A microporous corundum brick and its preparation method
By using modified phenolic resin and specific raw materials, microporous corundum bricks with excellent slag resistance, alkali resistance and thermal shock resistance are prepared, which solves the insufficient thermal stability and slag resistance of microporous corundum bricks in the prior art. The problem of this achieves higher overall performance.
Patent Information
- Application Number
- CN202410644987.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-05-23
AI Technical Summary
The existing microporous corundum bricks lack thermal stability during high-temperature firing, which affects their comprehensive performance, and have poor alkali and slag resistance, making it difficult to replace French ceramic cup bricks.
Brown corundum and dense white corundum are used as the main raw materials, alumina powder, silicon carbide, and metal silicon powder are used as additives, and modified phenolic resin is used as the binding agent. By reasonably controlling the proportion of raw materials and the dosage of bonding agents, a good strength is prepared. Microporous corundum bricks with slag resistance, iron corrosion resistance, alkali resistance and thermal shock resistance.
It significantly improves the comprehensive performance of microporous corundum bricks, including improving compressive strength, slag resistance, alkali resistance and thermal shock resistance. The high residual carbon content and good dispersion of modified phenolic resin ensure the compactness of the bricks. and mechanical properties.
Smart Images

Figure CN118619691B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of refractory materials, and in particular relates to a microporous corundum brick and a preparation method thereof. Background Art
[0002] Corundum bricks are widely used in linings and kiln tools of various high-temperature kilns such as iron-making blast furnaces, blast furnace hot blast furnaces, steel-making refining furnaces, glass melting furnaces, and petrochemical industrial furnaces because of their excellent properties such as high hardness, corrosion resistance, high temperature resistance, wear resistance, and impact resistance. Among them, microporous corundum bricks are made of fused dense corundum and fused brown corundum as raw materials, with special additives and binders, and adopt a special microporous production process, which is molded and fired at high temperature. When microporous corundum bricks are used as bricks for blast furnace ceramic cups, they are required to have good alkali resistance, slag resistance, and iron corrosion resistance. Compared with the expensive French ceramic cup bricks, the microporous corundum bricks manufactured by domestic technology have relatively poor alkali resistance and slag resistance, poor micropore effect, and many disadvantages. Therefore, the development of microporous corundum bricks with better comprehensive performance is crucial to replace French ceramic cup bricks.
[0003] Chinese patent CN110483023B discloses a microporous corundum brick and its preparation method, wherein the main raw materials are 75-95% dense corundum, 0-10% andalusite, 0-8% silicon carbide, 3-5% combined clay powder and 0.4-2% metallic silicon powder; phenolic resin is used as a binder, the above raw materials are mixed in a specific order, pressed into a brick blank, dried and fired to obtain the obtained microporous corundum brick; the room temperature compressive strength range of the obtained microporous corundum brick is too large, the performance is unstable, and the alkali resistance and slag resistance of the microporous corundum brick have not been tested; Chinese patent CN116947522A discloses a Microporous corundum bricks and preparation method thereof, the microporous corundum bricks are prepared from raw materials including granular materials, fine powders and resin binders; the granular materials are corundum particles; the fine powders include corundum fine powders, alumina powders, metallic silicon powders, ferrosilicon nitride, carbon black and binding clay; the resin binder is a thermosetting phenolic resin; by adjusting the product formula, introducing metallic silicon powders, ferrosilicon nitride, nano-scale carbon black, alumina powders and binding clays, and limiting the particle size range of the raw material components, the obtained microporous corundum bricks have good resistance to slag, alkali and molten iron corrosion, and have good thermal shock resistance, but their compressive strength is insufficient and there is a large room for improvement.
[0004] The above patents all use conventional phenolic resin as a binder. Due to the presence of a large number of phenolic hydroxyl groups in its structure, it is easy to break at a certain temperature, resulting in a decrease in its thermal stability, which affects the use effect during high-temperature firing, and further affects the comprehensive performance of the microporous corundum brick. Therefore, it is necessary to further improve the thermal stability of the phenolic resin binder and apply it to microporous corundum bricks to obtain microporous corundum bricks with excellent comprehensive performance. Summary of the invention
[0005] The purpose of the present invention is to provide a microporous corundum brick and a preparation method thereof in view of the deficiencies in the prior art. Brown corundum and dense white corundum are used as the main raw materials of the microporous corundum brick, alumina powder, silicon carbide and metallic silicon powder are used as additives, and modified phenolic resin with excellent performance is used as a binder. By reasonably controlling the ratio of each raw material and the amount of the binder, a microporous corundum brick with good strength, slag resistance, iron liquid corrosion resistance, alkali resistance and thermal shock resistance is obtained.
