Slow-release antioxidant inhibitor and preparation method thereof
By molecularly modifying anthocyanins and combining it with modified super-absorbent resin, a slow-release antioxidant inhibitor is prepared, which solves the problem that existing inhibitors are prone to failure at high temperatures and improves thermal stability and resistance. The oxidation ability achieves a green and environmentally friendly coal spontaneous combustion suppression effect.
Patent Information
- Application Number
- CN202411080741.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-08
AI Technical Summary
Existing inhibitors have poor stability under high temperature conditions and are prone to failure. Their chemical components pose a threat to the environment and human health, and they are expensive.
By molecularly modifying anthocyanins and combining it with modified super absorbent resin, a slow-release antioxidant inhibitor is prepared. Vacuum drying and even mixing of deionized water are used to form a stable gel-like substance to improve Thermal stability.
Improves the thermal stability and antioxidant capacity of anthocyanins, allowing them to continuously capture free radicals under high temperature conditions, extending the service life of inhibitors, solving the problem of traditional inhibitors being prone to failure, and reducing environmental impact and harm to the human body.
Smart Images

Figure CN118601658B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of inhibitors and relates to a slow-release antioxidant inhibitor and a preparation method thereof. Background Art
[0002] Coal will remain an important cornerstone for ensuring my country's energy strategic security for a long time, but more than 90% of my country's mined coal seams have a tendency to spontaneously combust or spontaneously combust. Coal spontaneous combustion fires not only cause waste of resources and damage to mining equipment, but also threaten the safety of underground personnel with harmful gases, and induce secondary disasters such as gas and coal dust explosions. Inhibitors are an effective technical means to prevent coal spontaneous combustion.
[0003] However, the existing inhibitors for preventing coal spontaneous combustion generally have the following defects: Under high temperature conditions, the stability and inhibitory ability of the inhibitor are reduced, and the inhibitory effect is not as expected. After the use of chemical inhibitors, they penetrate into the soil and water sources, and have a long-term impact on the ecosystem. Some inhibitors contain chemicals that are harmful to the human body and will face health risks during use. They are expensive, which increases the economic burden of coal mines.
[0004] As a renewable green resource and natural product with antioxidant function, anthocyanin has been developed and utilized in recent years in many industries such as medicine, health products, cosmetics and food. Studies have shown that anthocyanin is the most effective antioxidant and the most powerful free radical scavenger. Anthocyanin can react with active functional groups in the coal structure, capture free radicals and generate stable groups. Therefore, applying anthocyanin as an antioxidant to the field of coal spontaneous combustion prevention and control technology can terminate the coal-oxygen chain reaction and achieve the purpose of inhibiting coal spontaneous combustion in a green and environmentally friendly way. However, the molecular structure of anthocyanin makes it susceptible to environmental factors such as temperature, and its thermal stability needs to be improved so that it can continue to play an inhibitory role at high temperatures. Summary of the invention
[0005] One object of the present invention is to provide a slow-release antioxidant inhibitor, which solves the problem that the existing inhibitor has poor stability and is easily ineffective in the high-temperature stage of coal spontaneous combustion.
[0006] Another object of the present invention is to provide a method for preparing the slow-release antioxidant inhibitor.
[0007] The first technical solution adopted by the present invention is a method for preparing a slow-release antioxidant inhibitor, comprising the following steps:
[0008] Step 1, preparing an antioxidant, wherein the antioxidant is formed by molecularly modifying anthocyanins;
[0009] Step 2, preparing a composite super absorbent resin, wherein the composite super absorbent resin is formed by modifying a super absorbent resin with hydrotalcite;
[0010] Step 3, placing an antioxidant and a composite super absorbent resin in a weight ratio of 1:1 to 7 in a beaker, adding deionized water to the beaker, stirring while adding, so that the antioxidant, the composite super absorbent resin and the deionized water are evenly mixed and present a gel state, and then placing it in a vacuum drying oven and vacuum drying it at a temperature of 40 to 50° C. to obtain a slow-release antioxidant inhibitor.
[0011] The specific process of step 1 is as follows:
[0012] Step 1.1, protecting the hydroxyl group of gallic acid, comprising mixing anhydrous gallic acid, propionic anhydride and anhydrous pyridine, then adding deionized water to the reaction system, stirring thoroughly, and then adding hydrochloric acid solution to adjust the pH value of the reaction system to 1-2, collecting the white precipitate by suction filtration after standing, washing the product with deionized water, and vacuum drying to constant weight to obtain acylated gallic acid;
[0013] Step 1.2, preparing galloyl chloride, adding the acylated gallic acid prepared in step 1.1 into anhydrous thionyl chloride, then adding dichloromethane to dissolve the reactant, then removing the thionyl chloride by rotary evaporation, precipitating crystals, repeatedly dissolving and evaporating, and vacuum drying to constant weight to obtain galloyl chloride;
[0014] Step 1.3, dissolving galloyl chloride in dioxane, then adding anthocyanidin and pyridine, stirring and reflux reaction for 5 to 8 hours, then adding deionized water and anhydrous ethanol, dioxane and pyridine are evaporated by rotary evaporator to obtain product crystals, filtering, washing and suction filtration, and finally vacuum drying to constant weight to obtain galloylated anthocyanidin;
[0015] Step 1.4, deacylation reaction of galloylated anthocyanidin, comprising dissolving galloylated anthocyanidin in acetone, adding sodium hydroxide solution dropwise for neutralization, then adding hydrochloric acid solution to adjust the pH value of the reaction system to 3-4, distilling off the acetone using a rotary evaporator to obtain a solid substance, filtering the solid substance, dissolving the filtered solid in ethyl acetate, washing the ester layer with deionized water, distilling off the ethyl acetate under reduced pressure to obtain a molecularly modified anthocyanidin, i.e., an antioxidant.
[0016] Step 1.1 includes adding anhydrous gallic acid, propionic anhydride and anhydrous pyridine in a molar ratio of 1:4 to 5:4 to 5 into a three-necked flask in an ice bath environment, stirring to completely dissolve the gallic acid, then adding 5 times the volume of deionized water into the three-necked flask, stirring evenly, and then adding hydrochloric acid solution to make the pH value of the solution in the three-necked flask 1 to 2, stirring until a white precipitate appears in the three-necked flask, standing for 24 hours to 36 hours, then collecting the white precipitate by suction, and finally washing with 5 to 6° C. deionized water, and then vacuum drying at room temperature to constant weight.
