 30-40°C for 3-12h, filter, wash the solid product with ethanol, and then vacuum dry at 40-55°C for 6-24h to obtain composite modified particles.

[0031] Preferably, the polyurethane acrylate oligomer is polyurethane acrylate oligomer A2116, the solvent is toluene, the tackifying resin is rosin pentaerythritol ester, and the curing agent is 2-ethyl-4-methylimidazole.

[0032] Preferably, the first surface paper layer, the first corrugated paper core layer, the middle paper layer, the second corrugated paper core layer and the second surface paper layer are all prepared using modified pulp liquid as raw materials, and the modified pulp liquid includes the following components in parts by weight:

[0033] 45-70 parts of lignin fiber;

[0034] 7-24 parts corn starch;

[0035] 13-52 parts corn stalk powder;

[0036] 11-36 parts of composite modified particles;

[0037] Polyvinyl alcohol 3.5-13 parts;

[0038] Polyacrylamide 3-15 parts;

[0039] 8-29 parts of modified carbon fiber dispersion slurry;

[0040] 150-400 parts of water.

[0041] Preferably, the modified carbon fiber dispersion slurry is prepared by the following method:

[0042] The chopped carbon fibers are added to a mixed acid consisting of 95 wt% concentrated sulfuric acid and 60 wt% concentrated nitric acid in a volume ratio of 2:1, heated under reflux at 80-95° C. for 2-8 hours, taken out, washed with deionized water until neutral, and dried at 90-110° C. for 3-12 hours to obtain acid-treated carbon fibers;

[0043] The acid-treated carbon fiber: sodium carboxymethyl cellulose: deionized water are mixed in a mass ratio of 10:1.5:30, and ultrasonically dispersed for 15-60 minutes to obtain a modified carbon fiber dispersion slurry.

[0044] The present invention also provides a method for producing the high-performance corrugated paperboard having a double corrugated paper core as described above, comprising the following steps:

[0045] Step 1, dividing water into a first part of water and a second part of water, wherein the mass ratio of the first part of water to the second part of water is 3:1; adding lignin fiber, corn stalk powder and corn starch to the first part of water, stirring evenly and then crushing, passing through a 50-100 mesh sieve, to obtain base paper pulp;

[0046] Step 2: adding polyvinyl alcohol, modified carbon fiber dispersion slurry and composite modified particles to the second part of water, stirring at 200-600 rpm for 10-30 min, adding the obtained mixed solution and polyacrylamide to the base paper pulp obtained in step 1, beating at 150-400 rpm and 60-75° C. for 20-60 min, and then standing for 30-90 min to obtain modified paper pulp;

[0047] Step 3, drying and forming the modified pulp liquid into paper to prepare a first paper layer, a middle paper layer, and a second paper layer;

[0048] The modified pulp liquid is used for papermaking to obtain corrugated base paper, and then corrugated paper is pressed to obtain a first corrugated paper core layer and a second corrugated paper core layer;

[0049] Step 4: Apply the modified adhesive on the inner surfaces of the first paper layer and the second paper layer, as well as the front and back surfaces of the first corrugated paper core layer, the middle paper layer, and the second corrugated paper core layer, respectively, and then bond the first paper layer, the first corrugated paper core layer, the middle paper layer, the second corrugated paper core layer, and the second paper layer in sequence, compact with a flattening roller, and dry at 65-80°C for 0.5-4h to obtain the high-performance corrugated paperboard with a double corrugated paper core.

[0050] The beneficial effects of the present invention are:

[0051] The corrugated paperboard prepared by the present invention has a double corrugated paper core structure, which can effectively improve its elasticity and mechanical strength;

[0052] The present invention uses self-made composite modified particles and modified carbon fibers to compositely modify the pulp raw materials used to prepare the main paper layer structure of each layer of the corrugated paperboard, and at the same time, the composite modified particles are used to enhance and modify the adhesive material between the main paper layers, which can significantly improve the comprehensive mechanical strength of the corrugated paperboard and improve its flame retardant performance. Furthermore, the composite modified particles can also be used to give the corrugated paperboard good antioxidant performance. On the one hand, the phenomenon that the corrugated paperboard itself becomes brittle due to oxidation and the phenomenon that the organic adhesive material between the paper layers reduces the bonding strength due to oxidation and aging can be suppressed, thereby greatly slowing down the speed at which the mechanical strength of the corrugated paperboard decreases due to oxidation and aging during use, and prolonging its service life; on the other hand, because it has antioxidant properties and has a good removal effect on gases such as ethylene, the carton product prepared by the corrugated paperboard can also be well suitable for the storage and transportation packaging of products with antioxidant and fresh-keeping requirements (such as fruits, vegetables and other products), and the carton can provide a certain fresh-keeping effect;

[0053] The composite modified particles prepared by the present invention can be added to the modified adhesive system and the modified pulp liquid system at the same time, and can play a multi-faceted enhancement effect; and the mesoporous cerium oxide and nickel-doped carbon dots in the composite modified particles can cooperate with each other, which can significantly improve the performance of multiple aspects of the system. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] Figure 1 is the test result of bursting strength;

[0055] Figure 2 is the test result of edge compression strength;

[0056] Figure 3 is the test result of bonding strength;

[0057] Figure 4 The test results of flame retardancy;

[0058] Figure 5 It is the DPPH clearance test result;

[0059] Figure 6 is the ethylene removal rate test result;

[0060] Figure 7 The infrared absorption spectrum of the surface modified CeO2-Go@Ni-CDs composite particles prepared in Example 1;

[0061] Figure 8 The test results of the antioxidant properties of the composite modified particles prepared in Example 1;

[0062] Fig. 9 These are the test results of the sustained release performance of the composite modified particles prepared in Example 1. DETAILED DESCRIPTION

[0063] The present invention is further described in detail below in conjunction with embodiments so that those skilled in the art can implement the invention with reference to the description.

[0064] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.

[0065] The test methods used in the following examples are conventional methods unless otherwise specified. The materials and reagents used in the following examples are all commercially available unless otherwise specified. In the following examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.

[0066] In a first aspect of the present invention, there is provided a high-performance corrugated paperboard with a double corrugated paper core, which comprises a first face paper layer, a first corrugated paper core layer, an intermediate paper layer, a second corrugated paper core layer and a second face paper layer stacked in sequence, wherein adjacent layers are bonded by a modified adhesive;

[0067] The modified adhesive comprises the following raw material components in parts by weight:

[0068] 35-65 parts of bisphenol A epoxy resin, 13-42 parts of polyurethane acrylate oligomer, 4-17 parts of tackifying resin, 7.5-28 parts of composite modified particles, 0.6-2 parts of curing agent, and 14-50 parts of solvent;

[0069] The modified adhesive is prepared by the following method:

[0070] According to the weight ratio, bisphenol A epoxy resin, polyurethane acrylate oligomer, tackifying resin and composite modified particles are added to the solvent, stirred, and then a curing agent is added and stirred evenly to obtain the modified adhesive.

