A VCSEL chip for releasing oxidation stress and a method for preparing the same
By designing alternating superlattice structure layers in VCSEL devices, oxidation stress is released, solving the problem of oxidation stress accumulation, improving device performance and reliability, and simplifying the process steps.
Patent Information
- Application Number
- CN202411085164.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-08
AI Technical Summary
In existing VCSEL devices, oxidation stress accumulation caused by lattice mismatch during the oxidation process affects the device's operating life and reliability.
By employing alternating growth of the first and second superlattice structure layers, and using a design where the materials of the layers are not identical, oxidation stress is released into the upper and lower superlattice structure layers, thus avoiding stress accumulation and simplifying the process steps.
It effectively relieves oxide layer stress, improves device performance, reduces failure probability, extends service life and reliability, and is compatible with general semiconductor laser device process technology.
Smart Images

Figure CN118610892B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor laser technology, and in particular to a VCSEL chip for releasing oxidation stress and a preparation method thereof. Background Art
[0002] Vertical Cavity Surface Emitting Laser (VCSEL) has the advantages of good beam quality, low threshold current, high frequency regulation, easy two-dimensional array integration and low manufacturing cost. In recent years, with the large-scale application of VCSEL in laser radar, 3D sensing and other fields, VCSEL has attracted more and more attention.
[0003] The current injection hole is an important structure for VCSEL devices to increase current density and achieve laser emission. In the process of AlGaAs-based VCSEL, the semiconductor material with a high Al component in the structure is usually oxidized into insulating Al2O3 material through a high-temperature oxidation process, forming a current injection path with the unoxidized semiconductor material.
[0004] While the oxidation process forms a current injection path within the device structure, it also changes the physical properties of the device material. The lattice constants of insulating Al2O3 materials and high Al component semiconductor materials are different. The lattice mismatch causes lattice stress at the tip of the oxide layer. The lattice deformation under stress can easily form a leakage channel under device operating conditions, reducing the device's operating life and reliability. Summary of the invention
[0005] In order to solve one or more of the above problems, the present application proposes a VCSEL chip that releases oxidation stress and a method for preparing the same.
[0006] According to one aspect of the present application, a VCSEL chip for releasing oxidation stress is provided, comprising:
[0007] substrate;
[0008] A buffer layer, an N-DBR layer, an N-type doping layer, an active region layer, a P-type doping layer, a P-DBR layer and an ohmic contact layer are sequentially grown on one side of the substrate;
[0009] The P-type doped layer includes a first doped layer, a first superlattice structure layer, an oxide layer, a second superlattice structure layer and a second doped layer stacked in sequence, and the first superlattice structure layer and the second superlattice structure layer respectively include two or more material layers grown alternately.
[0010] In some embodiments, the material of the oxide layer is Al x GaAs or AlAs, wherein the value range of x is x greater than 0.9 and x less than 1.
[0011] In some embodiments, the first superlattice structure layer and the second superlattice structure layer each include two or more material layers, and the material of the material layer is Al y GaAs, the values of y in two adjacent material layers in the first superlattice structure layer and the second superlattice structure layer are not equal, and the value range of y is greater than 0 and less than 0.9.
[0012] In some embodiments, the number of the two or more material layers alternately grown in the first superlattice structure layer and the second superlattice structure layer is greater than or equal to 1 and less than or equal to 10.
[0013] In some embodiments, two or more material layers are alternately grown in the first superlattice structure layer and the second superlattice structure layer, and the thickness of each material layer is in the range of 1 nm to 10 nm.
[0014] In some embodiments, the doping types of the first superlattice structure layer and the second superlattice structure layer are unintentional doping or P-type doping.
[0015] In some embodiments, the doping concentration of the first superlattice structure layer and the second superlattice structure layer is in the range of 1×10 16 cm -3 to 1×10 21 cm -3 .
[0016] In some embodiments, the doping concentration of the oxide layer is in the range of 1E16 cm -3 To 1E21cm -3 .
