A special mortar for energy-saving buildings and preparation method thereof

By using N-alkylated-O-quaternary chitosan on expanded perlite to form a pore sealing film, the problems of leakage of organic phase change materials and high water absorption rate of expanded perlite are solved, and the thermal inertia of the mortar is significantly improved and energy-saving effects.

CN118619623BActive Publication Date: 2024-12-06CHONGQING LEFAN ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410724979.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-12-06
Estimated Expiration
2044-06-06

AI Technical Summary

Technical Problem

Organic phase change materials are prone to leakage in expanded perlite pores, and the water absorption rate of expanded perlite is high, resulting in poor energy saving effect.

Method used

N-alkylated-O-quaternary chitosan is used to seal the expanded perlite to form a hydrophilic and hydrophobic sealing film on the inner side to prevent leakage of organic phase change materials and moisture infiltration.

Benefits of technology

It significantly improves the leakage phenomenon of organic phase change materials, reduces the water absorption rate of expanded perlite, and improves the thermal inertia and energy-saving effect of the mortar.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118619623B_ABST
    Figure CN118619623B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of new materials and the technical field of energy-saving, and provides a special mortar for energy-saving buildings and a preparation method thereof. The method first uses expanded perlite as a carrier to adsorb an organic phase change material, then seals the expanded perlite with N-alkylated-O-quaternary ammonium salt chitosan to obtain a phase change aggregate, and then mixes the phase change aggregate with cement, fly ash, redispersible latex powder, water and additives to prepare a special mortar for energy-saving buildings. The use of this mortar can significantly improve the thermal inertia of the building, reduce indoor temperature fluctuations, and achieve excellent energy-saving effects. In addition, by sealing the expanded perlite with N-alkylated-O-quaternary ammonium salt chitosan, not only the leakage phenomenon of the organic phase change material is significantly improved, but also the water absorption rate of the expanded perlite can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of new materials and the technical field of energy conservation, and provides a special mortar for energy-saving buildings and a preparation method thereof. Background Art

[0002] With the development of social economy and the improvement of people's living standards, the building energy consumption required to ensure indoor air quality has shown a rapid upward trend. In the building energy consumption, air conditioning energy consumption accounts for about 2 / 3. The development of energy-saving buildings is of great significance for saving energy and protecting the environment.

[0003] Mortar is an important building material. Adding thermal insulation materials to mortar can make it suitable for energy-saving buildings. The combination of traditional thermal insulation materials and phase change energy storage materials, while utilizing the thermal insulation function of porous materials and the energy storage function of phase change materials, can significantly improve the thermal inertia of buildings, reduce indoor temperature fluctuations, and achieve better energy-saving effects.

[0004] Compared with inorganic phase change materials, organic phase change materials have the advantages of no corrosion, no supercooling, stable properties, etc., and are more suitable for building energy conservation. Expanded perlite itself has a honeycomb porous structure, large specific surface area, non-toxic and tasteless, corrosion resistance, light specific gravity, heat insulation and sound absorption, and its pores have strong adsorption capacity, so it can be used as a carrier of organic phase change materials.

[0005] There have been studies that load organic phase change materials into the pores of expanded perlite and then add them to mortar. After the mortar is constructed, it can adjust the indoor temperature. However, this technology also has defects. For example, when the organic phase change material changes state, it is easy to leak out from the pores of expanded perlite. In addition, expanded perlite has the defect of high water absorption rate.

[0006] In order to solve the leakage problem of organic phase change materials, Yu Yongsheng's research used ultrafine bentonite to seal the expanded perlite. The specific method is to first use the vacuum adsorption method to adsorb the molten organic phase change material into the pores of the expanded perlite, and then after cooling, mix the dry ultrafine bentonite into the expanded perlite under a vacuum environment, take it out and sieve it. This method has played a good role in improving the leakage of phase change materials, but there is still room for improvement. Summary of the invention

[0007] In order to better solve the problem that organic phase change materials are easy to leak out from the pores of expanded perlite and the water absorption rate of expanded perlite is high, the present invention proposes a special mortar for energy-saving buildings and a preparation method thereof, which not only significantly improves the leakage phenomenon of organic phase change materials, but also reduces the water absorption rate of expanded perlite.

[0008] The specific technical solutions involved in the present invention are as follows:

[0009] Firstly, the present invention proposes a special mortar for energy-saving buildings, wherein the components of the special mortar include cement, phase change aggregate, fly ash, redispersible latex powder, air entraining agent, water reducing agent, starch ether, methyl cellulose ether and water.