[0071] In the present invention, the composite modified particles are prepared by the following method:

[0072] S1. Grafting mesoporous cerium oxide onto graphene oxide to obtain CeO2-Go mesoporous composite nanomaterials:

[0073] S1-1, take 2.5-10g of graphene oxide, add it into a mixed acid consisting of 25-100mL of 30% hydrogen peroxide and 75-300mL of 95% concentrated sulfuric acid, stir and reflux at 60-80°C for 3-12h, wash with deionized water until neutral, and dry at 80-100°C for 4-24h to obtain pretreated graphene oxide;

[0074] S1-2, add 1-4 g of pretreated graphene oxide to 100-350 mL of deionized water, ultrasonically disperse for 15-60 min, then add 1.63-6.54 g of cerium nitrate to the obtained dispersion, stir for 5-30 min, and obtain mixture A; add 0.75-3 g of P123 and 0.9-3.6 g of urea to 50-200 mL of deionized water, stir for 5-20 min, and obtain mixture B;

[0075] S1-3, adding mixture B to mixture A under stirring, transferring the resulting mixture to a polytetrafluoroethylene-lined reactor, and reacting at 120-140° C. for 3-8 hours;

[0076] S1-4. After the reaction is completed, cool to room temperature, filter, wash the solid product with deionized water, and then dry it at 100-120°C for 0.5-3h, and then calcine it at 400-500°C in an air atmosphere for 3-8h, grind it, and obtain CeO2-Go mesoporous composite nanomaterials.

[0077] S2. Modify nickel-doped carbon dots on CeO2-Go mesoporous composite nanomaterials to obtain CeO2-Go@Ni-CDs composite particles:

[0078] S2-1, take 0.5-2g CeO2-Go mesoporous composite nanomaterials and 0.183-0.732g nickel nitrate, add them into 50-160mL deionized water, and ultrasonically disperse for 30-60min;

[0079] S2-2, add 0.088-0.352 g of ascorbic acid, 0.15-0.6 g of tartaric acid, 0.06-0.24 g of ethylenediamine, and 0.054-0.216 g of o-phenylenediamine to an ethanol aqueous solution consisting of 15-60 mL of ethanol and 35-140 mL of deionized water, and stir for 5-30 min. Add the resulting mixed solution to the dispersion obtained in step S2-1, and ultrasonically disperse for 15-60 min to obtain a precursor solution;

[0080] S2-3. Add the precursor solution into a polytetrafluoroethylene-based reactor, react at 165-185°C for 4-16 hours, cool to room temperature after the reaction, filter, wash the solid product with ethanol, vacuum dry at 60-80°C for 2.5-10 hours, and grind to obtain CeO2-Go@Ni-CDs composite particles.

[0081] S3, modifying the CeO2-Go@Ni-CDs composite particles with a silane coupling agent to obtain surface-modified CeO2-Go@Ni-CDs composite particles:

[0082] Take 0.5-2g CeO2-Go@Ni-CDs composite particles and add them to 50-200mL acetone, then add 0.075-0.3g silane coupling agent A-172, stir at 50-60℃ for 0.5-2h, cool, filter, wash the solid product with ethanol, and then vacuum dry at 55-70℃ for 3-12h to obtain surface modified CeO2-Go@Ni-CDs composite particles.

[0083] S4, loading a flame retardant on the surface-modified CeO2-Go@Ni-CDs composite particles by an impregnation method to obtain the composite modified particles:

[0084] Take 1-4g of surface modified CeO2-Go@Ni-CDs composite particles and add them to 50-200mL of 8-12% mass fraction of tricresyl phosphate ethanol solution, shake on a shaker at 30-40°C for 3-12h, filter, wash the solid product with ethanol, and then vacuum dry at 40-55°C for 6-24h to obtain composite modified particles.

[0085] In a preferred embodiment, the polyurethane acrylate oligomer is polyurethane acrylate oligomer A2116, the solvent is toluene, the tackifying resin is rosin pentaerythritol ester, and the curing agent is 2-ethyl-4-methylimidazole.

[0086] In a preferred embodiment, the first surface paper layer, the first corrugated paper core layer, the middle paper layer, the second corrugated paper core layer and the second surface paper layer are all prepared using modified pulp liquid as raw materials, and the modified pulp liquid includes the following components in parts by weight:

[0087] 45-70 parts of lignin fiber;

[0088] 7-24 parts corn starch;

[0089] 13-52 parts corn stalk powder;

[0090] 11-36 parts of composite modified particles;

[0091] Polyvinyl alcohol 3.5-13 parts;

[0092] Polyacrylamide 3-15 parts;

[0093] 8-29 parts of modified carbon fiber dispersion slurry;

[0094] 150-400 parts of water.

[0095] In the present invention, the modified carbon fiber dispersion slurry is prepared by the following method:

[0096] The chopped carbon fibers are added to a mixed acid consisting of 95 wt% concentrated sulfuric acid and 60 wt% concentrated nitric acid in a volume ratio of 2:1, heated under reflux at 80-95° C. for 2-8 hours, taken out, washed with deionized water until neutral, and dried at 90-110° C. for 3-12 hours to obtain acid-treated carbon fibers;

[0097] The acid-treated carbon fiber: sodium carboxymethyl cellulose: deionized water are mixed in a mass ratio of 10:1.5:30, and ultrasonically dispersed for 15-60 minutes to obtain a modified carbon fiber dispersion slurry.

[0098] In a preferred embodiment, the diameter of the chopped carbon fibers is 0.1-1 mm and the length is 5-50 mm.

[0099] A second aspect of the present invention provides a method for producing a high-performance corrugated paperboard having a double corrugated paper core as described above, comprising the following steps:

[0100] Step 1, dividing water into a first part of water and a second part of water, wherein the mass ratio of the first part of water to the second part of water is 3:1; adding lignin fiber, corn stalk powder and corn starch to the first part of water, stirring evenly and then crushing, passing through a 50-100 mesh sieve, to obtain base paper pulp;

[0101] Step 2: adding polyvinyl alcohol, modified carbon fiber dispersion slurry and composite modified particles to the second part of water, stirring at 200-600 rpm for 10-30 min, adding the obtained mixed solution and polyacrylamide to the base paper pulp obtained in step 1, beating at 150-400 rpm and 60-75° C. for 20-60 min, and then standing for 30-90 min to obtain modified paper pulp;

[0102] Step 3, drying and forming the modified pulp liquid into paper to prepare a first paper layer, a middle paper layer, and a second paper layer;

[0103] The modified pulp liquid is used for papermaking to obtain corrugated base paper, and then corrugated paper is pressed to obtain a first corrugated paper core layer and a second corrugated paper core layer;

[0104] Step 4: Apply the modified adhesive on the inner surfaces of the first paper layer and the second paper layer, as well as the front and back surfaces of the first corrugated paper core layer, the middle paper layer, and the second corrugated paper core layer, respectively, and then bond the first paper layer, the first corrugated paper core layer, the middle paper layer, the second corrugated paper core layer, and the second paper layer in sequence, compact with a flattening roller, and dry at 65-80°C for 0.5-4h to obtain the high-performance corrugated paperboard with a double corrugated paper core.