[0017] In some embodiments, when more than one active region layer is provided, the N-type doped layer, the active region layer and the P-type doped layer are periodically provided, and a tunneling junction layer is provided between each period.
[0018] According to another aspect of the present application, a method for preparing a VCSEL chip for releasing oxidation stress is provided, which is used to prepare any of the above VCSEL chips for releasing oxidation stress, comprising the following steps:
[0019] providing a substrate;
[0020] A buffer layer, an N-DBR layer, an N-type doping layer, an active region layer, a P-type doping layer, a P-DBR layer and an ohmic contact layer are sequentially grown on the substrate;
[0021] The P-type doped layer includes a first doped layer, a first superlattice structure layer, an oxide layer, a second superlattice structure layer and a second doped layer stacked in sequence, and the first superlattice structure layer and the second superlattice structure layer respectively include two or more material layers grown alternately.
[0022] The present application discloses a VCSEL chip for releasing oxidation stress and a preparation method thereof, which effectively relieves the stress of the oxide layer in the device without changing the device process conditions, and does not require stress release means such as post-process treatment, thereby simplifying the process steps and improving production efficiency and product yield; the tunneling effect of the first superlattice structure layer and the second superlattice structure layer can avoid the increase of series resistance caused by high Al component semiconductor materials, and effectively improve the performance of the device; the chip structure is simple, can be compatible with the process of general semiconductor laser devices, and can be widely used in all oxide-limited laser manufacturing fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A schematic structural diagram of a VCSEL chip for releasing oxidation stress provided in one embodiment of the present application.
[0024] Figure 2 A schematic structural diagram of a first superlattice structure layer, an oxide layer, and a second superlattice structure layer in a VCSEL chip for releasing oxidation stress provided in one embodiment of the present application.
[0025] Figure 3 A schematic diagram of the structure of another VCSEL chip for releasing oxidation stress provided in an embodiment of the present application.
[0026] Figure 4 A schematic diagram of the epitaxial structure obtained in step 2 of a method for preparing a VCSEL chip for releasing oxidation stress provided in an embodiment of the present application.
[0027] Figure 5 A schematic diagram of the epitaxial structure obtained in step 4 of a method for preparing a VCSEL chip for releasing oxidation stress provided in one embodiment of the present application.
[0028] Figure 6 A schematic diagram of the epitaxial structure obtained in step 5 of a method for preparing a VCSEL chip for releasing oxidation stress provided in one embodiment of the present application. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are part of the embodiments of the present invention, rather than all of the embodiments, and are only used to explain the present invention, and are not used to limit the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0030] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "front", "back", "vertical", "horizontal", "inner", "outer", "two ends", "both sides", "bottom", "top" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the referred elements must have a specific orientation or be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", "superior", "inferior", "primary", "secondary" and the like are only used for descriptive purposes and can be simply used to more clearly distinguish different components, but cannot be understood as indicating or implying relative importance.
[0031] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, an integral connection, a mechanical connection, an electrical connection, a direct connection, an indirect connection through an intermediate medium, or the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0032] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0033] Embodiment 1:
[0034] Reference Manual Attached Figure 1-2 , showing that an embodiment of the present invention provides a VCSEL chip for releasing oxidation stress, including:
[0035] Substrate 111;
[0036] A buffer layer 112, an N-DBR layer 113, an N-type doping layer 114, an active region layer 115, a P-type doping layer, a P-DBR layer 118 and an ohmic contact layer 119 grown sequentially on one side of the substrate 111;
[0037] The P-type doped layer includes a first doped layer 1161, a first superlattice structure layer 1171, an oxide layer 1172, a second superlattice structure layer 1173, and a second doped layer 1162 stacked in sequence, and the first superlattice structure layer 1171 and the second superlattice structure layer 1173 respectively include two or more material layers grown alternately;
[0038] A P-side metal layer 120 is disposed on a side of the ohmic contact layer 119 away from the substrate 111 , and an N-side metal layer 121 is disposed on a side of the substrate 111 away from the buffer layer 112 .