[0010] As a preferred embodiment of the present invention, the special mortar comprises, by weight, 100 parts of cement, 50-70 parts of phase change aggregate, 10-20 parts of fly ash, 2-4 parts of redispersible latex powder, 0.08-0.12 parts of air entraining agent, 0.8-1.2 parts of water reducer, 0.6-0.8 parts of starch ether, 0.5-0.6 parts of methyl cellulose ether and 90-100 parts of water.

[0011] In the scheme of the present invention, the phase change aggregate plays a key role in the energy saving of the mortar, and the selection of other components is not particularly limited. Preferably, the cement is silicate cement or ordinary silicate cement; the air entraining agent is an alkylbenzene sulfonate air entraining agent; the water reducer is a polycarboxylic acid high-efficiency water reducer; the starch ether is hydroxypropyl starch ether; and the methyl cellulose ether is hydroxypropyl methyl cellulose ether.

[0012] In the mortar component of the present invention, the preparation method of the phase change aggregate is: first, the organic phase change material is adsorbed on the expanded perlite as a carrier, and then the expanded perlite is sealed with N-alkylated-O-quaternary ammonium salt chitosan. Preferably, in the phase change aggregate, the mass ratio of the expanded perlite, the organic phase change material, and the N-alkylated-O-quaternary ammonium salt chitosan is 100:40-60:5-10.

[0013] The particle size and porosity of expanded perlite not only affect the mortar performance, but also affect its adsorption capacity for organic phase change materials. As a preferred embodiment of the present invention, the particle size of the expanded perlite is 20-60 meshes and the porosity is 60-80%.

[0014] For the selection of organic phase change materials, certain principles should be followed. For example, the phase change temperature of the phase change material should meet the needs of the application site. For energy-saving buildings, it is appropriate to be between 20-28°C; the phase change latent heat is large, and the heat absorption and release are smooth; there is no supercooling phenomenon or the supercooling is very small; there is no melting phenomenon; the volume expansion rate is low; safety and stability are good. According to some existing research results, it is found that binary or ternary composite phase change systems are more suitable for energy-saving buildings. As a preferred embodiment of the present invention, the organic phase change material is a mixture of decanoic acid and dodecanoic acid in a mass ratio of 40:60 (the phase change temperature is about 25°C), or a mixture of octadecane, dodecanoic acid, and stearic acid in a mass ratio of 50:40:10 (the phase change temperature is about 28°C), or a mixture of dodecanoic acid, hexadecanoic acid, and tetradecanoic acid in a mass ratio of 60:20:20 (the phase change temperature is about 27°C).

[0015] The present invention creatively seals the expanded perlite with N-alkylated-O-quaternary ammonium salt chitosan on the basis of using expanded perlite to adsorb and load organic phase change materials. It is well known that in the chitosan structure, the amino group on C2 and the hydroxyl group on C6 can react to connect other groups, thereby realizing the modification of chitosan. N-alkylated-O-quaternary ammonium salt chitosan is a chitosan derivative obtained by replacing the H of the amino group with an alkyl group and replacing the H of the hydroxyl group with a group containing a quaternary ammonium salt.

[0016] Preferably, the structural formula of the N-alkylated-O-quaternary ammonium salt chitosan is as shown in the attached figure. Figure 1 The preparation method thereof can refer to the prior art, preferably refer to method 2.2 in Ye Hui's "Preparation of Amphiphilic N-Alkylated-O-Quaternary Ammonium Salt Chitosan and Research on Its Use as Drug / Gene Carrier".

[0017] Preferably, the specific preparation process of the phase change aggregate is:

[0018] (1) adding an organic phase change material to a pear-shaped bottle, heating it in a water bath until the phase change material is completely melted, adding expanded perlite to the pear-shaped bottle, evacuating the bottle for 20-40 minutes, and then opening a valve to allow air to enter the pear-shaped bottle. The phase change material enters the micropores of the expanded perlite under the action of the air pressure difference, cooling to room temperature, and discharging the material to obtain expanded perlite adsorbing the phase change material;

[0019] (2) N-alkylated-O-quaternary ammonium salt chitosan and deionized water are added to a container, ultrasonically treated for 20-40 minutes, then spray-deposited on the surface of expanded perlite that adsorbs the phase change material, and then vacuum-dried to obtain a phase change aggregate.

[0020] Preferably, in the above step (2), the mass ratio of N-alkylated-O-quaternary ammonium salt chitosan to deionized water is 0.5-2:100.