[0006] The technical solution adopted by the present invention to achieve the above-mentioned purpose is:
[0007] A microporous corundum brick, comprising the following raw materials in percentage by mass: 28-35% brown corundum; 52-60% dense white corundum; 3-5% alumina powder; 6-8% silicon carbide; 1-2% metallic silicon powder; the microporous corundum brick also comprises 2-3% of the total weight of the raw materials in terms of modified phenolic resin;
[0008] Furthermore, the Al2O3 in the brown corundum is ≥95%; the brown corundum is composed of particles with a particle size of 5-3 mm and particles with a particle size of 3-1 mm in a mass ratio of 1.5-2:1.
[0009] Furthermore, the Al2O3 in the dense white corundum is ≥95%; the dense white corundum is composed of particles with a particle size of 3-1mm, particles with a particle size of 1-0mm, and fine powder with a particle size of 320 mesh in a mass ratio of 1.5-2:1:2.5-3.
[0010] Furthermore, the alumina powder is α-alumina powder with a particle size of ≤5um; the particle size of silicon carbide is 200 mesh; and the particle size of metallic silicon powder is ≤0.045mm.
[0011] Furthermore, the preparation method of the modified phenolic resin is:
[0012] S1. Add ethanol aqueous solution and modified silane to a reaction container, adjust the pH value to 4-5 with acetic acid, and stir for 5-6 hours to obtain a modified silane hydrolyzate; the volume ratio of ethanol to water in the ethanol aqueous solution is 8-9:1; the amount of the modified silane added is 8-10% of the mass of the ethanol aqueous solution;
[0013] S2, adding modified silane hydrolyzate and nano silicon nitride to a reaction container, after uniform dispersion, heating to 60-70°C, reacting for 3-4h, centrifuging after the reaction is completed, washing the precipitate with acetone, and drying to obtain modified nano silicon nitride; the amount of nano silicon nitride added is 10-15% of the mass of the modified silane hydrolyzate;
[0014] S3. Add phenol, formaldehyde and sodium hydroxide to a reaction container, heat to 50-60°C, stir for 20-30 minutes to obtain a mixed solution, add modified nano silicon nitride, adjust the pH of the modified silane hydrolyzate to be the same as that of the mixed solution, and then slowly add it dropwise to the mixed solution. After the dropwise addition, heat to 85-95°C and react for 1.5-2 hours. After the reaction is completed, use acetic acid to adjust the pH to neutral, vacuum dehydrate, and obtain a modified phenolic resin; the molar ratio of the phenol, formaldehyde, and sodium hydroxide is 1:1.2-1.3:0.02-0.03; the amount of the modified nano silicon nitride added is 8-10% of the mass of the mixed solution; the amount of the modified silane hydrolyzate added is 15-20% of the mass of the mixed solution.
[0015] Furthermore, the preparation method of the modified silane in step S1 is:
[0016] (1) Add anhydrous dichloromethane and 3-aminopropyltriethoxysilane to a reaction vessel, stir evenly, and dropwise add an anhydrous dichloromethane solution containing 4-chloromethylbenzoyl chloride under nitrogen protection. After the dropwise addition, raise the temperature to 30-35° C. and react for 3-4 hours. After the reaction is completed, remove the dichloromethane by vacuum distillation to obtain chloro-silane, the chemical structure of which is:
[0017] The molar ratio of 3-aminopropyltriethoxysilane to 4-chloromethylbenzoyl chloride is 1:1-1.1;
[0018] (2) adding anhydrous ethanol, chlorosilane and dodecyldimethyl tertiary amine to a reaction vessel, and reflux reacting for 10-12 hours. After the reaction is completed, removing ethanol by vacuum distillation to obtain modified silane having the chemical formula:
[0019] The molar ratio of the chlorosilane to dodecyldimethyl tertiary amine is 1:1-1.1.
[0020] The present invention also provides a method for preparing microporous corundum bricks, comprising the following steps: mixing brown corundum and dense white corundum according to a mass ratio for 2-3 minutes, adding modified phenolic resin, stirring for 3-5 minutes, adding alumina powder, silicon carbide, and metallic silicon powder, and mixing and grinding for 10-15 minutes to obtain a mixture; pressing the mixture into a shape by a machine, drying, and obtaining a brick blank; and sintering the brick blank at 1450-1470°C for 35-40 hours to obtain a microporous corundum brick.