[0105] In a preferred embodiment, the corrugating forming temperature is 150-165° C., the pressure is 1.5-4 MPa, the corrugated paper core has a corrugation height of 2-5 mm, and the number of corrugations is 5-15 / 100 mm.

[0106] The corrugated paperboard prepared by the present invention has a double corrugated paper core structure, which can effectively improve its elasticity and mechanical strength; the present invention uses self-made composite modified particles and modified carbon fibers to compositely modify the pulp raw materials used to prepare the main paper layer structure of each layer of the corrugated paperboard, and also uses the composite modified particles to enhance and modify the adhesive material between each main paper layer, which can significantly improve the comprehensive mechanical strength of the corrugated paperboard and improve its flame retardant performance. Further, the composite modified particles can also be used to give the corrugated paperboard good antioxidant performance, which can inhibit the phenomenon that the corrugated paperboard itself becomes brittle due to oxidation and the phenomenon that the organic adhesive material between the paper layers reduces the bonding strength due to oxidation and aging, thereby greatly slowing down the speed at which the mechanical strength of the corrugated paperboard decreases due to oxidation and aging during use, and prolonging its service life; on the other hand, because it has antioxidant performance and has a good removal effect on gases such as ethylene, the carton product prepared by the corrugated paperboard can also be well suitable for the storage and transportation packaging of products with antioxidant and fresh-keeping requirements (such as fruits, vegetables and other products), and the carton can provide a certain fresh-keeping effect. In a preferred use mode, when used for packaging of products such as fruits and vegetables, food-grade breathable inner packaging can be used to package the fruits and vegetables, and then placed in a carton to prevent the fruits and vegetables from directly contacting the carton products.

[0107] In the present invention, a strong acid is first used to acidify the flaky graphene oxide, so that abundant carboxyl functional groups can be introduced on the surface of the graphene oxide, which is beneficial to improve its dispersion performance; then a hydrothermal method-calcination method combined with a soft template method is used to in-situ synthesize mesoporous cerium oxide with abundant pore structure on the graphene oxide, in which process, cerium ions can be combined with carboxyl functional groups on the surface of the graphene oxide so as to be uniformly and massively loaded on the surface of the graphene oxide, and then P123 is used as a template agent, and mesoporous cerium oxide is synthesized through hydrothermal reaction and calcination to obtain a CeO2-Go mesoporous composite nanomaterial;

[0108] Then, the nickel ion solution is mixed with the CeO2-Go mesoporous composite nanomaterial. The nickel ions can combine with the remaining carboxyl functional groups on the surface of graphene oxide. After adding ascorbic acid, tartaric acid, ethylenediamine and o-phenylenediamine as precursor raw materials of carbon dots, these raw materials can combine with nickel ions through coordination, electrostatic adsorption and other effects. After a hydrothermal reaction, a large number of nickel-doped carbon dots can be grafted on the surface of graphene oxide (a small amount of nickel-doped carbon dots will also be generated on the surface of mesoporous cerium oxide), thereby obtaining CeO2-Go@Ni-CDs composite particles.

[0109] Finally, the CeO2-Go@Ni-CDs composite particles were surface modified by silane coupling agent A-172, and then a large amount of flame retardant tricresyl phosphate was loaded on the mesoporous structure of cerium oxide by impregnation method to obtain composite modified particles.

[0110] In the structural system of the composite modified particles, the modification of silane coupling agent A-17 can significantly improve the dispersibility of the composite modified particles, so that they can be evenly dispersed in the modified adhesive system and the modified paper pulp system, which can overcome the defect of graphene oxide being difficult to disperse; at the same time, the pulling effect of mesoporous cerium oxide ions on flaky graphene oxide can reduce the curling of graphene oxide and promote its full unfolding, so as to give full play to the reinforcing effect of graphene oxide on the modified adhesive system and the modified paper pulp system. Specifically, for the adhesive system, graphene oxide can significantly improve the bonding strength and aging resistance of the adhesive; for the modified paper pulp system, graphene oxide can significantly improve the mechanical strength and wear resistance of the prepared paper layer.

[0111] On the other hand, the modification of silane coupling agent A-17 can also improve the flame retardancy of corrugated cardboard. The mechanism is: siloxane can generate a carbon-silicon barrier layer when burning, which can isolate oxygen and prevent the melt from dripping, thereby achieving a flame retardant effect (Li Aixia. Research Progress of Halogen-free Organic Flame Retardants [J]. Guangdong Chemical Industry, 2005, 32(11): 4. DOI: 10.3969 / j.issn.1007-1865.2005.11.005.).

[0112] In the structural system of composite modified particles, mesoporous cerium oxide can at least play the following roles:

[0113] 1. It has good mechanical strength. As a filler, it can improve the bonding strength of adhesives and the compressive strength and wear resistance of modified pulp systems;

[0114] 2. Mesoporous cerium oxide is used as a carrier. By virtue of its mesoporous structure, the flame retardant tricresyl phosphate can be loaded, which can achieve the slow release effect of the flame retardant, thereby providing long-lasting flame retardant performance for the modified adhesive system and the modified pulp liquid system, and ultimately significantly improving the flame retardant ability of the prepared corrugated paperboard; and by loading the flame retardant with mesoporous cerium oxide, the surface migration of the flame retardant can be effectively avoided, so that it can be stably dispersed in the system;

[0115] At the same time, mesoporous cerium oxide itself can play a role in thermal stability, and its mesoporous structure and the presence of oxygen vacancies allow it to absorb surrounding oxygen, thereby improving flame retardancy (Shen Genli. Synthesis and flame retardant and smoke suppression properties of cerium-based flame retardant materials [J]. University of Chinese Academy of Sciences, 2013. DOI: http: / / ir.ipe.ac.cn / handle / 122111 / 8297.);

[0116] 3. The mesoporous structure of mesoporous cerium oxide gives it a certain physical adsorption effect, which can physically remove gases such as ethylene that are harmful to freshness preservation; and cerium has an affinity for oxygen, so it can cooperate with the reducing ability of nickel-doped carbon dots to better achieve the removal of oxygen free radicals, which can enhance the antioxidant capacity of corrugated cardboard.