[0017] Step 1.2 comprises adding acylated gallic acid to anhydrous thionyl chloride, wherein the molar mass ratio of acylated gallic acid to anhydrous thionyl chloride is 1:3-4, stirring to allow the acylated gallic acid to react completely, adding 1-2 times the volume of dichloromethane to dissolve the reactant, and then removing the thionyl chloride by rotary evaporation using a rotary evaporator to precipitate crystals, repeatedly dissolving and evaporating until brown crystals are obtained, and vacuum drying the brown crystals to constant weight to obtain galloyl chloride.
[0018] In step 1.3, galloyl chloride is dissolved in dioxane, wherein the concentration of galloyl chloride is 50-55 g / mL, and then anthocyanidin and pyridine are added, and the molar ratio of galloyl chloride, anthocyanidin and pyridine is 5:1:5, and then deionized water and anhydrous ethanol are added, and the volume of the added deionized water and anhydrous ethanol is the same as that of the dioxane.
[0019] In step 1.4, the galloylated anthocyanidin is dissolved in acetone, wherein the concentration of the galloylated anthocyanidin is 40-45 g / mL, the temperature of the reaction system is cooled to 0°C in an ice bath, sodium hydroxide solution is added dropwise with stirring to make the pH value of the reaction system 7-8, and then the mixture is allowed to stand at 0°C for 3h-4h, hydrochloric acid solution is added to make the pH value of the reaction system 3-4, acetone is evaporated by a rotary evaporator to obtain a solid substance, the solid substance is filtered, and then the filtered solid is dissolved in ethyl acetate, the concentration of the filtered solid in ethyl acetate is 40-45 g / mL, and finally the ester layer is washed with deionized water.
[0020] In step 2, a composite super absorbent resin is prepared, and the specific process is as follows:
[0021] Step 2.1, hydrotalcite intercalation, comprising adding sodium hydroxide solution dropwise to an acrylic acid solution, stirring for neutralization, adding magnesium aluminum hydrotalcite, carrying out ion exchange reaction under nitrogen atmosphere protection, and finally washing, filtering and drying the reaction product to obtain intercalated hydrotalcite;
[0022] Step 2.2, add sodium hydroxide solution dropwise to the acrylic acid solution, stir to neutralize, add intercalated hydrotalcite and crosslinking agent, stir evenly and place in an ultrasonic cleaner for dispersion, then heat to 75°C, add initiator, stir and react fully until the solution is completely converted into a gel, the reaction is terminated, and a preliminary product is obtained. The preliminary product is cut into pieces and dried to obtain a composite super absorbent resin, wherein the content of intercalated hydrotalcite in the composite super absorbent resin is 3-12%, the content of crosslinking agent is 5%, and the content of initiator is 10%.
[0023] In step 2.1, magnesium aluminum hydrotalcite is added, the mass ratio of magnesium aluminum hydrotalcite to the mixed solution is 1:5-6, and an ion exchange reaction is carried out under the protection of a nitrogen atmosphere. The ion exchange reaction temperature is 65-70° C. and the reaction time is 48h-60h.
[0024] Step 2.2 includes placing a four-necked flask equipped with a stirrer, a condenser, a thermometer and a nitrogen tube in ice water, adding an acrylic acid solution to the four-necked flask, and adding a sodium hydroxide solution dropwise, stirring continuously to neutralize until the neutralization degree reaches 90%, then adding intercalated hydrotalcite powder and a cross-linking agent, stirring evenly and placing in an ultrasonic cleaning machine for dispersion, then passing nitrogen into the four-necked flask to remove oxygen in the flask, heating the four-necked flask to 75° C., adding an initiator dropwise, stirring until the solution is completely converted into a gel, and the reaction is terminated, the cross-linking agent used is N, N'-methylenebisacrylamide, and the initiator used is potassium persulfate.
[0025] The second technical solution adopted by the present invention is to prepare the slow-release antioxidant inhibitor using the above preparation method.
[0026] The beneficial effects of the present invention are as follows: an antioxidant is formed by modifying anthocyanin molecules, the antioxidant has strong antioxidant capacity and a more stable structure; after the hydrotalcite is treated with intercalation, the separation phenomenon from the organic resin is improved, the dispersion of the hydrotalcite is increased, and the agglomeration of the hydrotalcite is prevented; the hydrotalcite modifies the super absorbent resin, the hydrotalcite is cross-linked to the side chain of the super absorbent resin through chemical bonds, the super absorbent resin network chain is expanded, the thermal stability of the super absorbent resin modified by the hydrotalcite is greatly improved, the disadvantage of the low ignition point of anthocyanin is overcome, and the antioxidant has a good ability to eliminate free radicals in the high temperature stage, and the finally prepared slow-release antioxidant inhibitor can realize the continuous capture of free radicals in the high temperature stage of coal spontaneous combustion, and solves the problem that the traditional inhibitor is easy to fail at high temperature. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic diagram of the internal structure of the slow-release antioxidant inhibitor of the present invention;
[0028] Figure 2 It is a comparison chart of the liquid absorption rate of the composite super absorbent resin prepared in Comparative Example 1 and Examples 1 to 4 of the present invention;
[0029] Figure 3 The heat flow curves of the molecularly modified anthocyanin prepared in Example 1 and the slow-release antioxidant inhibitors prepared in Examples 1 to 7 of the present invention;
[0030] Figure 4 is the heat flow curve of the non-sticky raw coal and the retardant coal in the present invention;
[0031] Figure 5 It is the heat flow curve of the long flame coal and the retardant coal in the present invention.