[0021] The present invention has the following beneficial effects:
[0022] In order to obtain a modified phenolic resin binder with high residual carbon content, good mechanical properties and good heat resistance, the present invention adopts modified silane and modified silicon nitride to modify the phenolic resin. The structures of the modified silane and the modified silicon nitride both contain long-chain quaternary ammonium salt and rigid benzene ring group with good dispersing effect, so that the hydrolyzed modified silane can be uniformly dispersed in the system and react with free phenol, which is helpful to increase the solid content and tensile strength. The modified silicon nitride can also have better dispersibility and be uniformly dispersed in the system, so as to prevent the modified silicon nitride from agglomerating, thereby greatly improving the residual carbon content, mechanical properties and heat resistance of the phenolic resin.
[0023] The present invention further uses modified phenolic resin as a binder for microporous corundum bricks. On the one hand, the modified silicon nitride and silicon carbide contained in the modified phenolic resin can also work together to improve the strength, corrosion resistance and thermal shock resistance of the microporous corundum bricks. On the other hand, the modified phenolic resin contains long-chain quaternary ammonium salt groups with good dispersing effect, which is beneficial to the dispersion of various raw materials, has good bonding effect, and helps to form a solid brick structure. In addition, the modified phenolic resin has a high residual carbon content, good mechanical properties, good heat resistance, and generates less gaseous substances during high-temperature firing. The formed carbon layer can be further combined with other raw materials, thereby increasing the density of the brick structure, thereby effectively improving the comprehensive performance of the microporous corundum bricks.
[0024] The invention uses brown corundum and dense white corundum as main raw materials of microporous corundum bricks, alumina micropowder, silicon carbide and metallic silicon micropowder as additives, and modified phenolic resin with excellent performance as a binder. By reasonably controlling the ratio of various raw materials and the amount of the binder, microporous corundum bricks with good strength, slag resistance, iron liquid corrosion resistance, alkali resistance and thermal shock resistance are prepared. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a SEM picture of the microporous corundum brick prepared in the present invention, in which 1 is the corundum particles and 2 is the matrix part. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0027] In the technical scheme of the present invention, all chemical reagents in the following embodiments and comparative examples are commonly available on the market, among which phenol CAS No. 108-95-2; formaldehyde CAS No. 50-00-0; sodium hydroxide CAS No. 1310-73-2; acetic acid CAS No. 64-19-7; acetic acid CAS No. 64-19-7; 3-aminopropyltriethoxysilane CAS No. 919-30-2; 4-chloromethylbenzoyl chloride CAS No. 876-08-4; dodecyldimethyl tertiary amine CAS No. 112-18-5; acetone CAS No. 67-64-1; dichloromethane CAS No. 75-09-2; ethanol CAS No. 64-17-5.
[0028] In the technical solution of the present invention, the preparation method of modified silane is:
[0029] (1) Synthesis of chlorosilane
[0030]
[0031] Add 400 mL of anhydrous dichloromethane and 22.0 g of 3-aminopropyltriethoxysilane to the reaction vessel, stir evenly, and under nitrogen protection, dropwise add 100 mL of anhydrous dichloromethane solution containing 18.8 g of 4-chloromethylbenzoyl chloride. After the dropwise addition, heat to 35 ° C. and react for 3 h. After the reaction is completed, remove dichloromethane by vacuum distillation to obtain 32.6 g of chloro-silane; the molar ratio of 3-aminopropyltriethoxysilane to 4-chloromethylbenzoyl chloride is 1:1; chloro-silane: ESI (m / z): 374.9 [M+H] + , 1 H-NMR (600MHz, DMSO-d6, δppm): 8.50 (s, 1H), 7.92 (d, J=8.5Hz, 2H), 7.46 (d, J=8.5Hz, 2H), 4.64 (s, 2H ), 3.82-3.86 (m, 6H), 3.42-3.45 (m, 2H), 1.55-1.58 (m, 2H), 1.21 (d, J=7.2Hz, 9H), 0.54-0.57 (m, 2H).