[0021] The present invention creatively uses N-alkylated-O-quaternary ammonium salt chitosan to seal the expanded perlite adsorbing organic phase change material, which can not only significantly improve the leakage of the organic phase change material, but also reduce the water absorption rate of the expanded perlite. The principle is:

[0022] N-alkylated-O-quaternary ammonium salt chitosan is an amphiphilic material, the alkyl group gives it lipophilicity, the quaternary ammonium salt gives it hydrophilicity, and the quaternary ammonium salt part of the material is positively charged. When N-alkylated-O-quaternary ammonium salt chitosan is deposited on the surface of expanded perlite, chitosan forms a film on the surface of expanded perlite to achieve pore sealing. During the deposition process, since the surface of expanded perlite is negatively charged, according to the principle of mutual attraction of heterogeneous charges, N-alkylated-O-quaternary ammonium salt chitosan tends to be deposited in the following manner: the quaternary ammonium salt part with positive charge (i.e., the hydrophilic part) tends to be located on the inner side of the film (i.e., in contact with the expanded perlite), while the lipophilic alkyl part tends to be located on the outer side of the film, that is, N-alkylated-O-quaternary ammonium salt chitosan forms a pore sealing film with a hydrophilic inner side and a hydrophobic outer side on the surface of the expanded perlite adsorbed with the organic phase change material. Thus, on the one hand, the inner side of the sealing membrane is hydrophilic, which is more conducive to preventing the hydrophobic organic phase change material in the pores of the expanded perlite from leaking out; on the other hand, the outer side of the sealing membrane is hydrophobic, which is conducive to preventing water from penetrating into the pores of the expanded perlite. Therefore, the present invention can significantly improve the leakage of the organic phase change material and reduce the water absorption rate of the expanded perlite by using N-alkylated-O-quaternary ammonium salt chitosan.

[0023] In addition, compared with the prior art of using ultrafine bentonite to seal expanded perlite, the method of the present invention has the following advantages: first, the surface of the ultrafine bentonite in the method is negatively charged and cannot form electrostatic adsorption with the expanded perlite with the same negative charge, so it only achieves end-capping through pore adsorption, while the N-alkylated-O-quaternary ammonium salt chitosan of the present invention has the dual effects of pore adsorption and electrostatic adsorption, so it can achieve a more solid end-capping effect. Second, the ultrafine bentonite in the method is discontinuous and has gaps, while the N-alkylated-O-quaternary ammonium salt chitosan of the present invention seals the expanded perlite by film formation. Since the film layer has continuity, it can better prevent the leakage of organic phase change materials and the infiltration of water.

[0024] The present invention also provides a method for preparing the special mortar for energy-saving buildings, comprising the following preparation steps:

[0025] (1) Add cement and fly ash into a mixer and mix for 1-3 minutes;

[0026] (2) Add redispersible latex powder, air entraining agent, water reducing agent, starch ether and methyl cellulose ether into a blender and mix for 2-4 minutes;

[0027] (3) Add phase change aggregate into a mixer and mix for 1-2 minutes;

[0028] (4) Slowly add water into the blender and mix well.

[0029] As can be seen from the above, the present invention provides a special mortar for energy-saving buildings and a preparation method thereof, which has the following beneficial effects:

[0030] First, the present invention forms a hydrophilic sealing film on the surface of expanded perlite by N-alkylated-O-quaternary ammonium salt chitosan, which can significantly prevent the hydrophobic organic phase change material in the pores of expanded perlite from seeping out. Second, the present invention forms a hydrophobic sealing film on the surface of expanded perlite by N-alkylated-O-quaternary ammonium salt chitosan, which can prevent external moisture from penetrating into the pores of expanded perlite. Third, the quaternary ammonium salt part of the N-alkylated-O-quaternary ammonium salt chitosan of the present invention has a positive charge, and the surface of expanded perlite has a negative charge, and the two form electrostatic adsorption, which can achieve a more solid end-capping effect. Fourth, the sealing film formed by the N-alkylated-O-quaternary ammonium salt chitosan on the surface of expanded perlite of the present invention has continuity, which can better prevent the outward leakage of organic phase change materials and the inward infiltration of moisture. In summary, the method of the present invention not only significantly improves the leakage phenomenon of organic phase change materials, but also reduces the water absorption rate of expanded perlite. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 is the structural formula of N-alkylated-O-quaternary ammonium salt chitosan used in the examples. DETAILED DESCRIPTION

[0032] The present invention is further described in detail below through specific embodiments, but this should not be construed as limiting the scope of the present invention to the following examples. Without departing from the above-mentioned method concept of the present invention, various substitutions or changes made according to common technical knowledge and conventional means in the art should be included in the scope of the present invention.

[0033] Description of raw materials: In the following examples and comparative examples, the cement is ordinary Portland cement PO 42.5, purchased from Xi'an Linya Cement Sales Co., Ltd.; the air entraining agent is sodium dodecylbenzene sulfonate, purchased from Nanjing Milan New Materials Co., Ltd.; the water reducer is polycarboxylic acid high-efficiency water reducer, purchased from Langfang Longteng New Materials Co., Ltd.; the starch ether is hydroxypropyl starch ether, purchased from Beijing Yiwei New Materials Technology Co., Ltd.; the methyl cellulose ether is hydroxypropyl methyl cellulose ether, purchased from Shanghai Shenye Industrial Co., Ltd.; the expanded perlite was purchased from Chengdu Jinliushun Building Materials Co., Ltd., with a particle size range of 30-50 mesh, an SiO2 content of 86%, and a porosity of about 65%; the other raw materials and reagents involved are all common chemical products.