[0032] In the figure, 1. Main chain, 2. Side chain, 3. Antioxidant, 4. Hydrotalcite. DETAILED DESCRIPTION
[0033] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0034] Example 1
[0035] A method for preparing a slow-release antioxidant inhibitor comprises the following steps:
[0036] Step 1, preparing an antioxidant, wherein the antioxidant is formed by molecular modification of anthocyanidins, and the specific process is as follows:
[0037] Step 1.1, placing gallic acid in a vacuum drying oven, drying at 120° C. for 50 hours, drying to constant weight, obtaining anhydrous gallic acid, adding anhydrous gallic acid, propionic anhydride and anhydrous pyridine in a molar ratio of 1:4:4 to a 1000 mL three-necked flask in an ice bath environment, stirring to completely dissolve the gallic acid, then slowly stirring for 15 hours under 25° C. oil bath conditions, the stirrer speed is 200 rpm, so that there is no gallic acid residue in the reaction system, and then adding 5 times the volume of deionized water to the three-necked flask, quickly stirring evenly, the stirrer speed is 550 rpm, and then slowly adding hydrochloric acid solution, adjusting the pH value of the solution in the three-necked flask to 1, stirring until a white precipitate appears in the three-necked flask, standing for 24 hours, and then filtering to collect the white precipitate, and finally washing with 5° C. deionized water, and vacuum drying at room temperature to constant weight, to obtain acylated gallic acid;
[0038] Step 1.2, acylated gallic acid and anhydrous thionyl chloride are added to a 1000 mL round-bottom flask in a molar mass ratio of 1:3, and refluxed in an oil bath at 80° C. with stirring to allow the acylated gallic acid to react completely. The progress of the reaction is tracked by thin layer chromatography (TLC). When no acylated gallic acid is detected, the reaction is terminated, and 2 volumes of dichloromethane are added to the flask to dissolve the reactants. Finally, the thionyl chloride is removed by rotary evaporation at 50° C. to precipitate crystals. The dissolution and evaporation are repeated many times until brown crystals are obtained. The brown crystals are vacuum dried to constant weight to obtain a white powder, namely galloyl chloride;
[0039] Step 1.3, weigh 16.10g of galloyl chloride and dissolve it in 30mL of dioxane, then add 2.87g of anthocyanidin and 4.0mL of pyridine, and stir and reflux for 5h at 50°C, then add 30mL of deionized water and 30mL of anhydrous ethanol through a rotary evaporator under a negative pressure of 0.08Mpa, and evaporate the dioxane and pyridine through a rotary evaporator to obtain product crystals, filter, wash and filter, and finally vacuum dry to constant weight to obtain galloylated anthocyanidin;
[0040] Step 1.4, deacylation reaction of galloylated anthocyanidin, comprising dissolving galloylated anthocyanidin in 20 ml of acetone, wherein the concentration of galloylated anthocyanidin is 40 g / mL, cooling the temperature of the reaction system to 0°C in an ice bath, adding sodium hydroxide solution dropwise with stirring to make the pH value of the reaction system 8, then standing at 0°C for 3 hours, and then adding hydrochloric acid solution to make the pH value of the reaction system 3, distilling off the acetone with a rotary evaporator to obtain a solid substance, filtering the solid substance, and then dissolving the filtered solid in ethyl acetate, wherein the concentration of the filtered solid in the solution is 40 g / mL, washing the ester layer with deionized water, and distilling off the ethyl acetate under reduced pressure to obtain a molecularly modified anthocyanidin, i.e., an antioxidant.
[0041] Step 2, preparing a composite super absorbent resin, the specific process is as follows:
[0042] Step 2.1, hydrotalcite intercalation, measure 100 mL of 25% acrylic acid solution, add 30% sodium hydroxide solution to the acrylic acid solution in an ice water bath environment for neutralization, so that the pH value of the mixed solution is 7, then add 20 g of magnesium aluminum hydrotalcite, under nitrogen atmosphere protection, at 65 ° C for 48 hours, finally wash the reaction product, filter, and dry the filter cake at 70 ° C for 24 hours to obtain intercalated hydrotalcite;
[0043] Step 2.2, placing a four-necked flask equipped with a stirrer, a condenser, a thermometer and a nitrogen tube in ice water, adding acrylic acid solution to the four-necked flask, and adding sodium hydroxide solution dropwise, stirring continuously to neutralize until the neutralization degree reaches 90%, and then adding intercalated hydrotalcite powder and N, N'-methylenebisacrylamide to the mixed solution, stirring evenly and placing in an ultrasonic cleaner for 30 minutes of dispersion, and then passing nitrogen into the four-necked flask to exclude oxygen, heating to 75°C, adding potassium persulfate dropwise, stirring until the solution is completely converted into a gel, the reaction is terminated, and a primary product is obtained. The primary product is cut into pieces and placed in a vacuum drying oven at 80°C for 20 hours of vacuum drying to obtain a composite super absorbent resin, wherein the content of intercalated hydrotalcite in the composite super absorbent resin is 3%, the content of N, N'-methylenebisacrylamide is 5%, and the content of potassium persulfate is 10%;
[0044] Step 3, placing an antioxidant and a composite super absorbent resin in a weight ratio of 1:1 in a 100 mL beaker, adding 5 times the mass of deionized water to the beaker, using a magnetic stirrer, setting the speed to 200 rpm, stirring at room temperature for 1 hour to mix the antioxidant, the composite super absorbent resin and the deionized water evenly and present a gel state, and then placing it in a vacuum drying oven and vacuum drying it at 40°C until the sample has a constant weight. The dried sample is crushed into a powder with a particle size of 200 mesh, and a slow-release antioxidant inhibitor is obtained, whose structure is as follows Figure 1As shown, it includes a main chain 1, a side chain 2, an antioxidant 3 and a hydrotalcite 4. It can be seen that the slow-release antioxidant inhibitor forms a three-dimensional network structure with the main chain 1 as the skeleton, and the side chain 2 is a hydrotalcite 4 modified by chemical cross-linking, which expands the resin network chain structure and further enhances the thermal stability of the slow-release antioxidant inhibitor. Antioxidant 3 is an anthocyanin after molecular modification, which contains a large number of phenolic hydroxyl groups and has good polarity. The composite absorbent resin side chain 2 has a strong adsorption capacity for it and is not easy to elute after adsorption. During the spontaneous combustion and oxidation heating process of coal, the stable network structure can continuously release antioxidants to block the chain elementary reactions occurring in each stage of coal spontaneous combustion.