[0039] The first superlattice structure layer 1171 and the second superlattice structure layer 1173 each include more than two material layers, and the material of the material layer is Al y GaAs, the values of y in the two adjacent material layers in the first superlattice structure layer and the second superlattice structure layer are not equal, and the value range of y is greater than 0 and less than 0.9. Therefore, the material layers, stacked structures, total number of layers and total thickness used in the first superlattice structure layer 1171 and the second superlattice structure layer 1173 are not required to be completely consistent. The materials of the two adjacent material layers in the first superlattice structure layer 1171 and the second superlattice structure layer 1173 are different, which can meet the requirements of releasing oxidation stress.
[0040] For example, the first superlattice structure layer 1171 may include a first material layer, a second material layer and a third material layer; the second superlattice structure layer 1173 may include a first material layer and a second material layer, wherein the materials of the first material layer, the second material layer and the third material layer are respectively Al y1 GaAs, Al y2 GaAs and Al y3 For GaAs, the value ranges of y1, y2 and y3 are all greater than 0 and less than 0.9.
[0041] In a possible embodiment, the first superlattice structure layer 1171 can be stacked with a first material layer, a second material layer, a third material layer, a second material layer and a first material layer in sequence, and the second superlattice structure layer 1173 can be stacked with a first material layer, a second material layer, a first material layer and a second material layer in sequence. At this time, the values of y1 and y2 are not equal, and the values of y2 and y3 are not equal.
[0042] Specifically, under the premise of ensuring that the materials of the two adjacent material layers in the first superlattice structure layer 1171 and the second superlattice structure layer 1173 are inconsistent, there is no requirement for the stacking order of the material layers. The thickness of each material layer can be equal or unequal; the number of each material layer can be the same or different. Therefore, under the premise of effectively releasing the oxidation stress, the process difficulty can be further reduced.
[0043] In an optional embodiment, the material selected for each material layer in the first superlattice structure layer 1171 may be completely identical, partially identical, or completely different from the material selected for each material layer in the second superlattice structure layer 1173 .
[0044] In an alternative embodiment, the material of the oxide layer 1172 may be Al x GaAs or AlAs, wherein the value range of x is x greater than 0.9 and x less than 1.
[0045] In an optional embodiment, the material of the first doping layer 1161 and the second doping layer 1162 can be selected from AlGaAs, or gradient AlGaAs, or a combination of AlGaAs with different components, the doping type is p-type, and the doping concentration can be 1E16cm -3 To 1E19cm -3 The material and thickness of the first doping layer 1161 and the second doping layer 1162 may be the same, thereby making epitaxial growth simpler.
[0046] In an optional embodiment, two or more material layers are alternately grown in the first superlattice structure layer 1171 and the second superlattice structure layer 1173 , and the number of each material layer is greater than or equal to 1 and less than or equal to 10.
[0047] In an optional embodiment, two or more material layers are alternately grown in the first superlattice structure layer 1171 and the second superlattice structure layer 1173 , and the layer thickness of each material layer ranges from 1 nm to 10 nm, including the endpoints.
[0048] Under the condition that the total thickness of the N-type doped layer 114, the active area layer 115 and the P-type doped layer satisfies an integer multiple of half the optical thickness of the chip, the more layers of each material in the first superlattice structure layer 1171 and the second superlattice structure layer 1173, the better the stress release effect.
[0049] In an optional embodiment, the doping type of the first superlattice structure layer 1171 and the second superlattice structure layer 1173 is unintentional doping or P-type doping.
[0050] In an optional embodiment, the doping concentration of the first superlattice structure layer 1171 and the second superlattice structure layer 1173 is in the range of 1E16 cm -3 To 1E21cm -3 .