[0032] (2) Synthesis of modified silane
[0033]
[0034] 350 mL of anhydrous ethanol, 25.0 g of chloro-silane and 14.3 g of dodecyl dimethyl tertiary amine were added to the reaction vessel, and the reaction was refluxed for 12 h. After the reaction was completed, ethanol was removed by vacuum distillation to obtain 34.5 g of modified silane; the molar ratio of chloro-silane to dodecyl dimethyl tertiary amine was 1:1; modified silane: ESI (m / z): 588.3 [M+H] + ,1 H-NMR (600MHz, DMSO-d6, δppm): 8.48 (s, 1H), 7.84 (d, J=8.5Hz, 2H), 7.34 (d, J=8.5Hz, 2H), 4.50 (s, 2H), 3.83-3.86 (m, 6H), 3.43-3.46 (m, 2H), 3.30 (s, 6H), 3.22-3.25 (m, 2H), 1.71-1.74 (m, 2H), 1.55-1.58 (m, 2H), 1.23-1.29 (m, 27H), 0.88 (d, J=6.8Hz, 3H), 0.56-0.58 (m, 2H).
[0035] Example 1
[0036] A microporous corundum brick comprises the following raw materials in percentage by weight: 30% brown corundum; 57% dense white corundum; 5% alumina micropowder; 6% silicon carbide; 2% metallic silicon micropowder; and 3% modified phenolic resin by weight of the total weight of the raw materials.
[0037] The Al2O3 in brown corundum is ≥95%; brown corundum is composed of particles with a particle size of 5-3mm and particles with a particle size of 3-1mm in a mass ratio of 2:1; the Al2O3 in dense white corundum is ≥95%; dense white corundum is composed of particles with a particle size of 3-1mm, particles with a particle size of 1-0mm, and fine powder with a particle size of 320 mesh in a mass ratio of 2:1:2.7; alumina micropowder is α-alumina micropowder with a particle size of 5um; the particle size of silicon carbide is 200 mesh; the particle size of metallic silicon micropowder is 0.045mm.
[0038] A preparation method of microporous corundum bricks, comprising the following steps: mixing brown corundum and dense white corundum according to mass ratio for 3 minutes, adding modified phenolic resin, stirring for 3 minutes, adding alumina powder, silicon carbide, and metal silicon powder, and mixing and grinding for 15 minutes to obtain a mixed material; pressing the mixed material into a shape by a machine, drying, and obtaining a brick; sintering the brick at 1450°C for 40 hours to obtain a microporous corundum brick having a structure as shown in FIG. Figure 1 shown.
[0039] The preparation method of modified phenolic resin is:
[0040] S1. Add ethanol aqueous solution and modified silane to a reaction container, adjust the pH value to 5 with acetic acid, and stir for 6 hours to obtain a modified silane hydrolyzate; the volume ratio of ethanol to water in the ethanol aqueous solution is 8:1; the amount of modified silane added is 10% of the mass of the ethanol aqueous solution;
[0041] S2, adding modified silane hydrolyzate and nano silicon nitride to a reaction container, after uniform dispersion, heating to 70°C, reacting for 3 hours, centrifuging after the reaction is completed, washing the precipitate with acetone, and drying to obtain modified nano silicon nitride; the amount of nano silicon nitride added is 15% of the mass of the modified silane hydrolyzate;
[0042] S3. Add phenol, formaldehyde and sodium hydroxide to a reaction container, heat to 60°C, stir for 30 minutes to obtain a mixed solution, add modified nano silicon nitride, adjust the pH of the modified silane hydrolyzate to be the same as that of the mixed solution, and then slowly drop it into the mixed solution. After the drop is completed, heat to 95°C and react for 1.5 hours. After the reaction is completed, use acetic acid to adjust the pH to neutral, vacuum dehydrate, and obtain a modified phenolic resin; the molar ratio of phenol, formaldehyde, and sodium hydroxide is 1:1.2:0.03; the amount of modified nano silicon nitride added is 10% of the mass of the mixed solution; the amount of modified silane hydrolyzate added is 20% of the mass of the mixed solution.
[0043] Example 2
[0044] A microporous corundum brick comprises the following raw materials in percentage by weight: 28% brown corundum; 60% dense white corundum; 3% alumina micropowder; 8% silicon carbide; 1% metallic silicon micropowder; and 2% modified phenolic resin by weight of the total weight of the raw materials.