[0045] Example 2
[0046] A method for preparing a slow-release antioxidant inhibitor comprises the following steps:
[0047] Step 1, preparing an antioxidant, the preparation process is the same as in Example 1;
[0048] Step 2, preparing a composite super absorbent resin, the specific process is as follows:
[0049] Step 2.1, hydrotalcite intercalation, measuring 100 mL of 25% acrylic acid solution, adding 30% sodium hydroxide solution to the acrylic acid solution in an ice water bath environment for neutralization, so that the pH value of the mixed solution is 7, and then adding 20 g of magnesium aluminum hydrotalcite, wherein the mass ratio of magnesium aluminum hydrotalcite to the mixed solution is 1:5, under the protection of nitrogen atmosphere, ion exchange reaction is carried out at 70° C. for 52 hours, and finally the reaction product is washed and filtered, and the filter cake is dried at 70° C. for 20 hours to obtain intercalated hydrotalcite;
[0050] Step 2.2, placing a four-necked flask equipped with a stirrer, a condenser, a thermometer and a nitrogen tube in ice water, adding acrylic acid solution to the four-necked flask, and adding sodium hydroxide solution dropwise, stirring continuously to neutralize until the neutralization degree reaches 90%, and then adding intercalated hydrotalcite powder and N, N'-methylenebisacrylamide to the mixed solution, stirring evenly and placing in an ultrasonic cleaner for 30 minutes of dispersion, and then passing nitrogen into the four-necked flask to exclude oxygen, heating to 75°C, adding potassium persulfate dropwise, stirring until the solution is completely converted into a gel, the reaction is terminated, and a primary product is obtained. The primary product is cut into pieces and placed in a vacuum drying oven at 80°C for 20 hours of vacuum drying to obtain a composite super absorbent resin, wherein the content of intercalated hydrotalcite in the composite super absorbent resin is 6%, the content of N, N'-methylenebisacrylamide is 5%, and the content of potassium persulfate is 10%;
[0051] Step 3, placing an antioxidant and a composite super absorbent resin in a weight ratio of 1:2 in a 100mL beaker, adding 5 times the mass of deionized water to the beaker, using a magnetic stirrer, setting the speed to 200 rpm, stirring at room temperature for 1 hour to mix the antioxidant, the composite super absorbent resin and the deionized water evenly and present a gel state, and then placing it in a vacuum drying oven and vacuum drying it at 40°C until the sample has a constant weight. The dried sample is crushed into a powder with a particle size of 200 mesh, and a sustained-release antioxidant inhibitor is obtained.
[0052] Example 3
[0053] A method for preparing a slow-release antioxidant inhibitor comprises the following steps:
[0054] Step 1, preparing an antioxidant, wherein the antioxidant is formed by molecular modification of anthocyanidins, and the specific process is as follows:
[0055] Step 1.1, placing gallic acid in a vacuum drying oven, drying at 120°C for 50 hours, drying to constant weight, obtaining anhydrous gallic acid, adding anhydrous gallic acid, propionic anhydride and anhydrous pyridine in a molar ratio of 1:5:5 to a 1000mL three-necked flask in an ice bath environment, stirring to completely dissolve the gallic acid, then slowly stirring for 20 hours under 25°C oil bath conditions, the stirrer speed is 200 rpm, so that there is no gallic acid residue in the reaction system, and then adding 5 times the volume of deionized water to the three-necked flask, quickly stirring evenly, the stirrer speed is 550 rpm, and then slowly adding hydrochloric acid solution, adjusting the pH value of the solution in the three-necked flask to 2, stirring until a white precipitate appears in the three-necked flask, standing for 30 hours, and then filtering to collect the white precipitate, and finally washing with 6°C deionized water, and vacuum drying at room temperature to constant weight, that is, obtaining acylated gallic acid;
[0056] Step 1.2, acylated gallic acid and anhydrous thionyl chloride are added to a 1000 mL round-bottom flask in a molar mass ratio of 1:4, and refluxed in an oil bath at 80° C. with stirring to allow the acylated gallic acid to react completely. The progress of the reaction is tracked by thin layer chromatography (TLC). When no acylated gallic acid is detected, the reaction is completed, and the same volume of dichloromethane is added to the flask to dissolve the reactants. Finally, the thionyl chloride is removed by rotary evaporation at 50° C. to precipitate crystals. The dissolution and evaporation are repeated many times until brown crystals are obtained. The brown crystals are vacuum dried to constant weight to obtain a white powder, namely galloyl chloride;
[0057] Step 1.3, weigh 16.10g (0.05mol) of galloyl chloride and dissolve it in 30mL of dioxane, then add 2.87g (0.01mol) of anthocyanin and 4.0mL (0.05mol) of pyridine, and stir and reflux for 8h at 50°C, then add 30mL of deionized water and 30mL of anhydrous ethanol through a rotary evaporator under a negative pressure of 0.08Mpa, and evaporate the dioxane and pyridine through a rotary evaporator to obtain product crystals, filter, wash and filter, and finally vacuum dry to constant weight to obtain galloylated anthocyanin;
[0058] Step 1.4, deacylation reaction of galloylated anthocyanidin, comprising dissolving galloylated anthocyanidin in 20 ml of acetone, wherein the concentration of galloylated anthocyanidin is 45 g / mL, cooling the temperature of the reaction system to 0°C in an ice bath, adding sodium hydroxide solution dropwise with stirring to make the pH value of the reaction system 7, then standing at 0°C for 3 hours, and then adding hydrochloric acid solution to make the pH value of the reaction system 4, distilling off the acetone with a rotary evaporator to obtain a solid substance, filtering the solid substance, and then dissolving the filtered solid in ethyl acetate, wherein the concentration of the filtered solid in the solution is 45 g / mL, washing the ester layer with deionized water, and distilling off the ethyl acetate under reduced pressure to obtain a molecularly modified anthocyanidin, i.e., an antioxidant.
[0059] Step 2, preparing a composite super absorbent resin, the specific process is as follows:
[0060] Step 2.1, hydrotalcite intercalation, measuring 100 mL of 25% acrylic acid solution, adding 30% sodium hydroxide solution to the acrylic acid solution in an ice water bath environment for neutralization, so that the pH value of the mixed solution is 7, and then adding 20 g of magnesium aluminum hydrotalcite, wherein the mass ratio of magnesium aluminum hydrotalcite to the mixed solution is 1:5, under the protection of nitrogen atmosphere, ion exchange reaction is carried out at 70° C. for 52 hours, and finally the reaction product is washed and filtered, and the filter cake is dried at 70° C. for 20 hours to obtain intercalated hydrotalcite;
[0061] Step 2.2, placing a four-necked flask equipped with a stirrer, a condenser, a thermometer and a nitrogen tube in ice water, adding acrylic acid solution to the four-necked flask, and adding sodium hydroxide solution dropwise, stirring continuously to neutralize until the neutralization degree reaches 90%, and then adding intercalated hydrotalcite powder and N, N'-methylenebisacrylamide, stirring evenly and placing in an ultrasonic cleaner for 30 minutes of dispersion, and then passing nitrogen into the four-necked flask to exclude oxygen, heating to 75°C, adding potassium persulfate dropwise, stirring until the solution is completely converted into a gel, the reaction is terminated, and a primary product is obtained. The primary product is cut into pieces and placed in a vacuum drying oven at 80°C for 20 hours of vacuum drying to obtain a composite super absorbent resin, wherein the content of intercalated hydrotalcite in the composite super absorbent resin is 9%, the content of N, N'-methylenebisacrylamide is 5%, and the content of potassium persulfate is 10%;
[0062] Step 3, placing an antioxidant and a composite super absorbent resin in a weight ratio of 1:3 in a 100mL beaker, adding 5 times the mass of deionized water to the beaker, using a magnetic stirrer, setting the speed to 200 rpm, stirring at room temperature for 1 hour to mix the antioxidant, the composite super absorbent resin and the deionized water evenly and present a gel state, and then placing it in a vacuum drying oven and vacuum drying it at 50°C until the sample has a constant weight. The dried sample is crushed into a powder with a particle size of 200 mesh, and a slow-release antioxidant inhibitor is obtained.