[0117] Oxidation is one of the main factors that cause the aging of corrugated cardboard itself and the adhesive layer that connects its layers: under oxidation, the cellulose in the cardboard itself will decompose, causing the toughness of the paper to decrease and become "brittle"; the organic components in the adhesive will cause the polymer molecular chains to be destroyed under the action of oxygen, which will reduce the interfacial bonding strength and deteriorate the flexibility, ultimately leading to a significant decline in the overall performance of the corrugated cardboard and a significantly shortened service life.

[0118] In the structural system of composite modified particles, nickel-doped carbon dots can at least play the following roles:

[0119] (1) The carbon dots in the present invention inherit the reducing properties of ascorbic acid and exhibit good antioxidant function, which can effectively remove free radicals generated inside the corrugated board and the adhesive layer, thereby overcoming the above problems and extending its service life;

[0120] (2) Nickel has a specific adsorption effect on ethylene (Zhuang Youyi. Adsorption and decomposition of ethylene on transition metal surfaces [J]. Journal of Wenzhou Normal University (3): 10-12 [2024-05-07]. DOI: 10.3875 / j.issn.1674-3563.2001.03.003.), thereby enhancing the removal effect of the composite modified particles on ethylene gas;

[0121] (3) The antioxidant properties of nickel-doped carbon dots, the specific adsorption of nickel on ethylene, and the physical adsorption capacity of mesoporous cerium oxide make it possible for the carton products made of corrugated cardboard to be used as outer packaging for vegetables, fruits, etc., and to slow down the oxidation of the internal vegetables, fruits, etc. by scavenging free radicals and absorbing ethylene, thereby achieving a certain preservation effect.

[0122] (4) The physical isolation effect of the carbonization of nickel-doped carbon dots themselves also helps to improve the flame retardant properties.

[0123] The above analysis shows that the composite modified particles prepared by the present invention can be added to the modified adhesive system and the modified pulp liquid system at the same time, and can play a multi-faceted enhancement effect; and the mesoporous cerium oxide and nickel-doped carbon dots in the composite modified particles can cooperate with each other, which can significantly improve the performance of multiple aspects of the system.

[0124] Carbon fiber can improve the mechanical strength, wear resistance and aging resistance of paperboard, but its wettability is poor and difficult to disperse. In the present invention, the above problems can be overcome by preparing a modified carbon fiber dispersion slurry. The present invention first introduces oxygen-containing functional groups such as carboxyl groups on the surface of carbon fiber through a strong acid to improve its wettability, and then mixes it with sodium carboxymethyl cellulose, which can better wet the carbon fiber and promote its uniform dispersion; and when the modified carbon fiber dispersion slurry is added to the modified paper pulp liquid system, the modified carbon fiber dispersion slurry is first mixed with polyvinyl alcohol and composite modified particles. The bonding effect of polyvinyl alcohol can make the carbon fiber and the graphene oxide in the composite modified particles interconnected to form an overlapping network structure, so that the carbon fiber and graphene oxide can better play the enhancement effect of mechanical properties.

[0125] The above is the overall concept of the present invention, and detailed embodiments and comparative examples are provided below on the basis of the overall concept of the present invention to further illustrate the present invention.

[0126] The main sources of raw materials involved in the following examples and comparative examples are as follows:

[0127] Bisphenol A epoxy resin, Suzhou Senfeida Chemical Co., Ltd.;

[0128] Polyurethane acrylate oligomer A2116, Hubei Handafei Biotechnology Co., Ltd.;

[0129] Rosin pentaerythritol ester, brand: Pentalyn H, manufacturer: American Pinova, purchased from Shanghai Maitian Chemical Co., Ltd.;

[0130] 2-Ethyl-4-methylimidazole, Jiangsu Bosite Chemical Technology Co., Ltd.;

[0131] Graphene oxide, single-layer flake, flake diameter: 2-5 μm, thickness: 0.8-1.5 nm; Suzhou Kaifa New Materials Technology Co., Ltd.;

[0132] P123, template agent, polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer, Nanjing Ruichuang Chemical Technology Co., Ltd.;

[0133] Silane coupling agent A-172, namely vinyl tris(β-methoxyethoxy)silane, Nanjing Pinyoudao Chemical Technology Co., Ltd.;

[0134] Tricresyl phosphate; Shanghai MacLean Biochemical Technology Co., Ltd.;

[0135] Lignin fiber, Xuzhou Yihuiyang New Materials Co., Ltd.;

[0136] Corn straw powder, Henan Mingjie Animal Husbandry Co., Ltd.;

[0137] Corn starch, Xuzhou Yihuiyang New Materials Co., Ltd.;

[0138] Polyvinyl alcohol, Jiangsu Rayen Environmental Protection Technology Co., Ltd.;

[0139] Polyacrylamide, Jiangsu Rayen Environmental Protection Technology Co., Ltd.;

[0140] Chopped carbon fiber, diameter 0.2mm, length 5-20mm, Yancheng Xiangsheng Carbon Fiber Technology Co., Ltd.

[0141] The other raw materials not mentioned are conventional commercially available products.

[0142] Example 1

[0143] A high-performance corrugated paperboard with a double corrugated paper core, comprising a first face paper layer, a first corrugated paper core layer, an intermediate paper layer, a second corrugated paper core layer and a second face paper layer stacked in sequence, with adjacent layers bonded by a modified adhesive;

[0144] The modified adhesive comprises the following raw material components in parts by weight:

[0145] 50 parts of bisphenol A epoxy resin, 26 parts of polyurethane acrylate oligomer A2116, 8.5 parts of tackifying resin (rosin pentaerythritol ester), 15 parts of composite modified particles, 1.2 parts of 2-ethyl-4-methylimidazole, and 28 parts of toluene;

[0146] The modified adhesive is prepared by the following method:

[0147] According to the weight ratio, bisphenol A epoxy resin, polyurethane acrylate oligomer, tackifying resin and composite modified particles are added to the solvent toluene, stirred for 10 minutes, and then 2-ethyl-4-methylimidazole is added and stirred for 5 minutes to obtain the modified adhesive.