[0045] The Al2O3 in brown corundum is ≥95%; brown corundum is composed of particles with a particle size of 5-3mm and particles with a particle size of 3-1mm in a mass ratio of 1.5:1; the Al2O3 in dense white corundum is ≥95%; dense white corundum is composed of particles with a particle size of 3-1mm, particles with a particle size of 1-0mm, and fine powder with a particle size of 320 mesh in a mass ratio of 1.5:1:3; alumina micropowder is α-alumina micropowder with a particle size of 2um; the particle size of silicon carbide is 200 mesh; the particle size of metallic silicon micropowder is 0.035mm.
[0046] A preparation method of microporous corundum bricks comprises the following steps: mixing brown corundum and dense white corundum according to mass ratio for 2 minutes, adding modified phenolic resin, stirring for 5 minutes, adding alumina powder, silicon carbide and metallic silicon powder, and mixing and grinding for 10 minutes to obtain a mixture; pressing the mixture into a shape by a machine, drying it, and obtaining a brick; and sintering the brick at 1470°C for 35 hours to obtain a microporous corundum brick.
[0047] The preparation method of modified phenolic resin is:
[0048] S1. Add ethanol aqueous solution and modified silane to a reaction container, adjust the pH value to 4 with acetic acid, and stir for 5.5 hours to obtain a modified silane hydrolyzate; the volume ratio of ethanol to water in the ethanol aqueous solution is 9:1; the amount of modified silane added is 9% of the mass of the ethanol aqueous solution;
[0049] S2, adding modified silane hydrolyzate and nano silicon nitride to a reaction container, after uniform dispersion, heating to 65°C, reacting for 4 hours, centrifuging after the reaction is completed, washing the precipitate with acetone, and drying to obtain modified nano silicon nitride; the amount of nano silicon nitride added is 10% of the mass of the modified silane hydrolyzate;
[0050] S3. Add phenol, formaldehyde and sodium hydroxide to a reaction container, heat to 50°C, stir for 20 minutes to obtain a mixed solution, add modified nano silicon nitride, adjust the pH of the modified silane hydrolyzate to be the same as that of the mixed solution, and then slowly drop it into the mixed solution. After the drop is completed, heat to 90°C and react for 2 hours. After the reaction is completed, use acetic acid to adjust the pH to neutral, vacuum dehydrate, and obtain modified phenolic resin; the molar ratio of phenol, formaldehyde, and sodium hydroxide is 1:1.3:0.02; the amount of modified nano silicon nitride added is 8% of the mass of the mixed solution; the amount of modified silane hydrolyzate added is 15% of the mass of the mixed solution.
[0051] Example 3
[0052] A microporous corundum brick comprises the following raw materials in percentage by weight: 35% brown corundum; 52% dense white corundum; 4% alumina micropowder; 7% silicon carbide; 2% metallic silicon micropowder; and 2.5% of the total weight of the raw materials in terms of modified phenolic resin.
[0053] The Al2O3 in brown corundum is ≥95%; brown corundum is composed of particles with a particle size of 5-3mm and particles with a particle size of 3-1mm in a mass ratio of 1.8:1; the Al2O3 in dense white corundum is ≥95%; dense white corundum is composed of particles with a particle size of 3-1mm, particles with a particle size of 1-0mm, and fine powder with a particle size of 320 mesh in a mass ratio of 1.6:1:2.5; alumina micropowder is α-alumina micropowder with a particle size of 3um; the particle size of silicon carbide is 200 mesh; the particle size of metallic silicon micropowder is 0.025mm.
[0054] A preparation method of a microporous corundum brick comprises the following steps: mixing brown corundum and dense white corundum according to a mass ratio for 2.5 minutes, adding modified phenolic resin, stirring for 4 minutes, adding alumina micropowder, silicon carbide, and metallic silicon micropowder, and mixing and grinding for 13 minutes to obtain a mixed material; pressing the mixed material into a shape by a machine, drying it, and obtaining a brick blank; and sintering the brick blank at 1460° C. for 38 hours to obtain a microporous corundum brick.