[0063] Example 4
[0064] A method for preparing a slow-release antioxidant inhibitor comprises the following steps:
[0065] Step 1, preparing an antioxidant, the preparation process is the same as in Example 3;
[0066] Step 2, preparing a composite super absorbent resin, the specific process is as follows:
[0067] Step 2.1, hydrotalcite intercalation, measuring 100 mL of 25% acrylic acid solution, adding 30% sodium hydroxide solution to the acrylic acid solution in an ice water bath environment for neutralization, so that the pH value of the mixed solution is 7, and then adding 20 g of magnesium aluminum hydrotalcite, wherein the mass ratio of magnesium aluminum hydrotalcite to the mixed solution is 1:5, under the protection of nitrogen atmosphere, ion exchange reaction is carried out at 70° C. for 52 hours, and finally the reaction product is washed and filtered, and the filter cake is dried at 70° C. for 20 hours to obtain intercalated hydrotalcite;
[0068] Step 2.2, placing a four-necked flask equipped with a stirrer, a condenser, a thermometer and a nitrogen tube in ice water, adding acrylic acid solution to the four-necked flask, and adding sodium hydroxide solution dropwise, stirring continuously to neutralize until the neutralization degree reaches 90%, and then adding intercalated hydrotalcite powder and N, N'-methylenebisacrylamide, stirring evenly and placing in an ultrasonic cleaner for 30 minutes of dispersion, and then passing nitrogen into the four-necked flask to exclude oxygen, heating to 75°C, adding potassium persulfate dropwise, stirring until the solution is completely converted into a gel, the reaction is terminated, and a primary product is obtained. The primary product is cut into pieces and placed in a vacuum drying oven at 80°C for 20 hours of vacuum drying to obtain a composite super absorbent resin, wherein the content of intercalated hydrotalcite in the composite super absorbent resin is 12%, the content of N, N'-methylenebisacrylamide is 5%, and the content of potassium persulfate is 10%;
[0069] Step 3, placing an antioxidant and a composite super absorbent resin in a weight ratio of 1:4 in a 100mL beaker, adding 5 times the mass of deionized water to the beaker, using a magnetic stirrer, setting the speed to 200 rpm, stirring at room temperature for 1 hour to mix the antioxidant, the composite super absorbent resin and the deionized water evenly and present a gel state, and then placing it in a vacuum drying oven and vacuum drying it at 40°C until the sample has a constant weight. The dried sample is crushed into a powder with a particle size of 200 mesh, and a sustained-release antioxidant inhibitor is obtained.
[0070] Example 5
[0071] A method for preparing a slow-release antioxidant inhibitor comprises the following steps:
[0072] Step 1, preparing an antioxidant, wherein the antioxidant is formed by molecular modification of anthocyanidins, and the specific process is as follows:
[0073] Step 1.1, placing gallic acid in a vacuum drying oven, drying at 120° C. for 50 hours, drying to constant weight, obtaining anhydrous gallic acid, adding anhydrous gallic acid, propionic anhydride and anhydrous pyridine in a molar ratio of 1:5:5 to a 1000 mL three-necked flask in an ice bath environment, stirring to completely dissolve the gallic acid, then slowly stirring for 20 hours under 25° C. oil bath conditions, the stirrer speed is 200 rpm, so that there is no gallic acid residue in the reaction system, and then adding 5 times the volume of deionized water to the three-necked flask, quickly stirring evenly, the stirrer speed is 550 rpm, and then slowly adding hydrochloric acid solution, adjusting the pH value of the solution in the three-necked flask to 2, stirring until a white precipitate appears in the three-necked flask, standing for 36 hours, and then filtering to collect the white precipitate, and finally washing with 6° C. deionized water, and vacuum drying to constant weight at room temperature, that is, obtaining acylated gallic acid;
[0074] Step 1.2, acylated gallic acid and anhydrous thionyl chloride are added to a 1000 mL round-bottom flask in a molar mass ratio of 1:4, and refluxed in an oil bath at 80° C. with stirring to allow the acylated gallic acid to react completely. The progress of the reaction is tracked by thin layer chromatography (TLC). When no acylated gallic acid is detected, the reaction is completed, and the same volume of dichloromethane is added to the flask to dissolve the reactants. Finally, the thionyl chloride is removed by rotary evaporation at 50° C. to precipitate crystals. The dissolution and evaporation are repeated many times until brown crystals are obtained. The brown crystals are vacuum dried to constant weight to obtain a white powder, namely galloyl chloride;
[0075] Step 1.3, weigh 16.10g of galloyl chloride and dissolve it in 30mL of dioxane, then add 2.87g of anthocyanidin and 4.0mL of pyridine, and stir and reflux for 6h at 50°C, then add 30mL of deionized water and 30mL of anhydrous ethanol through a rotary evaporator under a negative pressure of 0.08Mpa, and evaporate the dioxane and pyridine through a rotary evaporator to obtain product crystals, filter, wash and filter, and finally vacuum dry to constant weight to obtain galloylated anthocyanidin;
[0076] Step 1.4, deacylation reaction of galloylated anthocyanidin, comprising dissolving galloylated anthocyanidin in 20 ml of acetone, wherein the concentration of galloylated anthocyanidin is 42 g / mL, cooling the temperature of the reaction system to 0°C in an ice bath, adding sodium hydroxide solution dropwise with stirring to make the pH value of the reaction system 7, then standing at 0°C for 4 hours, and then adding hydrochloric acid solution to make the pH value of the reaction system 4, distilling off the acetone with a rotary evaporator to obtain a solid substance, filtering the solid substance, and then dissolving the filtered solid in ethyl acetate, wherein the concentration of the filtered solid in the solution is 43 g / mL, washing the ester layer with deionized water, and distilling off the ethyl acetate under reduced pressure to obtain a molecularly modified anthocyanidin, i.e., an antioxidant.