[0034] Example 1

[0035] First, according to the method 2.2 in Ye Hui's "Preparation of Amphiphilic N-Alkyl-O-Quaternary Chitosan and Research on Its Use as Drug / Gene Carrier", 3-chloro-2-hydroxypropyltrimethylammonium chloride was used as a quaternary ammonium salt reagent to prepare O-quaternary chitosan; then the chitosan was deacetylated to obtain O-quaternary chitosan; further, decanal was used as an alkylating reagent to obtain N-alkyl-O-quaternary chitosan, whose structural formula is shown in the attached figure. Figure 1 ;

[0036] Then, the phase change aggregate is prepared according to the following steps:

[0037] (1) adding an organic phase change material into a pear-shaped bottle, rotating and heating in a water bath until the phase change material is completely melted, adding expanded perlite into the pear-shaped bottle, first evacuating the bottle for 30 minutes, then opening a valve to allow air to enter the pear-shaped bottle, and allowing the phase change material to enter the micropores of the expanded perlite under the action of the air pressure difference, cooling to room temperature, and discharging the material to obtain expanded perlite adsorbing the phase change material;

[0038] (2) adding N-alkylated-O-quaternary ammonium salt chitosan and deionized water into a container, ultrasonically treating for 30 minutes, then spraying and depositing on the surface of expanded perlite adsorbing the phase change material, and then vacuum drying to obtain a phase change aggregate;

[0039] in:

[0040] The organic phase change material is a mixture of decanoic acid and dodecanoic acid in a mass ratio of 40:60;

[0041] The mass ratio of expanded perlite, organic phase change material, and N-alkylated-O-quaternary ammonium salt chitosan is 100:50:10; the mass ratio of N-alkylated-O-quaternary ammonium salt chitosan and deionized water is 1:100;

[0042] Finally, prepare the mortar as follows:

[0043] (1) Add cement and fly ash into a mixer and mix for 2 minutes;

[0044] (2) Add redispersible latex powder, air entraining agent, water reducing agent, starch ether and methyl cellulose ether into a blender and mix for 3 minutes;

[0045] (3) Add phase change aggregate into the mixer and mix for 2 minutes;

[0046] (4) Slowly add water into the blender and mix well;

[0047] in:

[0048] The components are calculated by weight: 100 parts of cement, 60 parts of phase change aggregate, 15 parts of fly ash, 3 parts of redispersible latex powder, 0.1 parts of air entraining agent, 1 part of water reducing agent, 0.7 parts of starch ether, 0.55 parts of methyl cellulose ether, and 95 parts of water.

[0049] Example 2

[0050] First, according to the method 2.2 in Ye Hui's "Preparation of Amphiphilic N-Alkyl-O-Quaternary Chitosan and Research on Its Use as Drug / Gene Carrier", 3-chloro-2-hydroxypropyltrimethylammonium chloride was used as a quaternary ammonium salt reagent to prepare O-quaternary chitosan; then the chitosan was deacetylated to obtain O-quaternary chitosan; further, decanal was used as an alkylating reagent to obtain N-alkyl-O-quaternary chitosan, whose structural formula is shown in the attached figure. Figure 1 ;

[0051] Then, the phase change aggregate is prepared according to the following steps:

[0052] (1) adding an organic phase change material into a pear-shaped bottle, rotating and heating in a water bath until the phase change material is completely melted, adding expanded perlite into the pear-shaped bottle, first evacuating the bottle for 30 minutes, then opening a valve to allow air to enter the pear-shaped bottle, and allowing the phase change material to enter the micropores of the expanded perlite under the action of the air pressure difference, cooling to room temperature, and discharging the material to obtain expanded perlite adsorbing the phase change material;

[0053] (2) adding N-alkylated-O-quaternary ammonium salt chitosan and deionized water into a container, ultrasonically treating for 30 minutes, then spraying and depositing on the surface of expanded perlite adsorbing the phase change material, and then vacuum drying to obtain a phase change aggregate;

[0054] in:

[0055] The organic phase change material is a mixture of decanoic acid and dodecanoic acid in a mass ratio of 40:60;

[0056] The mass ratio of expanded perlite, organic phase change material, and N-alkylated-O-quaternary ammonium salt chitosan is 100:50:5; the mass ratio of N-alkylated-O-quaternary ammonium salt chitosan and deionized water is 1:100;