[0055] The preparation method of modified phenolic resin is:
[0056] S1. Add ethanol aqueous solution and modified silane to a reaction container, adjust the pH value to 4.5 with acetic acid, and stir for 5 hours to obtain a modified silane hydrolyzate; the volume ratio of ethanol to water in the ethanol aqueous solution is 8.5:1; the amount of modified silane added is 8% of the mass of the ethanol aqueous solution;
[0057] S2, add modified silane hydrolyzate and nano silicon nitride into the reaction container, disperse them evenly, heat to 60°C, react for 3.5h, centrifuge after the reaction is completed, wash the precipitate with acetone, and dry to obtain modified nano silicon nitride; the amount of nano silicon nitride added is 12% of the mass of the modified silane hydrolyzate;
[0058] S3. Add phenol, formaldehyde and sodium hydroxide to a reaction container, heat to 55°C, stir for 25 minutes to obtain a mixed solution, add modified nano silicon nitride, adjust the pH of the modified silane hydrolyzate to be the same as that of the mixed solution, and then slowly drop it into the mixed solution. After the drop is completed, heat to 85°C and react for 1.8 hours. After the reaction is completed, use acetic acid to adjust the pH to neutral, vacuum dehydrate, and obtain modified phenolic resin; the molar ratio of phenol, formaldehyde, and sodium hydroxide is 1:1.25:0.025; the amount of modified nano silicon nitride added is 9% of the mass of the mixed solution; the amount of modified silane hydrolyzate added is 18% of the mass of the mixed solution.
[0059] Comparative Example 1
[0060] Compared with Example 1, the preparation method of the modified phenolic resin is different, and the rest is the same as Example 1.
[0061] The preparation method of modified phenolic resin is:
[0062] S1, the same as step S1 in Example 1;
[0063] S2. Add phenol, formaldehyde and sodium hydroxide to a reaction container, heat to 60°C, stir for 30 minutes to obtain a mixed solution, add nano-silicon nitride, adjust the pH of the modified silane hydrolyzate to be the same as that of the mixed solution, and then slowly add it dropwise to the mixed solution. After the dropwise addition, heat to 95°C and react for 1.5 hours. After the reaction is completed, use acetic acid to adjust the pH to neutral, vacuum dehydrate, and obtain a modified phenolic resin; the molar ratio of phenol, formaldehyde, and sodium hydroxide is 1:1.2:0.03; the amount of nano-silicon nitride added is 10% of the mass of the mixed solution; the amount of modified silane hydrolyzate added is 20% of the mass of the mixed solution.
[0064] Comparative Example 2
[0065] Compared with Example 1, the preparation method of the modified phenolic resin is different, and the rest is the same as Example 1.
[0066] The preparation method of modified phenolic resin is:
[0067] S1, the same as step S1 in Example 1;
[0068] S2, the same as step S2 in Example 1;
[0069] S3. Add phenol, formaldehyde and sodium hydroxide to a reaction container, heat to 60°C, stir for 30 minutes to obtain a mixed solution, add modified nano silicon nitride, heat to 95°C, react for 1.5 hours, and after the reaction is completed, use acetic acid to adjust the pH to neutral, vacuum dehydrate, and obtain modified phenolic resin; the molar ratio of phenol, formaldehyde and sodium hydroxide is 1:1.2:0.03; the amount of modified nano silicon nitride added is 10% of the mass of the mixed solution.
[0070] Comparative Example 3
[0071] Compared with Example 1, the preparation method of the modified phenolic resin is different, and the rest is the same as Example 1.
[0072] The preparation method of the modified phenolic resin is as follows: phenol, formaldehyde and sodium hydroxide are added into a reaction container, the temperature is raised to 60°C, stirred for 30 minutes to obtain a mixed solution, the temperature is raised to 95°C, and the reaction is carried out for 1.5 hours. After the reaction is completed, acetic acid is used to adjust the pH to neutral, vacuum dehydration is carried out, and the modified phenolic resin is obtained; the molar ratio of phenol, formaldehyde and sodium hydroxide is 1:1.2:0.03.
[0073] 1. Performance test of modified phenolic resin
[0074] The modified phenolic resins prepared in Examples 1-3 and Comparative Examples 1-3 were subjected to performance tests; the solid content and the residual carbon content were tested as follows: the mass of the crucible was weighed as A1, an appropriate amount of resin (accurate to 0.0001 g) was weighed as A, added to an open crucible, and treated at a constant temperature for 1.5 h in an electric furnace at 250° C., removed and air-cooled to near room temperature, placed in a dryer to room temperature, and weighed as A2; the covered crucible was treated in an electric furnace at 800° C. for 7 min, removed and air-cooled to near room temperature, placed in a dryer to room temperature, and weighed as A3; solid content %=(A2-A1)A×100%, residual carbon %=(A3-A1)A×100%; refer to GB / T 2567-2008 tested the tensile strength of the modified phenolic resin after curing; the mass loss of the modified phenolic resin after curing at 800°C was tested by TGA, the test conditions were: nitrogen atmosphere, air flow rate of 15 mL / min, from room temperature to 800°C, the heating rate was 10°C / min; the results are shown in Table 1.