[0077] Step 2, preparing a composite super absorbent resin, the specific process is as follows:
[0078] Step 2.1, hydrotalcite intercalation, measuring 100 mL of 25% acrylic acid solution, adding 30% sodium hydroxide solution to the acrylic acid solution in an ice water bath environment for neutralization, so that the pH value of the mixed solution is 7, and then adding 20 g of magnesium aluminum hydrotalcite, wherein the mass ratio of magnesium aluminum hydrotalcite to the mixed solution is 1:6, under the protection of nitrogen atmosphere, ion exchange reaction is carried out at 80° C. for 60 hours, and finally the reaction product is washed and filtered, and the filter cake is dried at 70° C. for 22 hours to obtain intercalated hydrotalcite;
[0079] Step 2.2, placing a four-necked flask equipped with a stirrer, a condenser, a thermometer and a nitrogen tube in ice water, adding acrylic acid solution to the four-necked flask, and adding sodium hydroxide solution dropwise, stirring continuously to neutralize until the neutralization degree reaches 90%, and then adding intercalated hydrotalcite powder and N, N'-methylenebisacrylamide, stirring evenly and placing in an ultrasonic cleaner for 30 minutes of dispersion, and then passing nitrogen into the four-necked flask to exclude oxygen, heating to 75°C, adding potassium persulfate dropwise, stirring until the solution is completely converted into a gel, the reaction is terminated, and a primary product is obtained. The primary product is cut into pieces and placed in a vacuum drying oven at 80°C for 20 hours of vacuum drying to obtain a composite super absorbent resin, wherein the content of intercalated hydrotalcite in the composite super absorbent resin is 9%, the content of N, N'-methylenebisacrylamide is 5%, and the content of potassium persulfate is 10%;
[0080] Step 3, placing an antioxidant and a composite super absorbent resin in a weight ratio of 1:5 in a 100mL beaker, adding 5 times the mass of deionized water to the beaker, using a magnetic stirrer, setting the speed to 200 rpm, stirring at room temperature for 1 hour to mix the antioxidant, the composite super absorbent resin and the deionized water evenly and present a gel state, and then placing it in a vacuum drying oven and vacuum drying it at 45°C until the sample has a constant weight. The dried sample is crushed into a powder with a particle size of 200 mesh, and a sustained-release antioxidant inhibitor is obtained.
[0081] Example 6
[0082] A method for preparing a slow-release antioxidant inhibitor comprises the following steps:
[0083] Step 1, preparing an antioxidant, the preparation process is the same as in Example 5;
[0084] Step 2, preparing a composite super absorbent resin, the preparation process is the same as in Example 5;
[0085] Step 3, placing an antioxidant and a composite super absorbent resin in a weight ratio of 1:6 in a 100mL beaker, adding 5 times the mass of deionized water to the beaker, using a magnetic stirrer, setting the speed to 200 rpm, stirring at room temperature for 1 hour to mix the antioxidant, the composite super absorbent resin and the deionized water evenly and present a gel state, and then placing it in a vacuum drying oven and vacuum drying it at 40°C until the sample has a constant weight. The dried sample is crushed into a powder with a particle size of 200 mesh, and a slow-release antioxidant inhibitor is obtained.
[0086] Example 7
[0087] A method for preparing a slow-release antioxidant inhibitor comprises the following steps:
[0088] Step 1, preparing an antioxidant, the preparation process is the same as in Example 5;
[0089] Step 2, preparing a composite super absorbent resin, the preparation process is the same as in Example 5;
[0090] Step 3, placing an antioxidant and a composite super absorbent resin in a weight ratio of 1:7 in a 100mL beaker, adding 5 times the mass of deionized water to the beaker, using a magnetic stirrer, setting the speed to 200 rpm, stirring at room temperature for 1 hour to mix the antioxidant, the composite super absorbent resin and the deionized water evenly and present a gel state, and then placing it in a vacuum drying oven and vacuum drying it at 40°C until the sample has a constant weight. The dried sample is crushed into a powder with a particle size of 200 mesh, and a sustained-release antioxidant inhibitor is obtained.
[0091] Comparative Example 1
[0092] A preparation method of a composite super absorbent resin comprises placing a four-necked flask equipped with a stirrer, a condenser, a thermometer and a nitrogen tube in ice water, adding an acrylic acid solution into the four-necked flask, and then adding a sodium hydroxide solution dropwise, stirring continuously for neutralization until the neutralization degree reaches 90%, then adding N, N'-methylenebisacrylamide into the mixed solution, stirring evenly and then placing in an ultrasonic cleaning machine for dispersion for 30 minutes, then introducing nitrogen into the four-necked flask to exclude oxygen, heating to 75°C, and then adding potassium persulfate dropwise, wherein the mass ratio of N, N'-methylenebisacrylamide to potassium persulfate is 2:1, stirring until the solution is completely converted into a gel state, the reaction is terminated, and a primary product is obtained, and the primary product is cut into pieces and placed in a vacuum drying oven at 80°C for vacuum drying for 20 hours to obtain a composite super absorbent resin.
[0093] The antioxidant activity of anthocyanidins and the antioxidant prepared in Example 1 was tested. The free radical elimination performance of anthocyanidins and the antioxidant prepared in Example 1 was compared and analyzed by DPPH spectrometry. The DPPH free radical was configured into a 200 μmol / L ethanol solution, and the anthocyanidins to be tested and the antioxidant prepared in Example 1 were configured into solutions of different concentrations for testing. 2 mL of DPPH ethanol solution and 2 mL of the solution to be tested were added to test tubes, respectively, and the mixture was mixed evenly. The residual amount was tested after standing in a dark place for 30 min.
[0094] The calculation formula of the substance's ability to eliminate DPPH free radicals is as follows:
[0095]
[0096] S A is the DPPH elimination rate, %; A i is the absorbance of the sample at 517 nm, and A0 is the absorbance of the DPPH solution at 517 nm.
[0097] The calculated free radical scavenging rates of anthocyanidins and the antioxidant prepared in Example 1 are shown in Table 1.
[0098] Table 1 Free radical scavenging rate of anthocyanidins and antioxidants prepared in Example 1
[0099]
[0100] It can be seen from Table 1 that anthocyanidin and the antioxidant prepared in Example 1 both have the ability to eliminate DPPH free radicals. By comparing the free radical scavenging rates of anthocyanidin and the antioxidant prepared in Example 1, it is found that at the same concentration, the free radical scavenging rate of the antioxidant prepared in Example 1 is higher than that of anthocyanidin, and with the increase of concentration, the elimination rate of DPPH free radicals is also significantly enhanced, indicating that the antioxidant prepared by the method of the present invention has good antioxidant properties, and its antioxidant properties are significantly improved compared with anthocyanidin.