[0051] In an optional embodiment, the doping concentration of the oxide layer 1172 is in the range of 1E16 cm -3 To 1E21cm -3 .
[0052] In an optional embodiment, when more than one active region layer 115 is provided in the VCSEL chip, the N-type doped layer 114, the active region layer 115 and the P-type doped layer are periodically provided, and a tunneling junction layer 122 is provided between each period. Figure 3, shows a schematic structural diagram of another VCSEL chip for releasing oxidation stress, wherein the number of active region layers 115 is 2, and a buffer layer 112, an N-DBR layer 113, an N-type doped layer 114, an active region layer 115, a P-type doped layer, a tunnel junction layer 122, an N-type doped layer 114, an active region layer 115, a P-type doped layer, a P-DBR layer 118 and an ohmic contact layer 119 are sequentially arranged on one side of the substrate 111.
[0053] The present application discloses a VCSEL chip for releasing oxidation stress. Without changing the device process conditions, the material stress caused by the oxidation process is released into the superlattice structure layer to avoid the phenomenon of stress accumulation, effectively relieve the stress of the oxide layer in the device, and relax the stress into the upper and lower superlattice structure layers while ensuring the normal current limiting capability. There is no need to adopt stress release means such as post-process treatment, simplify the process steps, improve production efficiency, reduce the failure probability of the device, and improve the service life and reliability of the device. The tunneling effect of the first superlattice structure layer and the second superlattice structure layer can avoid the increase of series resistance caused by high Al component semiconductor materials, and effectively improve the performance of the device. The chip has a simple structure and is compatible with the process of general semiconductor laser devices, and can be widely used in all oxide-limited laser manufacturing fields.
[0054] Embodiment 2:
[0055] An embodiment of the present invention further provides a method for preparing a VCSEL chip for releasing oxidation stress, which is applied to any one of the VCSEL chips for releasing oxidation stress in the above embodiments, and comprises the following steps:
[0056] Step 1: providing a substrate;
[0057] Step 2: On the substrate, a buffer layer, an N-DBR layer, an N-type doped layer, an active region layer, a P-type doped layer, a P-DBR layer and an ohmic contact layer are sequentially grown. Figure 4 , showing a schematic diagram of the epitaxial structure obtained in step 2;
[0058] The P-type doped layer includes a first doped layer, a first superlattice structure layer, an oxide layer, a second superlattice structure layer, and a second doped layer which are sequentially arranged. In the present embodiment, the first superlattice structure layer and the second superlattice structure layer respectively include two material layers which are grown alternately. In a possible embodiment, the first superlattice structure layer and the second superlattice structure layer may also include multiple material layers which are grown alternately.
[0059] Step 3: using photolithography, metal evaporation, etching, and stripping techniques to evaporate a p-side patterned metal electrode on the epitaxial structure obtained in step 2, and growing a dielectric film for protection;
[0060] Step 4: The epitaxial structure obtained in step 3 is subjected to photolithography, exposure and development processes to expose the mesa etching area, and the semiconductor material is etched by ICP to form a mesa structure. The damaged layer is etched by wet processing. Refer to the attached manual Figure 5 , showing a schematic diagram of the epitaxial structure obtained in step 4;
[0061] Step 5: Place the wet-etched cleaned sample into a high-temperature oxidation furnace to oxidize the exposed high-Al component material into Al2O3 to form a current injection hole. Figure 6 , showing a schematic diagram of the epitaxial structure obtained in step 5;
[0062] Step 6: Using photolithography, etching, thin film deposition and evaporation processes, a passivation layer is continued to be grown on the epitaxial wafer obtained in step 5, a P-side electrode window is opened in the P-side metal layer, and an N-side metal layer is evaporated. The obtained epitaxial wafer is annealed at 420°C for 30s in a nitrogen environment to form an N-type ohmic contact, thereby preparing a VCSEL chip that releases oxidation stress.