[0148] In this embodiment, the composite modified particles are prepared by the following method:

[0149] S1. Grafting mesoporous cerium oxide onto graphene oxide to obtain CeO2-Go mesoporous composite nanomaterials:

[0150] S1-1, take 5g of graphene oxide and add it into a mixed acid consisting of 50mL of 30% hydrogen peroxide and 150mL of 95% concentrated sulfuric acid, stir and reflux at 70°C for 6h, wash with deionized water until neutral, and dry at 90°C for 8h to obtain pretreated graphene oxide;

[0151] S1-2, add 2 g of pretreated graphene oxide to 200 mL of deionized water, and ultrasonically disperse for 30 min, then add 3.26 g of cerium nitrate to the obtained dispersion, and stir for 15 min to obtain a mixture A; add 1.5 g of P123 and 1.8 g of urea to 100 mL of deionized water, and stir for 10 min to obtain a mixture B;

[0152] S1-3, adding mixture B to mixture A under stirring, transferring the resulting mixture to a polytetrafluoroethylene-lined reactor, and reacting at 125° C. for 6 h;

[0153] S1-4. After the reaction is completed, the mixture is cooled to room temperature and filtered. The solid product is washed with deionized water and then dried at 110°C for 1 h. The solid product is then calcined at 450°C in an air atmosphere for 6 h and ground to obtain a CeO2-Go mesoporous composite nanomaterial.

[0154] S2. Modify nickel-doped carbon dots on CeO2-Go mesoporous composite nanomaterials to obtain CeO2-Go@Ni-CDs composite particles:

[0155] S2-1, take 1g CeO2-Go mesoporous composite nanomaterial and 0.366g nickel nitrate, add them into 80mL deionized water, and ultrasonically disperse for 45min;

[0156] S2-2, add 0.176g ascorbic acid, 0.3g tartaric acid, 0.12g ethylenediamine, and 0.108g o-phenylenediamine to an ethanol aqueous solution consisting of 30mL ethanol and 70mL deionized water, stir for 10min, add the resulting mixture to the dispersion obtained in step S2-1, and ultrasonically disperse for 30min to obtain a precursor solution;

[0157] S2-3. Add the precursor solution into a polytetrafluoroethylene-based reactor and react at 175°C for 8 hours. After the reaction is completed, cool to room temperature, filter, wash the solid product with ethanol, vacuum dry at 70°C for 5 hours, and grind to obtain CeO2-Go@Ni-CDs composite particles.

[0158] S3, modifying the CeO2-Go@Ni-CDs composite particles with a silane coupling agent to obtain surface-modified CeO2-Go@Ni-CDs composite particles:

[0159] Take 1 g of CeO2-Go@Ni-CDs composite particles and add them to 100 mL of acetone, then add 0.15 g of silane coupling agent A-172, stir at 55 °C for 1 h, cool, filter, wash the solid product with ethanol, and then vacuum dry at 60 °C for 6 h to obtain surface-modified CeO2-Go@Ni-CDs composite particles.

[0160] S4, loading a flame retardant on the surface-modified CeO2-Go@Ni-CDs composite particles by an impregnation method to obtain the composite modified particles:

[0161] Take 2 g of surface modified CeO2-Go@Ni-CDs composite particles and add them into 100 mL of 10% mass dispersion of tricresyl phosphate ethanol solution, shake on a shaker at 35 °C for 6 h, filter, wash the solid product with ethanol, and then vacuum dry at 50 °C for 12 h to obtain composite modified particles.

[0162] In this embodiment, the first surface paper layer, the first corrugated paper core layer, the middle paper layer, the second corrugated paper core layer and the second surface paper layer are all prepared using modified pulp liquid as raw materials, and the modified pulp liquid includes the following components in parts by weight:

[0163] 55 parts of lignin fiber;

[0164] 14 parts corn starch;

[0165] Corn stalk powder 27 parts;

[0166] 23 parts of composite modified particles;

[0167] 6.5 parts of polyvinyl alcohol;

[0168] Polyacrylamide 7 parts;

[0169] 16 parts of modified carbon fiber dispersion slurry;

[0170] 200 parts of water.

[0171] Wherein, the modified carbon fiber dispersion slurry is prepared by the following method:

[0172] The chopped carbon fibers were added into a mixed acid consisting of 95 wt% concentrated sulfuric acid and 60 wt% concentrated nitric acid in a volume ratio of 2:1, heated under reflux at 90°C for 4 hours, taken out, washed with deionized water until neutral, and dried at 100°C for 6 hours to obtain acid-treated carbon fibers;

[0173] The acid-treated carbon fiber: sodium carboxymethyl cellulose: deionized water were mixed in a mass ratio of 10:1.5:30, and ultrasonically dispersed for 30 minutes to obtain a modified carbon fiber dispersion slurry.

[0174] In this embodiment, the method for producing the high-performance corrugated paperboard with a double corrugated paper core comprises the following steps:

[0175] Step 1, dividing water into a first part of water and a second part of water, wherein the mass ratio of the first part of water to the second part of water is 3:1; adding lignin fiber, corn stalk powder and corn starch to the first part of water, stirring evenly and then crushing, passing through an 80-mesh sieve, to obtain base paper pulp;

[0176] Step 2: adding polyvinyl alcohol, modified carbon fiber dispersion slurry and composite modified particles to the second part of water, stirring at 400 rpm for 20 min, adding the obtained mixed solution and polyacrylamide to the base paper pulp, beating at 250 rpm and 70° C. for 40 min, and standing for 60 min to obtain a modified paper pulp;

[0177] Step 3, drying and forming the modified pulp liquid into paper to prepare a first paper layer, a middle paper layer, and a second paper layer;

[0178] The modified pulp liquid is used for papermaking to obtain corrugated base paper, which is then corrugated and formed, and dried at 110°C for 3 minutes to obtain the first corrugated paper core layer and the second corrugated paper core layer; wherein, the corrugating forming temperature is 155°C, the pressure is 2.5MPa, the corrugation height of the corrugated paper core is 3mm, and the number of corrugations is 8 / 100mm.

[0179] Step 4: Apply the modified adhesive on the inner surfaces of the first paper layer and the second paper layer, as well as the front and back surfaces of the first corrugated paper core layer, the middle paper layer, and the second corrugated paper core layer, respectively, and then bond the first paper layer, the first corrugated paper core layer, the middle paper layer, the second corrugated paper core layer, and the second paper layer in sequence, compact them with a flattening roller, and dry them at 70°C for 2 hours to obtain the high-performance corrugated paperboard with a double corrugated paper core.

[0180] Among them, the thickness of the adhesive layer formed by the modified adhesive between adjacent layers is 0.5mm; the thickness of the first outer paper layer and the second outer paper layer is 0.8mm; the thickness of the middle paper layer is 1.5mm, and the thickness of the first corrugated paper core layer and the second corrugated paper core layer is 1.2mm.

[0181] Example 2

[0182] This example is basically the same as Example 1, and only the differences are listed below.