[0075] Table 1 Performance test results of modified phenolic resin
[0076]
[0077] As shown in Table 1, the modified phenolic resins prepared in Examples 1-3 of the present invention have higher solid content, carbon residue, tensile strength and residual mass, indicating that the modified phenolic resins prepared in the present invention have high carbon residue, good mechanical properties and good heat resistance. Compared with Comparative Examples 1-3, in Example 1, modified silane and modified silicon nitride are used to modify the phenolic resin, and the structures of the modified silane and the modified silicon nitride both contain long-chain quaternary ammonium salts and rigid benzene ring groups with good dispersibility, so that the hydrolyzed modified silane can be uniformly dispersed in the system and react with free phenol, thereby contributing to increasing the solid content and tensile strength, and the dispersibility of the modified silicon nitride can be better, and the modified silicon nitride can be uniformly dispersed in the system to prevent the modified silicon nitride from agglomerating, thereby greatly improving the carbon residue, mechanical properties and heat resistance of the phenolic resin.
[0078] 2. Performance test of microporous corundum bricks
[0079] The performance tests of the microporous corundum bricks prepared in Examples 1-3 and Comparative Examples 1-3 were carried out; the sample preparation of the bricks was carried out in accordance with GB / T7321 standard, wherein the determination of Al2O3 and Fe2O3 contents was carried out in accordance with GB / T 6900-2006 standard, the apparent porosity and bulk density tests were carried out in accordance with GB / T 2997-2000 standard, the compressive strength test was carried out in accordance with GB / T 5072-2008 standard, the slag resistance (slag dissolution rate) test was carried out in accordance with YB / T 117 standard, the molten iron corrosion index test was carried out in accordance with YB / T 4036 standard, the air permeability test was carried out in accordance with GB / T3000 standard, the average pore size and pore volume ratio test of <1 μm was carried out in accordance with YB / T 118 standard, the alkali resistance (strength change rate) test was carried out in accordance with GB / T 14983 standard, thermal shock stability test (1100℃ water quenching method) refers to YB / T376.1-1995 standard, the test results are shown in Table 2.
[0080] Table 2 Performance test results of microporous corundum bricks
[0081]
[0082] From the results in Table 2, it can be seen that the microporous corundum bricks prepared in Examples 1-3 of the present invention have high Al2O3 content, low apparent porosity, high pore volume ratio of <1μm, and an average pore size of 0.23-0.26μm, which meets the requirements of micropores. The compressive strength, slag resistance, molten iron corrosion index, alkali resistance, and thermal shock stability are much greater than those of Comparative Examples 1-3, indicating that the microporous corundum bricks prepared in the present invention have good strength, slag resistance, molten iron corrosion resistance, alkali resistance, and thermal shock resistance. Compared with Comparative Examples 1-3, the modified phenolic resin used in Example 1 contains a good decomposition The long-chain quaternary ammonium salt group with dispersing effect is used as a binder for microporous corundum bricks, which is beneficial to the dispersion of various raw materials, has good bonding effect, and helps to form a solid brick structure. In addition, the modified phenolic resin has a high residual carbon content, good mechanical properties, good heat resistance, and produces less gaseous matter during high-temperature firing. The formed carbon layer can be further combined with other raw materials, increasing the density of the brick structure, thereby effectively improving the comprehensive performance of the microporous corundum brick. In addition, the modified silicon nitride and silicon carbide contained in the modified phenolic resin can also work together to improve the strength, corrosion resistance and thermal shock resistance of the microporous corundum brick.
[0083] It should be noted that, in this document, terms such as "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device that includes a series of elements includes not only those elements, but also includes other elements that are not explicitly listed, or also includes elements inherent to such process, method, article or device; although the embodiments of the present application have been shown and described, it can be understood by those of ordinary skill in the art that various changes, modifications, substitutions and variations may be made to these embodiments without departing from the principles and spirit of the present application, and the scope of the present application is defined by the appended claims and their equivalents.