[0063] The substrate provided in step 1 may be a GaAs substrate.
[0064] In step 2, sequentially growing a buffer layer, an N-DBR layer, an N-type doped layer, an active region layer, a P-type doped layer, a P-DBR layer and an ohmic contact layer on the substrate may specifically include:
[0065] The substrate is placed in a reaction furnace, which may be a CVD, MOCVD or MBE reaction furnace capable of achieving epitaxial growth;
[0066] A buffer layer, an N-DBR layer, an N-type doping layer, an active region layer, a P-type doping layer, a P-DBR layer and an ohmic contact layer are sequentially grown on the substrate.
[0067] In an optional embodiment, the first superlattice structure layer and the second superlattice structure layer respectively include more than two material layers, and the material of the material layer is Al y GaAs, the values of y in two adjacent material layers in the first superlattice structure layer and the second superlattice structure layer are not equal, and the value range of y is greater than 0 and less than 0.9.
[0068] In an optional embodiment, the material of the oxide layer may be Al x GaAs or AlAs, wherein the value range of x is x greater than 0.9 and x less than 1, and the thickness of the oxide layer can be 5-30 nm.
[0069] In an optional embodiment, the material of the first doping layer and the second doping layer can be selected from AlGaAs, or gradient AlGaAs, or a combination of AlGaAs with different components, the doping type is p-type, and the doping concentration can be 1E16cm-3 To 1E19cm -3 In this embodiment, the material of the first doping layer and the second doping layer is AlGaAs, and the doping concentration is 1E18cm -3 .
[0070] In an optional embodiment, the number of two or more material layers alternately grown in the first superlattice structure layer and the second superlattice structure layer is greater than or equal to 1 and less than or equal to 10.
[0071] In an optional embodiment, two or more material layers are alternately grown in the first superlattice structure layer and the second superlattice structure layer, and the layer thickness of each material layer is in the range of 1 nm-10 nm, including the endpoints.
[0072] In an optional embodiment, the doping types of the first superlattice structure layer and the second superlattice structure layer are unintentional doping or P-type doping.
[0073] In an optional embodiment, the doping concentration range of the first superlattice structure layer and the second superlattice structure layer is 1E16cm -3 To 1E21cm -3 .
[0074] In an optional embodiment, the doping concentration of the oxide layer is in the range of 1E16 cm -3 To 1E21cm -3 .
[0075] In an optional embodiment, in step 3, the metal electrode can be a Ti / Pt / Au metal electrode, each metal can be deposited by electron beam evaporation, the thickness of the metal can be 20nm, 30nm and 150nm respectively, and metal patterning can be achieved by degumming.
[0076] The dielectric film material can be grown by PECVD or ALD. The dielectric film material can be SiO2, SiN or Al2O3, and the thickness can be 20-100 nm.
[0077] In an optional embodiment, in step 4, the etching mask may be a photoresist, the ICP etching gas may be SiCl 4 or BCl 3 , and the wet treatment solution may be a weak acid or a weak base, such as aqueous ammonia.
[0078] In an optional embodiment, the thickness of the buffer layer may be 300 nm, and the material of the buffer layer may be GaAs; the N-DBR layer and the P-DBR layer may each include 40 pairs of Al 0.9 GaAs / Al 0.12GaAs material layer; the active region layer may include three pairs of InGaAs / AlGaAs material layers; the material of the first doping layer and the second doping layer in the P-type doping layer may be GaAs.
[0079] In this embodiment, the material of the material layer in the first superlattice structure layer and the second superlattice structure layer may be Al 0.7 GaAs and Al 0.2 GaAs, in the first superlattice structure layer, the number of the two material layers is set to 3 layers, and the thickness of each layer is 5nm; in the second superlattice structure layer, the number of the two material layers is set to 3 layers, and the thickness of each layer is 5nm.
[0080] The material of the oxide layer can be Al 0.98 For GaAs, the oxide layer thickness can be 20 nm.