[0183] In this example, the modified adhesive includes the following raw material components in parts by weight:

[0184] 50 parts of bisphenol A type epoxy resin, 28 parts of polyurethane acrylate oligomer A2116, 9 parts of tackifying resin (rosin pentaerythritol ester), 13.5 parts of composite modified particles, 1.2 parts of 2-ethyl-4-methylimidazole, and 28 parts of toluene;

[0185] The modified pulp liquid comprises the following components by weight:

[0186] 58 parts of lignin fiber;

[0187] 15 parts corn starch;

[0188] Corn stalk powder 26 parts;

[0189] 22 parts of composite modified particles;

[0190] 7 parts of polyvinyl alcohol;

[0191] Polyacrylamide 7 parts;

[0192] 15 parts of modified carbon fiber dispersion slurry;

[0193] 200 parts of water.

[0194] Example 3

[0195] This example is basically the same as Example 1, and only the differences are listed below.

[0196] In this example, the modified adhesive includes the following raw material components in parts by weight:

[0197] 52 parts of bisphenol A epoxy resin, 24 parts of polyurethane acrylate oligomer A2116, 9.5 parts of tackifying resin (rosin pentaerythritol ester), 15 parts of composite modified particles, 1.4 parts of 2-ethyl-4-methylimidazole, and 28 parts of toluene;

[0198] The modified pulp liquid comprises the following components by weight:

[0199] 60 parts of lignin fiber;

[0200] 12 parts corn starch;

[0201] 25 parts corn stalk powder;

[0202] 23 parts of composite modified particles;

[0203] 7 parts of polyvinyl alcohol;

[0204] 7.5 parts of polyacrylamide;

[0205] 17 parts of modified carbon fiber dispersion slurry;

[0206] 200 parts of water.

[0207] Comparative Example 1

[0208] This example is basically the same as Example 1, and only the differences are listed below.

[0209] In this example, the modified adhesive includes the following raw material components in parts by weight:

[0210] 50 parts of bisphenol A epoxy resin, 26 parts of polyurethane acrylate oligomer A2116, 8.5 parts of tackifying resin (rosin pentaerythritol ester), 1.2 parts of 2-ethyl-4-methylimidazole, and 28 parts of toluene;

[0211] The modified pulp liquid comprises the following components by weight:

[0212] 55 parts of lignin fiber;

[0213] 14 parts corn starch;

[0214] Corn stalk powder 27 parts;

[0215] 6.5 parts of polyvinyl alcohol;

[0216] Polyacrylamide 7 parts;

[0217] 16 parts of modified carbon fiber dispersion slurry;

[0218] 200 parts of water.

[0219] Comparative Example 2

[0220] This example is basically the same as Example 1, and only the differences are listed below.

[0221] In this example, the modified adhesive includes the following raw material components in parts by weight:

[0222] 50 parts of bisphenol A type epoxy resin, 26 parts of polyurethane acrylate oligomer A2116, 8.5 parts of tackifying resin (rosin pentaerythritol ester), 1.2 parts of 2-ethyl-4-methylimidazole, and 28 parts of toluene.

[0223] Comparative Example 3

[0224] This example is basically the same as Example 1, and only the differences are listed below.

[0225] In this example, the modified pulp liquid includes the following components by weight:

[0226] 55 parts of lignin fiber;

[0227] 14 parts corn starch;

[0228] Corn stalk powder 27 parts;

[0229] 6.5 parts of polyvinyl alcohol;

[0230] Polyacrylamide 7 parts;

[0231] 16 parts of modified carbon fiber dispersion slurry;

[0232] 200 parts of water.

[0233] Comparative Example 4

[0234] This example is basically the same as Example 1, and only the differences are listed below.

[0235] In this example, the modified pulp liquid includes the following components by weight:

[0236] 55 parts of lignin fiber;

[0237] 14 parts corn starch;

[0238] Corn stalk powder 27 parts;

[0239] 23 parts of composite modified particles;

[0240] 6.5 parts of polyvinyl alcohol;

[0241] Polyacrylamide 7 parts;

[0242] 4 pieces of chopped carbon fiber;

[0243] 200 parts of water.

[0244] Comparative Example 5

[0245] This example is basically the same as Example 1, and only the differences are listed below.

[0246] In this example, the composite modified particles are prepared by the following method:

[0247] S1, grafting mesoporous cerium oxide onto graphene oxide to obtain CeO2-Go mesoporous composite nanomaterial; the specific steps are the same as those in Example 1;

[0248] S2. Take 1 g of CeO2-Go mesoporous composite nanomaterial and add it to 100 mL of acetone, then add 0.15 g of silane coupling agent A-172, stir at 55°C for 1 h, cool, filter, wash the solid product with ethanol, and then vacuum dry at 60°C for 6 h to obtain a surface-modified CeO2-Go mesoporous composite nanomaterial.

[0249] S3. Take 2 g of surface modified CeO2-Go mesoporous composite nanomaterial and add it to 100 mL of 10% mass dispersion of tricresyl phosphate ethanol solution, shake it on a shaker at 35°C for 6 h, filter it, wash the solid product with ethanol, and then vacuum dry it at 50°C for 12 h to obtain composite modified particles.

[0250] Comparative Example 6

[0251] This example is basically the same as Example 1, and only the differences are listed below.

[0252] In this example, the composite modified particles are prepared by the following method:

[0253] S1, grafting mesoporous cerium oxide onto graphene oxide to obtain CeO2-Go mesoporous composite nanomaterial; the specific steps are the same as those in Example 1;

[0254] S2. Modify carbon dots on CeO2-Go mesoporous composite nanomaterials to obtain CeO2-Go@CDs composite particles:

[0255] S2-1, take 1g CeO2-Go mesoporous composite nanomaterial, add it into 80mL deionized water, and disperse it by ultrasonic for 45min;

[0256] S2-2, add 0.176g ascorbic acid, 0.3g tartaric acid, 0.12g ethylenediamine, and 0.108g o-phenylenediamine to an ethanol aqueous solution consisting of 30mL ethanol and 70mL deionized water, stir for 10min, add the resulting mixture to the dispersion obtained in step S2-1, and ultrasonically disperse for 30min to obtain a precursor solution;

[0257] S2-3. Add the precursor solution into a polytetrafluoroethylene-based reactor and react at 175°C for 8 hours. After the reaction is completed, cool to room temperature, filter, wash the solid product with ethanol, vacuum dry at 70°C for 5 hours, and grind to obtain CeO2-Go@CDs composite particles.

[0258] S3, modifying the CeO2-Go@CDs composite particles with a silane coupling agent to obtain surface-modified CeO2-Go@CDs composite particles, the specific steps are the same as those in Example 1;

[0259] S4. Loading a flame retardant on the surface-modified CeO2-Go@CDs composite particles by an impregnation method to obtain the composite modified particles. The specific steps are the same as those in Example 1.