Claims
1. A microporous corundum brick, characterized in that: The microporous corundum brick comprises the following raw materials in percentage by mass: 28-35% brown corundum; 52-60% dense white corundum; 3-5% alumina powder; 6-8% silicon carbide; 1-2% metallic silicon powder; the microporous corundum brick also comprises 2-3% of the total weight of the raw materials of modified phenolic resin; the preparation method of the modified phenolic resin is: S1. Add ethanol aqueous solution and modified silane to a reaction container, adjust the pH value to 4-5 with acetic acid, and stir for 5-6 hours to obtain a modified silane hydrolyzate; the chemical structural formula of the modified silane is: S2, adding modified silane hydrolyzate and nano silicon nitride into a reaction container, after uniform dispersion, heating to 60-70°C, reacting for 3-4 hours, after the reaction is completed, centrifuging, washing the precipitate with acetone, and drying to obtain modified nano silicon nitride; S3. Add phenol, formaldehyde and sodium hydroxide to a reaction container, heat to 50-60°C, stir for 20-30 minutes to obtain a mixed solution, add modified nano silicon nitride, adjust the pH of the modified silane hydrolyzate to be the same as that of the mixed solution, and then slowly drop it into the mixed solution. After the drop is completed, heat to 85-95°C and react for 1.5-2 hours. After the reaction is completed, use acetic acid to adjust the pH to neutral, vacuum dehydrate, and obtain modified phenolic resin.
2. The microporous corundum brick according to claim 1, characterized in that: The preparation method of the modified silane in step S1 is: (1) Add anhydrous dichloromethane and 3-aminopropyltriethoxysilane to a reaction vessel, stir evenly, and dropwise add an anhydrous dichloromethane solution containing 4-chloromethylbenzoyl chloride under nitrogen protection. After the dropwise addition, raise the temperature to 30-35° C. and react for 3-4 hours. After the reaction is completed, remove the dichloromethane by vacuum distillation to obtain chloro-silane, the chemical structure of which is: (2) adding anhydrous ethanol, chlorosilane and dodecyldimethylamine to a reaction vessel, and subjecting the mixture to reflux reaction for 10-12 hours. After the reaction is completed, removing the ethanol by vacuum distillation to obtain modified silane.
3. The microporous corundum brick according to claim 2, characterized in that: The molar ratio of 3-aminopropyltriethoxysilane to 4-chloromethylbenzoyl chloride in step (1) is 1:1-1.1; the molar ratio of chlorosilane to dodecyldimethyl tertiary amine in step (2) is 1:1-1.
1.
4. The microporous corundum brick according to claim 1, characterized in that: The volume ratio of ethanol to water in the ethanol aqueous solution in step S1 is 8-9:1; the added amount of the modified silane is 8-10% of the mass of the ethanol aqueous solution.
5. The microporous corundum brick according to claim 1, characterized in that: The amount of nano silicon nitride added in step S2 is 10-15% of the mass of the modified silane hydrolyzate.
6. The microporous corundum brick according to claim 1, characterized in that: In step S3, the molar ratio of phenol, formaldehyde and sodium hydroxide is 1:1.2-1.3:0.02-0.03; the amount of modified nano silicon nitride added is 8-10% of the mass of the mixed solution; and the amount of modified silane hydrolyzate added is 15-20% of the mass of the mixed solution.
7. The microporous corundum brick according to claim 1, characterized in that: The Al2O3 in the brown corundum is ≥95%; the brown corundum is composed of particles with a particle size of 5-3mm and particles with a particle size of 3-1mm in a mass ratio of 1.5-2:
1.
8. The microporous corundum brick according to claim 1, characterized in that: The Al2O3 in the dense white corundum is ≥95%; the dense white corundum is composed of particles with a particle size of 3-1mm, particles with a particle size of 1-0mm, and fine powder with a particle size of 320 mesh in a mass ratio of 1.5-2:1:2.5-3.
9. The microporous corundum brick according to claim 1, characterized in that: The alumina powder is α-alumina powder with a particle size of ≤5um; the particle size of the silicon carbide is 200 mesh; and the particle size of the metallic silicon powder is ≤0.045mm.
10. A method for preparing a microporous corundum brick according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: mixing brown corundum and dense white corundum according to the mass ratio for 2-3 minutes, adding modified phenolic resin, stirring for 3-5 minutes, adding alumina micropowder, silicon carbide and metallic silicon micropowder, and mixing and grinding for 10-15 minutes to obtain a mixture; pressing the mixture into a shape by a machine, drying it, and obtaining a brick; and sintering the brick at 1450-1470°C for 35-40 hours to obtain a microporous corundum brick.