[0057] Finally, prepare the mortar as follows:

[0058] (1) Add cement and fly ash into a mixer and mix for 2 minutes;

[0059] (2) Add redispersible latex powder, air entraining agent, water reducing agent, starch ether and methyl cellulose ether into a blender and mix for 3 minutes;

[0060] (3) Add phase change aggregate into the mixer and mix for 2 minutes;

[0061] (4) Slowly add water into the blender and mix well;

[0062] in:

[0063] The components are calculated by weight: 100 parts of cement, 60 parts of phase change aggregate, 15 parts of fly ash, 3 parts of redispersible latex powder, 0.1 parts of air entraining agent, 1 part of water reducing agent, 0.7 parts of starch ether, 0.55 parts of methyl cellulose ether, and 95 parts of water.

[0064] Example 3

[0065] First, according to the method 2.2 in Ye Hui's "Preparation of Amphiphilic N-Alkyl-O-Quaternary Chitosan and Research on Its Use as Drug / Gene Carrier", 3-chloro-2-hydroxypropyltrimethylammonium chloride was used as a quaternary ammonium salt reagent to prepare O-quaternary chitosan; then the chitosan was deacetylated to obtain O-quaternary chitosan; further, decanal was used as an alkylating reagent to obtain N-alkyl-O-quaternary chitosan, whose structural formula is shown in the attached figure. Figure 1 ;

[0066] Then, the phase change aggregate is prepared according to the following steps:

[0067] (1) adding an organic phase change material into a pear-shaped bottle, rotating and heating in a water bath until the phase change material is completely melted, adding expanded perlite into the pear-shaped bottle, first evacuating the bottle for 30 minutes, then opening a valve to allow air to enter the pear-shaped bottle, and allowing the phase change material to enter the micropores of the expanded perlite under the action of the air pressure difference, cooling to room temperature, and discharging the material to obtain expanded perlite adsorbing the phase change material;

[0068] (2) adding N-alkylated-O-quaternary ammonium salt chitosan and deionized water into a container, ultrasonically treating for 30 minutes, then spraying and depositing on the surface of expanded perlite adsorbing the phase change material, and then vacuum drying to obtain a phase change aggregate;

[0069] in:

[0070] The organic phase change material is a mixture of octadecane, dodecanoic acid and stearic acid in a mass ratio of 50:40:10;

[0071] The mass ratio of expanded perlite, organic phase change material, and N-alkylated-O-quaternary ammonium salt chitosan is 100:50:10; the mass ratio of N-alkylated-O-quaternary ammonium salt chitosan and deionized water is 1:100;

[0072] Finally, prepare the mortar as follows:

[0073] (1) Add cement and fly ash into a mixer and mix for 2 minutes;

[0074] (2) Add redispersible latex powder, air entraining agent, water reducing agent, starch ether and methyl cellulose ether into a blender and mix for 3 minutes;

[0075] (3) Add phase change aggregate into a mixer and mix for 2 minutes;

[0076] (4) Slowly add water into the blender and mix well;

[0077] in:

[0078] The components are calculated by weight: 100 parts of cement, 60 parts of phase change aggregate, 15 parts of fly ash, 3 parts of redispersible latex powder, 0.1 parts of air entraining agent, 1 part of water reducing agent, 0.7 parts of starch ether, 0.55 parts of methyl cellulose ether, and 95 parts of water.

[0079] Example 4

[0080] First, according to the method 2.2 in Ye Hui's "Preparation of Amphiphilic N-Alkyl-O-Quaternary Chitosan and Research on Its Use as Drug / Gene Carrier", 3-chloro-2-hydroxypropyltrimethylammonium chloride was used as a quaternary reagent to prepare O-quaternary chitosan; then the chitosan was deacetylated to obtain O-quaternary chitosan; further, decanal was used as an alkylating reagent to obtain N-alkyl-O-quaternary chitosan, whose structural formula is shown in the attached figure. Figure 1 ;

[0081] Then, the phase change aggregate is prepared according to the following steps:

[0082] (1) adding an organic phase change material into a pear-shaped bottle, rotating and heating in a water bath until the phase change material is completely melted, adding expanded perlite into the pear-shaped bottle, first evacuating the bottle for 30 minutes, then opening a valve to allow air to enter the pear-shaped bottle, and allowing the phase change material to enter the micropores of the expanded perlite under the action of the air pressure difference, cooling to room temperature, and discharging the material to obtain expanded perlite adsorbing the phase change material;

[0083] (2) adding N-alkylated-O-quaternary ammonium salt chitosan and deionized water into a container, ultrasonically treating for 30 minutes, then spraying and depositing on the surface of expanded perlite adsorbing the phase change material, and then vacuum drying to obtain a phase change aggregate;

[0084] in:

[0085] The organic phase change material is a mixture of octadecane, dodecanoic acid and stearic acid in a mass ratio of 50:40:10;

[0086] The mass ratio of expanded perlite, organic phase change material, and N-alkylated-O-quaternary ammonium salt chitosan is 100:50:5; the mass ratio of N-alkylated-O-quaternary ammonium salt chitosan and deionized water is 1:100;

[0087] Finally, prepare the mortar as follows:

[0088] (1) Add cement and fly ash into a mixer and mix for 2 minutes;

[0089] (2) Add redispersible latex powder, air entraining agent, water reducing agent, starch ether and methyl cellulose ether into a blender and mix for 3 minutes;

[0090] (3) Add phase change aggregate into the mixer and mix for 2 minutes;

[0091] (4) Slowly add water into the blender and mix well;

[0092] in:

[0093] The components are calculated by weight: 100 parts of cement, 60 parts of phase change aggregate, 15 parts of fly ash, 3 parts of redispersible latex powder, 0.1 parts of air entraining agent, 1 part of water reducing agent, 0.7 parts of starch ether, 0.55 parts of methyl cellulose ether, and 95 parts of water.

[0094] Example 5

[0095] First, according to the method 2.2 in Ye Hui's "Preparation of Amphiphilic N-Alkyl-O-Quaternary Chitosan and Research on Its Use as Drug / Gene Carrier", 3-chloro-2-hydroxypropyltrimethylammonium chloride was used as a quaternary ammonium salt reagent to prepare O-quaternary chitosan; then the chitosan was deacetylated to obtain O-quaternary chitosan; further, decanal was used as an alkylating reagent to obtain N-alkyl-O-quaternary chitosan, whose structural formula is shown in the attached figure. Figure 1 ;

[0096] Then, the phase change aggregate is prepared according to the following steps:

[0097] (1) adding an organic phase change material into a pear-shaped bottle, rotating and heating in a water bath until the phase change material is completely melted, adding expanded perlite into the pear-shaped bottle, first evacuating the bottle for 30 minutes, then opening a valve to allow air to enter the pear-shaped bottle, and allowing the phase change material to enter the micropores of the expanded perlite under the action of the air pressure difference, cooling to room temperature, and discharging the material to obtain expanded perlite adsorbing the phase change material;

[0098] (2) adding N-alkylated-O-quaternary ammonium salt chitosan and deionized water into a container, ultrasonically treating for 30 minutes, then spraying and depositing on the surface of expanded perlite adsorbing the phase change material, and then vacuum drying to obtain a phase change aggregate;

[0099] in:

[0100] The organic phase change material is a mixture of dodecanoic acid, hexadecanoic acid and tetradecanoic acid in a mass ratio of 60:20:20;

[0101] The mass ratio of expanded perlite, organic phase change material, and N-alkylated-O-quaternary ammonium salt chitosan is 100:50:10; the mass ratio of N-alkylated-O-quaternary ammonium salt chitosan and deionized water is 1:100;

[0102] Finally, prepare the mortar as follows:

[0103] (1) Add cement and fly ash into a mixer and mix for 2 minutes;

[0104] (2) Add redispersible latex powder, air entraining agent, water reducing agent, starch ether and methyl cellulose ether into a blender and mix for 3 minutes;

[0105] (3) Add phase change aggregate into the mixer and mix for 2 minutes;

[0106] (4) Slowly add water into the blender and mix well;

[0107] in:

[0108] The components are calculated by weight: 100 parts of cement, 60 parts of phase change aggregate, 15 parts of fly ash, 3 parts of redispersible latex powder, 0.1 parts of air entraining agent, 1 part of water reducing agent, 0.7 parts of starch ether, 0.55 parts of methyl cellulose ether, and 95 parts of water.

[0109] Example 6

[0110] First, according to the method 2.2 in Ye Hui's "Preparation of Amphiphilic N-Alkyl-O-Quaternary Chitosan and Research on Its Use as Drug / Gene Carrier", 3-chloro-2-hydroxypropyltrimethylammonium chloride was used as a quaternary ammonium salt reagent to prepare O-quaternary chitosan; then the chitosan was deacetylated to obtain O-quaternary chitosan; further, decanal was used as an alkylating reagent to obtain N-alkyl-O-quaternary chitosan, whose structural formula is shown in the attached figure. Figure 1 ;

[0111] Then, the phase change aggregate is prepared according to the following steps:

[0112] (1) adding an organic phase change material into a pear-shaped bottle, rotating and heating in a water bath until the phase change material is completely melted, adding expanded perlite into the pear-shaped bottle, first evacuating the bottle for 30 minutes, then opening a valve to allow air to enter the pear-shaped bottle, and allowing the phase change material to enter the micropores of the expanded perlite under the action of the air pressure difference, cooling to room temperature, and discharging the material to obtain expanded perlite adsorbing the phase change material;