[0260] Performance Test:

[0261] 1. Burst strength: tested according to the standard "GB / T6544-2008";

[0262] 2. Edge compression strength: tested in accordance with the standard "GB / T6544-2008";

[0263] 3. Bond strength: tested according to the standard "GB / T6548-2011";

[0264] 4. Flame retardant performance: Limiting oxygen index (LOI) test is carried out in accordance with the standard "GB / T5454-1997";

[0265] 5. DPPH clearance rate detection:

[0266] The DPPH free radical scavenging rate detection kit (Shanghai Beibo Biotechnology Co., Ltd., BB-47382) was used for detection. The detection method is as follows:

[0267] For each embodiment and comparative example, two groups of DPPH solutions (5 mL each) were prepared, one group was used as a control group, and the other group was added with a corrugated cardboard sample (2 mg, cut perpendicular to the cardboard surface, that is, the sample included each structural layer in the thickness direction) as an experimental group. After 1 hour, the absorbance of the solution at 517 nm was measured respectively. The absorbance of the control group and the experimental group was recorded as Ac and As respectively, and the free radical scavenging rate η was calculated according to the following formula:

[0268]

[0269] DPPH free radicals have strong absorption near 517nm. Adding substances with antioxidant properties can scavenge DPPH free radicals and reduce the absorbance at 517nm, which can reflect the strength of the free radical scavenging ability. The stronger the antioxidant ability, the higher the free radical scavenging rate.

[0270] 6. Ethylene removal rate test

[0271] For each embodiment and comparative example, 1 g of corrugated cardboard sample (cut perpendicular to the cardboard surface, that is, the sample includes each structural layer in the thickness direction) was taken and added to a conical flask with a volume of 250 mL. Air with an ethylene concentration of 200 ppm was introduced into the flask and filled up the conical flask, then sealed and left at room temperature for 1 h. Then, a handheld portable VOC detector (PV6001-VOC-EX) was used to measure the ethylene concentration in the air in the conical flask, thereby calculating the ethylene removal rate.

[0272] The above performance test results are shown in Table 1 and Figure 1-6 shown.

[0273] Table 1

[0274]

[0275]

[0276] It can be seen from the above test results that the corrugated cardboard prepared in Examples 1-3 has high bursting strength, edge compression strength and bonding strength, excellent mechanical strength, and obvious flame retardant properties, as well as excellent antioxidant capacity and ethylene removal capacity. Comparison of the results of Comparative Examples 1-3 with those of Example 1 shows that the composite modified particles have a significant enhancing and improving effect on both the modified adhesive system and the modified pulp liquid system, and can comprehensively improve the mechanical strength, flame retardant properties and antioxidant properties of the corrugated cardboard. In Comparative Example 4, the mechanical strength has decreased due to the failure to effectively solve the problem of difficult dispersion of carbon fibers. Comparison of Comparative Example 5 with Example 1 shows that the antioxidant properties in the composite modified particles mainly come from nickel-doped carbon dots. Comparison of Comparative Example 6 with Example 1 shows that the doping of nickel in the composite modified particles helps to improve the ability to remove ethylene.

[0277] Performance characterization:

[0278] Taking Example 1 as an example, the following performance characterization is performed to further illustrate the mechanism of the present invention.

[0279] 1. The surface modified CeO2-Go@Ni-CDs composite particles prepared in Example 1 were characterized by infrared absorption spectroscopy. The results are as follows: Figure 7 As shown; the appearance of the characteristic peaks of Si-C, Si-O, and Si-O-Si bonds indicates that the silane coupling agent A-172 has been successfully modified; 485cm -1 The characteristic peak near it comes from nickel oxide, 2995cm -1 、830cm -1 、705cm -1 The characteristic peaks nearby come from CeO2; the infrared absorption spectrum results show the successful synthesis of surface modified CeO2-Go@Ni-CDs composite particles.

[0280] 2. Testing the antioxidant properties of the composite modified particles prepared in Example 1;

[0281] The composite modified particles prepared in Example 1 were prepared into a solution with a concentration of 0.5 mg / mL using acetone, and the absorbance at 517 nm at different times was detected using a DPPH free radical scavenging rate detection kit (Shanghai Beibo Biotechnology Co., Ltd., BB-47382).

[0282] DPPH is a free radical with strong absorption near 517nm. Adding substances with antioxidant properties can remove DPPH free radicals and reduce the absorbance at 517nm, which can reflect the strength of the antioxidant ability. The lower the absorbance at 517nm, the stronger the antioxidant ability.

[0283] Test results such as Figure 8As shown, it can be seen that the composite modified particles prepared in Example 1 have excellent antioxidant properties.

[0284] 3. Testing the sustained release performance of the composite modified particles prepared in Example 1;

[0285] 0.2 g of the composite modified particles prepared in Example 1 was added to 10 mL of ethanol and allowed to stand at room temperature. The ethanol solution was taken out at regular intervals, and the concentration of tricresyl phosphate in the acetone solution was measured by a UV-visible spectrophotometer, and then new ethanol solution was added. The operation was repeated, and then the release percentage of tricresyl phosphate at different times was calculated, and a release curve was plotted.

[0286] The calculation method of the initial content of tricresyl phosphate in the composite modified particles is as follows: in step S4, the concentration of tricresyl phosphate in the ethanol solution of tricresyl phosphate after the immersion treatment is detected, and the loading amount of tricresyl phosphate in the composite modified particles can be converted to obtain the initial content.

[0287] The release curve obtained is as follows Fig. 9 As shown, it can be seen that the composite modified particles can release tricresyl phosphate for a long time, indicating that it has good sustained-release properties.

[0288] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.