[0101] Weigh 0.2 g of the composite superabsorbent resin prepared in Comparative Example 1 and Examples 1 to 4 respectively, add them to 500 mL of deionized water at room temperature and pressure to allow the test sample to fully absorb water, filter out excess water with a 200-mesh nylon bag, and weigh the sample to calculate the liquid absorption rate. The calculation formula is as follows:
[0102] Q =( M - M 0) / M 0
[0103] Where Q is the liquid absorption rate of the sample; M is the total mass of the resin after liquid absorption, that is, the mass of the sample after filtering out excess water; M0 is the mass of the dry resin before liquid absorption; and the units of M and M0 are both g.
[0104] Figure 2 The liquid absorption rate comparison chart of the composite super absorbent resin prepared by comparative example 1 (intercalated hydrotalcite content is 0) and examples 1 to 4 is shown in FIG. Figure 2 It can be seen that with the increase of the content of intercalated hydrotalcite, the liquid absorption rate of the prepared composite super absorbent resin increases first and then decreases. When the content of intercalated hydrotalcite is 9%, the liquid absorption rate of the prepared composite super absorbent resin is the largest. This is because as the amount of hydrotalcite added continues to increase, a large number of cross-linking points will be formed on the network structure, and some hydrotalcite will gradually turn into a physical additive and aggregate in the polymer network structure, resulting in a gradual decrease in the water absorption rate of the absorbent material.
[0105] The heat flow curves of the molecularly modified anthocyanin prepared in Example 1 and the slow-release antioxidant inhibitors prepared in Examples 1 to 7 were tested using a DSC differential scanning calorimeter. The test results are as follows: Figure 3 As shown, from Figure 3 It can be seen that when the molecular modified anthocyanin is oxidized and heated to 216°C, it begins to release heat, and the heat is released exponentially as the temperature rises, indicating that at this temperature point the material structure begins to pyrolyze and break, and a strong chemical reaction occurs with oxygen, accompanied by the release of a large amount of heat. This temperature point is the ignition point of the molecular modified anthocyanin.
[0106] The water-absorbing resin modified by hydrotalcite has excellent thermal stability. After the molecular modified anthocyanin is grafted onto the hydrotalcite modified resin, the disadvantage of the low ignition point of the molecular modified anthocyanin is overcome, and a thermally stable protective atmosphere is provided for the molecular modified anthocyanin, so that it can also have a good ability to eliminate free radicals at high temperatures. Figure 3 It can be seen that when the weight ratio of molecular modified anthocyanidin to composite super absorbent resin is 1:5, the slow-release antioxidant inhibitor material is oxidized and heated to 390°C, the chemical structure is pyrolyzed, and a large amount of heat is released. In the temperature range from room temperature to 390°C, the composite material always maintains the phenomenon of endothermic. When the weight ratio of molecular modified anthocyanidin to composite super absorbent resin reaches 1:6, the material is oxidized and heated to 420°C, the structure begins to decompose and oxidize to release heat, and the heat absorption within the endothermic temperature range is always better than the slow-release antioxidant inhibitor prepared by the molecular modified anthocyanidin and composite super absorbent resin weight ratio of 1:5, and the thermal stability is significantly improved. With the continuous increase of the content of hydrotalcite modified resin, the thermal stability of the slow-release antioxidant inhibitor material is gradually enhanced.
[0107] In order to test the effect of the slow-release antioxidant inhibitor of the present invention on inhibiting coal spontaneous combustion, non-sticky coal and long flame coal samples were collected from different coal seam mining areas in the Jurassic period in northern Shaanxi, sealed in sealed plastic bags and brought back to the laboratory, the surface layer was peeled off, and the samples with a particle size of 200 mesh were crushed and sieved. Then, the samples were placed in a vacuum drying oven and dried at room temperature for 24 hours to remove external moisture in the coal; a part of the coal was treated with the slow-release antioxidant inhibitor prepared in Example 6 as the inhibited coal sample, and the other part was untreated as the raw coal sample.
[0108] The DSC differential scanning calorimeter was used to test the characteristic temperature points and heat flux intensities of different coal oxidation. The heat flux intensity curves of raw coal and retardant coal are shown in Figure 4-5 As shown in the figure, according to the trend of heat flow change, the coal oxidation temperature rise process is divided into characteristic temperature points as follows: T1: the initial exothermic temperature of each coal sample, that is, the temperature of the coal sample when heat release begins; T2: the temperature at which the heat flow intensity is zero, that is, the thermal equilibrium shown on the DSC curve; T3: the peak temperature of the heat flow release rate.
[0109] According to the above characteristic temperature points, the heat flow curve of the coal low-temperature oxidation process is divided into four stages: water evaporation and gas desorption stage: from room temperature to T1; slow oxidation stage: from T1 to T2; accelerated oxidation stage: from T2 to T3; rapid oxidation stage: after T3.
[0110] The quantification method of characteristic temperature point values and corresponding heat flux intensity values is used to characterize the thermal effect in the process of inhibiting coal spontaneous combustion. The characteristic temperature points and related heat flux parameters of raw coal and inhibited coal obtained by the experiment are shown in Table 2.
[0111] Table 2 Characteristic temperature points and related heat flow parameters of raw coal and retardant coal
[0112]
[0113] It can be seen from Table 2 that the various characteristic temperature points of the retardant coal after the retardant treatment are delayed and the heat flux intensity decreases compared with the raw coal, indicating that the slow-release antioxidant inhibitor prepared by the present invention can well delay the exothermic oxidation reaction of coal.