[0113] (2) adding N-alkylated-O-quaternary ammonium salt chitosan and deionized water into a container, ultrasonically treating for 30 minutes, then spraying and depositing on the surface of expanded perlite adsorbing the phase change material, and then vacuum drying to obtain a phase change aggregate;

[0114] in:

[0115] The organic phase change material is a mixture of dodecanoic acid, hexadecanoic acid and tetradecanoic acid in a mass ratio of 60:20:20;

[0116] The mass ratio of expanded perlite, organic phase change material, and N-alkylated-O-quaternary ammonium salt chitosan is 100:50:5; the mass ratio of N-alkylated-O-quaternary ammonium salt chitosan and deionized water is 1:100;

[0117] Finally, prepare the mortar as follows:

[0118] (1) Add cement and fly ash into a mixer and mix for 2 minutes;

[0119] (2) Add redispersible latex powder, air entraining agent, water reducing agent, starch ether and methyl cellulose ether into a blender and mix for 3 minutes;

[0120] (3) Add phase change aggregate into the mixer and mix for 2 minutes;

[0121] (4) Slowly add water into the blender and mix well;

[0122] in:

[0123] The components are calculated by weight: 100 parts of cement, 60 parts of phase change aggregate, 15 parts of fly ash, 3 parts of redispersible latex powder, 0.1 parts of air entraining agent, 1 part of water reducing agent, 0.7 parts of starch ether, 0.55 parts of methyl cellulose ether, and 95 parts of water.

[0124] Comparative Example 1

[0125] Unloaded, unsealed expanded perlite was directly added to replace the phase change aggregate in Example 6, and other preparation conditions were consistent with Example 6.

[0126] Comparative Example 2

[0127] Compared with Example 6, only expanded perlite is used to adsorb the organic phase change material, and N-alkylated-O-quaternary ammonium chitosan is not used to seal the expanded perlite. Other preparation conditions are consistent with those in Example 6.

[0128] Comparative Example 3

[0129] After the expanded perlite adsorbs the organic phase change material, the expanded perlite is capped with ultrafine bentonite according to the method 3.2 in Yu Yongsheng's "Preparation and Application Research of Perlite Composite Phase Change Energy Storage Materials", and the amount of ultrafine bentonite is 5% of the mass of the expanded perlite. Other preparation conditions are consistent with Example 6.

[0130] Performance Test:

[0131] (1) Thermal insulation performance test: The mortars prepared in Examples 1-6 and Comparative Example 1 were respectively made into mortar boards with a length of 200 mm, a width of 200 mm, and a thickness of 30 mm. The mortar boards and 5 polystyrene boards of the same size were used to construct a cubic closed space with a side length of 200 mm. A thermometer was installed at the center of the closed space, and the mortar board was heated by a heating table. The thermometer reading was recorded every 5 minutes. The initial temperature was 25°C, and the heating rate of the heating table was 1°C / 8 minutes. When the temperature reached 50°C, the heating was stopped, and the thermometer reading was continuously recorded within 3 hours thereafter. The maximum value T of the central temperature reached can be obtained by the thermometer reading. m , and the time t required to reach the highest value. The results are shown in Table 1;

[0132] (2) Anti-leakage performance test: Using the diffusion-seepage circle method, take a filter paper with a diameter of 12.5 cm, and define a test area with a diameter of 2 cm in the center. Disperse 10 g of the phase change aggregates prepared in Examples 5-6 and Comparative Examples 2-3 evenly in the test area, place in an oven, heat at 60°C for 24 hours, take out, measure the maximum diameter and minimum diameter of the seepage circle formed by the phase change component seeping out of the test area, and the average value of the two is the average diameter of the seepage circle; then calculate the seepage percentage according to the following formula: Seepage percentage = (average diameter of the seepage circle - diameter of the test area) × 100% / diameter of the test area. The results are shown in Table 2;

[0133] (3) Aggregate water absorption test: The phase change aggregates prepared in Examples 5-6 and Comparative Examples 2-3 were respectively placed in non-water-absorbent mesh bags, which were completely immersed in water and prevented from floating on the water surface with the help of tools. The bags were taken out after 1 hour and naturally hung to dry for 30 minutes. The water absorption was calculated according to the following formula: Water absorption = (mass after water absorption - mass before water absorption) × 100% / mass before water absorption.