Claims

1. A high-performance corrugated paperboard with a double corrugated paper core, characterized in that: It comprises a first face paper layer, a first corrugated paper core layer, an intermediate paper layer, a second corrugated paper core layer and a second face paper layer which are stacked in sequence, and adjacent layers are bonded by a modified adhesive; The modified adhesive comprises the following raw material components in parts by weight: 35-65 parts of bisphenol A epoxy resin, 13-42 parts of polyurethane acrylate oligomer, 4-17 parts of tackifying resin, 7.5-28 parts of composite modified particles, 0.6-2 parts of curing agent, and 14-50 parts of solvent; The modified adhesive is prepared by the following method: Add bisphenol A epoxy resin, polyurethane acrylate oligomer, tackifying resin and composite modified particles into a solvent according to weight ratio, stir, then add a curing agent, stir evenly, to obtain the modified adhesive; The composite modified particles are prepared by the following method: S1, grafting mesoporous cerium oxide onto graphene oxide to obtain CeO2-Go mesoporous composite nanomaterials; S2, modifying nickel-doped carbon dots on CeO2-Go mesoporous composite nanomaterials to obtain CeO2-Go@Ni-CDs composite particles; S3, modifying the CeO2-Go@Ni-CDs composite particles with a silane coupling agent to obtain surface-modified CeO2-Go@Ni-CDs composite particles; S4, loading a flame retardant on the surface-modified CeO2-Go@Ni-CDs composite particles by an impregnation method to obtain the composite modified particles; Step S1 specifically includes: S1-1, take 2.5-10g of graphene oxide, add it into a mixed acid consisting of 25-100mL of 30% by mass hydrogen peroxide and 75-300mL of 95% by mass concentrated sulfuric acid, stir and reflux at 60-80°C for 3-12h, wash with deionized water until neutral, and dry at 80-100°C for 4-24h to obtain pretreated graphene oxide; S1-2, add 1-4 g of pretreated graphene oxide to 100-350 mL of deionized water, ultrasonically disperse for 15-60 min, then add 1.63-6.54 g of cerium nitrate to the obtained dispersion, stir for 5-30 min, and obtain mixture A; add 0.75-3 g of P123 and 0.9-3.6 g of urea to 50-200 mL of deionized water, stir for 5-20 min, and obtain mixture B; S1-3, adding mixture B to mixture A under stirring, transferring the resulting mixture to a polytetrafluoroethylene-lined reactor, and reacting at 120-140° C. for 3-8 hours; S1-4, after the reaction is completed, the mixture is cooled to room temperature, filtered, the solid product is washed with deionized water, and then dried at 100-120° C. for 0.5-3 h, and then calcined at 400-500° C. for 3-8 h in an air atmosphere, and ground to obtain a CeO2-Go mesoporous composite nanomaterial; Step S2 specifically includes: S2-1, take 0.5-2g CeO2-Go mesoporous composite nanomaterials and 0.183-0.732g nickel nitrate, add them into 50-160mL deionized water, and ultrasonically disperse for 30-60min; S2-2, add 0.088-0.352 g of ascorbic acid, 0.15-0.6 g of tartaric acid, 0.06-0.24 g of ethylenediamine, and 0.054-0.216 g of o-phenylenediamine to an ethanol aqueous solution consisting of 15-60 mL of ethanol and 35-140 mL of deionized water, and stir for 5-30 min. Add the resulting mixed solution to the dispersion obtained in step S2-1, and ultrasonically disperse for 15-60 min to obtain a precursor solution; S2-3, adding the precursor solution into the reaction kettle of the polytetrafluoroethylene substrate, reacting at 165-185°C for 4-16 hours, cooling to room temperature after the reaction, filtering, washing the solid product with ethanol, vacuum drying at 60-80°C for 2.5-10 hours, grinding, and obtaining CeO2-Go@Ni-CDs composite particles; Step S3 specifically includes: Take 0.5-2g CeO2-Go@Ni-CDs composite particles and add them to 50-200mL acetone, then add 0.075-0.3g silane coupling agent A-172, stir at 50-60℃ for 0.5-2h, cool, filter, wash the solid product with ethanol, and then vacuum dry at 55-70℃ for 3-12h to obtain surface modified CeO2-Go@Ni-CDs composite particles; Step S4 specifically includes: 1-4 g of surface-modified CeO2-Go@Ni-CDs composite particles were added to 50-200 mL of 8-12% mass fraction tricresyl phosphate ethanol solution, shaken on a shaker at 30-40° C. for 3-12 h, filtered, the solid product was washed with ethanol, and then vacuum dried at 40-55° C. for 6-24 h to obtain composite modified particles; The first surface paper layer, the first corrugated paper core layer, the middle paper layer, the second corrugated paper core layer and the second surface paper layer are all prepared using modified pulp liquid as raw materials, and the modified pulp liquid includes the following components in parts by weight: 45-70 parts of lignin fiber; 7-24 parts corn starch; 13-52 parts of corn stalk powder; 11-36 parts of composite modified particles; Polyvinyl alcohol 3.5-13 parts; Polyacrylamide 3-15 parts; 8-29 parts of modified carbon fiber dispersion slurry; 150-400 parts of water; The modified carbon fiber dispersion slurry is prepared by the following method: The chopped carbon fibers are added to a mixed acid consisting of 95wt% concentrated sulfuric acid and 60wt% concentrated nitric acid in a volume ratio of 2:1, heated under reflux at 80-95°C for 2-8h, taken out, washed with deionized water until neutral, and dried at 90-110°C for 3-12h to obtain acid-treated carbon fibers; The acid-treated carbon fiber: sodium carboxymethyl cellulose: deionized water are mixed in a mass ratio of 10:1.5:30, and ultrasonically dispersed for 15-60 minutes to obtain a modified carbon fiber dispersion slurry.

2. The high performance corrugated paperboard with double corrugated paper core according to claim 1, characterized in that: The polyurethane acrylate oligomer is polyurethane acrylate oligomer A2116, the solvent is toluene, the tackifying resin is rosin pentaerythritol ester, and the curing agent is 2-ethyl-4-methylimidazole.

3. A method for producing high-performance corrugated paperboard with a double corrugated paper core as claimed in any one of claims 1 to 2, characterized in that: The following steps are involved: Step 1, dividing water into a first part of water and a second part of water, wherein the mass ratio of the first part of water to the second part of water is 3:1; adding lignin fiber, corn stalk powder and corn starch to the first part of water, stirring evenly and then crushing, passing through a 50-100 mesh sieve, to obtain base paper pulp; Step 2: adding polyvinyl alcohol, modified carbon fiber dispersion slurry and composite modified particles to the second part of water, stirring at 200-600 rpm for 10-30 min, adding the obtained mixed solution and polyacrylamide to the base paper pulp obtained in step 1, beating at 150-400 rpm and 60-75° C. for 20-60 min, and then standing for 30-90 min to obtain modified paper pulp; Step 3, drying and forming the modified pulp liquid into paper to prepare a first paper layer, a middle paper layer, and a second paper layer; The modified pulp liquid is used for papermaking to obtain corrugated base paper, and then corrugated paper is pressed to obtain a first corrugated paper core layer and a second corrugated paper core layer; Step 4: Apply the modified adhesive on the inner surfaces of the first paper layer and the second paper layer, as well as the front and back surfaces of the first corrugated paper core layer, the middle paper layer, and the second corrugated paper core layer, respectively, and then bond the first paper layer, the first corrugated paper core layer, the middle paper layer, the second corrugated paper core layer, and the second paper layer in sequence, compact with a flattening roller, and dry at 65-80°C for 0.5-4h to obtain the high-performance corrugated paperboard with a double corrugated paper core.

Citation Information

Patent Citations

  • A waterproof and flame-retardant coating for corrugated cardboard and its preparation method

    CN110306380B

  • High-strength and impact-resistant composite corrugated paper and its preparation method

    CN111907181B

  • High-elasticity corrugated board with double corrugated paper cores

    CN111959085A

  • High-strength impact-resistant composite corrugated paper and preparation method thereof

    CN111907181A

  • High-strength composite single corrugated board and preparation method thereof

    CN113352720A