[0081] The present application discloses a method for preparing a VCSEL chip for releasing oxidation stress. Without changing the device process conditions, the material stress caused by the oxidation process is released into the superlattice structure layer to avoid the phenomenon of stress accumulation, effectively relieve the stress of the oxide layer in the device, and relax the stress into the upper and lower superlattice structure layers while ensuring the normal current limiting capability. There is no need to adopt stress release means such as post-process treatment, simplify the process steps, improve production efficiency, reduce the failure probability of the device, and improve the service life and reliability of the device. The tunneling effect of the first superlattice structure layer and the second superlattice structure layer can avoid the increase of series resistance caused by high Al component semiconductor materials, and effectively improve the performance of the device. The chip structure is simple, compatible with the process of general semiconductor laser devices, and can be widely used in all oxide-limited laser manufacturing fields.
[0082] The above is only an optional implementation of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application. These improvements and modifications should also be regarded as the scope of protection of the present application.
Claims
1. A VCSEL chip for releasing oxidation stress, characterized in that: include: substrate; A buffer layer, an N-DBR layer, an N-type doping layer, an active region layer, a P-type doping layer, a P-DBR layer and an ohmic contact layer grown in sequence on one side of the substrate; The P-type doped layer comprises a first doped layer, a first superlattice structure layer, an oxide layer, a second superlattice structure layer and a second doped layer stacked in sequence, and the first superlattice structure layer and the second superlattice structure layer respectively comprise two or more material layers grown alternately; The first superlattice structure layer and the second superlattice structure layer each include more than two material layers, and the material of the material layer is Al y GaAs, the values of y in two adjacent material layers in the first superlattice structure layer and the second superlattice structure layer are not equal, and the value range of y is greater than 0 and less than 0.
9.
2. A VCSEL chip for releasing oxidation stress according to claim 1, characterized in that: The material of the oxide layer is Al x GaAs or AlAs, wherein the value range of x is x greater than 0.9 and x less than 1.
3. A VCSEL chip for releasing oxidation stress according to claim 1, characterized in that: The number of the two or more material layers alternately grown in the first superlattice structure layer and the second superlattice structure layer is greater than or equal to 1 and less than or equal to 10.
4. A VCSEL chip for releasing oxidation stress according to claim 1, characterized in that: The two or more material layers alternately grown in the first superlattice structure layer and the second superlattice structure layer have a layer thickness of each material layer ranging from 1 nm to 10 nm.
5. A VCSEL chip for releasing oxidation stress according to claim 1, characterized in that: The doping types of the first superlattice structure layer and the second superlattice structure layer are unintentional doping or P-type doping.
6. A VCSEL chip for releasing oxidation stress according to claim 1, characterized in that: The doping concentration range of the first superlattice structure layer and the second superlattice structure layer is 1E16cm -3 To 1E21cm -3 .
7. A VCSEL chip for releasing oxidation stress according to claim 1, characterized in that: The doping concentration of the oxide layer is in the range of 1E16cm -3 To 1E21cm -3 .
8. The VCSEL chip for releasing oxidation stress according to claim 1, characterized in that: When more than one active region layer is provided, the N-type doped layer, the active region layer and the P-type doped layer are periodically provided, and a tunneling junction layer is provided between each period.
9. A method for preparing a VCSEL chip for releasing oxidation stress, used for preparing a VCSEL chip for releasing oxidation stress according to any one of claims 1 to 8, characterized in that: The following steps are involved: providing a substrate; A buffer layer, an N-DBR layer, an N-type doping layer, an active region layer, a P-type doping layer, a P-DBR layer and an ohmic contact layer are sequentially grown on the substrate; The P-type doped layer includes a first doped layer, a first superlattice structure layer, an oxide layer, a second superlattice structure layer and a second doped layer stacked in sequence, and the first superlattice structure layer and the second superlattice structure layer respectively include two or more material layers grown alternately.