[0134] It can be seen from Tables 1-3 that: (1) The present invention can significantly improve the thermal inertia of the mortar after molding, reduce the temperature fluctuation of the internal space, and significantly improve the energy-saving effect of the building by using expanded perlite to adsorb the organic phase change material; (2) The present invention can significantly improve the phenomenon of leakage of the organic phase change material in the pores of the expanded perlite by sealing the pores of the expanded perlite by N-alkylated-O-quaternary ammonium salt chitosan; (3) The present invention can also significantly reduce the water absorption rate of the expanded perlite by sealing the pores of the expanded perlite by N-alkylated-O-quaternary ammonium salt chitosan.

[0135] Table 1:

[0136] Performance Indicators Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Comparative Example 1 <![CDATA[T m (℃)]]> 29.2 29.1 31.5 31.3 30.6 30.4 38.6 t(min) 300 300 285 285 290 290 255

[0137] Table 2:

[0138] Performance Indicators Example 5 Example 6 Comparative Example 2 Comparative Example 3 Percentage of exudation (%) 5.5 7.1 21.7 12.4

[0139] Table 3:

[0140] Performance Indicators Example 5 Example 6 Comparative Example 2 Comparative Example 3 Water absorption (%) 24.9 32.1 77.5 42.8

Claims

1. A special mortar for energy-saving buildings, the components of which include cement, phase change aggregate, fly ash, redispersible latex powder, air entraining agent, water reducing agent, starch ether, methyl cellulose ether, and water, characterized in that: The preparation method of the phase change aggregate is as follows: firstly, the organic phase change material is adsorbed by using expanded perlite as a carrier, and then the expanded perlite is sealed by using N-alkylated-O-quaternary ammonium salt chitosan.

2. The special mortar for energy-saving buildings according to claim 1, characterized in that: In the special mortar, the components are, by weight, 100 parts of cement, 50-70 parts of phase change aggregate, 10-20 parts of fly ash, 2-4 parts of redispersible latex powder, 0.08-0.12 parts of air entraining agent, 0.8-1.2 parts of water reducer, 0.6-0.8 parts of starch ether, 0.5-0.6 parts of methyl cellulose ether, and 90-100 parts of water.

3. The special mortar for energy-saving buildings according to claim 1, characterized in that: The cement is silicate cement or ordinary silicate cement; The air entraining agent is an alkylbenzene sulfonate air entraining agent; The water reducer is a polycarboxylic acid high-efficiency water reducer; The starch ether is hydroxypropyl starch ether; The methyl cellulose ether is hydroxypropyl methyl cellulose ether.

4. The special mortar for energy-saving buildings according to claim 1, characterized in that: The expanded pearlite has a particle size of 20-60 meshes and a porosity of 60-80%.

5. The special mortar for energy-saving buildings according to claim 1, characterized in that: The organic phase change material is a mixture of decanoic acid and dodecanoic acid in a mass ratio of 40:60, or a mixture of octadecane, dodecanoic acid and stearic acid in a mass ratio of 50:40:10, or a mixture of dodecanoic acid, hexadecanoic acid and tetradecanoic acid in a mass ratio of 60:20:

20.

6. The special mortar for energy-saving buildings according to claim 1, characterized in that: The structural formula of the N-alkylated-O-quaternary ammonium salt chitosan is 7. The special mortar for energy-saving buildings according to claim 1, characterized in that: In the phase change aggregate, the mass ratio of expanded perlite, organic phase change material and N-alkylated-O-quaternary ammonium salt chitosan is 100:40-60:5-10.

8. The special mortar for energy-saving buildings according to claim 1, characterized in that: The specific preparation process of the phase change aggregate is as follows: (1) adding an organic phase change material to a pear-shaped bottle, heating it in a water bath until the phase change material is completely melted, adding expanded perlite to the pear-shaped bottle, evacuating the bottle for 20-40 minutes, and then opening a valve to allow air to enter the pear-shaped bottle. The phase change material enters the micropores of the expanded perlite under the action of the air pressure difference, cooling to room temperature, and discharging the material to obtain expanded perlite adsorbing the phase change material; (2) N-alkylated-O-quaternary ammonium salt chitosan and deionized water are added to a container, ultrasonically treated for 20-40 minutes, then spray-deposited on the surface of expanded perlite that adsorbs the phase change material, and then vacuum-dried to obtain a phase change aggregate.

9. The special mortar for energy-saving buildings according to claim 8, characterized in that: The mass ratio of N-alkylated-O-quaternary ammonium salt chitosan to deionized water is 0.5-2:

100.

10. A method for preparing a special mortar for energy-saving buildings according to any one of claims 1 to 9, characterized in that: The method comprises the following preparation steps: (1) Add cement and fly ash into a mixer and mix for 1-3 minutes; (2) Add redispersible latex powder, air entraining agent, water reducing agent, starch ether and methyl cellulose ether into a blender and mix for 2-4 minutes; (3) Add phase change aggregate into a mixer and mix for 1-2 minutes; (4) Slowly add water into the blender and mix well.