Claims
1. Preparation method of slow-release antioxidant inhibitor, It is characterized in that The following steps are involved: Step 1, preparing an antioxidant, wherein the antioxidant is formed by molecularly modifying anthocyanins; The specific process of step 1 is as follows: Step 1.1, protecting the hydroxyl group of gallic acid, comprising mixing anhydrous gallic acid, propionic anhydride and anhydrous pyridine, then adding deionized water to the reaction system, stirring thoroughly, and then adding hydrochloric acid solution to adjust the pH value of the reaction system to 1-2, collecting the white precipitate by suction filtration after standing, washing the product with deionized water, and vacuum drying to constant weight to obtain acylated gallic acid; The step 1.1 comprises adding anhydrous gallic acid, propionic anhydride and anhydrous pyridine in a molar ratio of 1:4-5:4-5 to a three-necked flask in an ice bath environment, stirring to completely dissolve the gallic acid, then adding 5 times the volume of deionized water to the three-necked flask, stirring evenly, and then adding hydrochloric acid solution to make the pH value of the solution in the three-necked flask 1-2, stirring until a white precipitate appears in the three-necked flask, standing for 24h-36h, then collecting the white precipitate by suction filtration, and finally washing with 5-6°C deionized water, and vacuum drying at room temperature to constant weight; Step 1.2, preparing galloyl chloride, adding the acylated gallic acid prepared in step 1.1 into anhydrous thionyl chloride, then adding dichloromethane to dissolve the reactant, then removing the thionyl chloride by rotary evaporation, precipitating crystals, repeatedly dissolving and evaporating, and vacuum drying to constant weight to obtain galloyl chloride; The step 1.2 comprises adding acylated gallic acid to anhydrous thionyl chloride, wherein the molar mass ratio of acylated gallic acid to anhydrous thionyl chloride is 1:3-4, stirring to allow the acylated gallic acid to react completely, adding 1-2 times the volume of dichloromethane to dissolve the reactant, and then removing the thionyl chloride by rotary evaporation with a rotary evaporator to precipitate crystals, repeatedly dissolving and evaporating until brown crystals are obtained, and vacuum drying the brown crystals to constant weight to obtain galloyl chloride; Step 1.3, dissolving galloyl chloride in dioxane, then adding anthocyanidin and pyridine, stirring and reflux reaction for 5 to 8 hours, then adding deionized water and anhydrous ethanol, dioxane and pyridine are evaporated by rotary evaporator to obtain product crystals, filtering, washing and suction filtration, and finally vacuum drying to constant weight to obtain galloylated anthocyanidin; In the step 1.3, galloyl chloride is dissolved in dioxane, wherein the concentration of galloyl chloride is 50-55 g / mL, anthocyanidin and pyridine are added, and the molar ratio of galloyl chloride, anthocyanidin and pyridine is 5:1:5, and then deionized water and anhydrous ethanol are added, and the volume of the added deionized water and anhydrous ethanol is the same as that of the dioxane; Step 1.4, deacylation reaction of galloylated anthocyanidin, comprising dissolving galloylated anthocyanidin in acetone, then adding sodium hydroxide solution dropwise for neutralization, then adding hydrochloric acid solution to adjust the pH value of the reaction system to 3-4, evaporating acetone with a rotary evaporator to obtain a solid substance, filtering the solid substance, dissolving the filtered solid in ethyl acetate, washing the ester layer with deionized water, and evaporating ethyl acetate under reduced pressure to obtain a molecularly modified anthocyanidin, i.e., an antioxidant; In the step 1.4, the galloylated anthocyanidin is dissolved in acetone, wherein the concentration of the galloylated anthocyanidin is 40-45 g / mL, the temperature of the reaction system is cooled to 0°C in an ice bath, sodium hydroxide solution is added dropwise with stirring to adjust the pH value of the reaction system to 7-8, and then the mixture is allowed to stand at 0°C for 3-4 hours, hydrochloric acid solution is added to adjust the pH value of the reaction system to 3-4, acetone is evaporated by a rotary evaporator to obtain a solid substance, the solid substance is filtered, and then the filtered solid is dissolved in ethyl acetate, the concentration of the filtered solid in ethyl acetate is 40-45 g / mL, and finally the ester layer is washed with deionized water; Step 2, preparing a composite super absorbent resin, wherein the composite super absorbent resin is formed by modifying a super absorbent resin with hydrotalcite, and the specific process is as follows: Step 2.1, hydrotalcite intercalation, comprising adding sodium hydroxide solution dropwise to an acrylic acid solution, stirring for neutralization, adding magnesium aluminum hydrotalcite, carrying out ion exchange reaction under nitrogen atmosphere protection, and finally washing, filtering and drying the reaction product to obtain intercalated hydrotalcite; Step 2.2, adding sodium hydroxide solution dropwise to the acrylic acid solution, stirring for neutralization, adding intercalated hydrotalcite and a crosslinking agent, stirring evenly and placing in an ultrasonic cleaner for dispersion, then heating to 75° C., adding an initiator, stirring and reacting fully until the solution is completely converted into a gel state, the reaction is terminated, and a primary product is obtained, the primary product is cut into pieces and dried to obtain a composite super absorbent resin, wherein the content of intercalated hydrotalcite in the composite super absorbent resin is 3-12%, the content of the crosslinking agent is 5%, and the content of the initiator is 10%; Step 3, placing an antioxidant and a composite super absorbent resin in a weight ratio of 1:1 to 7 in a beaker, adding deionized water to the beaker, stirring while adding, so that the antioxidant, the composite super absorbent resin and the deionized water are evenly mixed and present a gel state, and then placing it in a vacuum drying oven and vacuum drying it at a temperature of 40 to 50° C. to obtain a slow-release antioxidant inhibitor.
2. The method for preparing the slow-release antioxidant inhibitor according to claim 1, It is characterized in that In the step 2.1, magnesium aluminum hydrotalcite is added, the mass ratio of magnesium aluminum hydrotalcite to the mixed solution is 1:5-6, and an ion exchange reaction is carried out under the protection of a nitrogen atmosphere. The ion exchange reaction temperature is 65-70° C. and the reaction time is 48h-60h.
3. The method for preparing the slow-release antioxidant inhibitor according to claim 1, It is characterized in that The step 2.2 comprises placing a four-necked flask equipped with a stirrer, a condenser, a thermometer and a nitrogen tube in ice water, adding an acrylic acid solution into the four-necked flask, and then adding a sodium hydroxide solution dropwise, stirring continuously to neutralize until the neutralization degree reaches 90%, then adding intercalated hydrotalcite powder and a cross-linking agent, stirring evenly and placing in an ultrasonic cleaning machine for dispersion, then passing nitrogen into the four-necked flask to remove oxygen in the flask, heating the four-necked flask to 75° C., adding an initiator dropwise, stirring until the solution is completely converted into a gel state, and the reaction is terminated, the cross-linking agent used is N, N'-methylenebisacrylamide, and the initiator used is potassium persulfate.
4. A sustained-release antioxidant inhibitor prepared by the preparation method according to any one of claims 1 to 3.
Citation Information
Patent Citations
Molecular modification method for enhancing biological activity of procyanidine
CN101747308A
Coal spontaneous combustion inhibitor based on rare earth hydrotalcite and preparation method thereof
CN117965180A