Impact-resistant recycled plastic and preparation method thereof
By combining waste polyester with glycol and ultraviolet absorbing monomer polycondensation, and then combining with polythiophene coated graphene, impact-resistant recycled plastic is produced, which solves the problems of environmental pollution and high production costs of waste plastics. It has achieved improvements in impact resistance, anti-aging and flame retardant properties.
Patent Information
- Application Number
- CN202410713104.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-06-04
AI Technical Summary
The prior art is difficult to effectively solve the environmental pollution problems and high production costs of waste plastics, and the impact resistance and flame retardant properties of recycled plastics are insufficient.
Regenerated polyester is prepared by alcoholizing the waste polyester with ethylene glycol, and polycondensation reaction with ultraviolet absorbing monomer and dimethyl allylmalonic acid ester, and graphene is coated with polythiophene. Modified polythiophene coated graphene is formed, and the impact-resistant recycled plastic is finally produced by molding.
It achieves excellent impact resistance, anti-aging and flame retardant properties of impact recycled plastics, improves anti-static properties, and reduces production costs.
Smart Images

Figure SMS_1 
Figure SMS_3 
Figure SMS_4
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, in particular to impact-resistant recycled plastic and a preparation method thereof. Background Art
[0002] With the rapid development of modern science and technology and the continuous progress of human society, plastics have occupied an increasingly large proportion in people's daily lives. Concepts such as "plastics instead of steel" and "plastics instead of wood" have made plastics more and more popular. Plastics are not only increasingly connected with people's lives, but also become an indispensable and important material in people's industry, agriculture, medical industry, and construction industry. Recycling and regenerating waste plastics can not only reduce production costs, but also solve the environmental pollution problem caused by waste plastics. It has very important practical significance and broad market prospects. Summary of the invention
[0003] The purpose of the present invention is to provide an impact-resistant recycled plastic and a preparation method thereof, so as to solve the problems existing in the prior art.
[0004] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0005] The invention discloses an impact-resistant recycled plastic. The impact-resistant recycled plastic is prepared by alcoholyzing waste polyester with ethylene glycol to obtain polyester oligomer; polycondensing the polyester oligomer, ultraviolet absorption monomer and dimethyl allyl malonate to obtain recycled polyester; reacting polythiophene-coated graphene with phenylphosphorous acid to obtain modified polythiophene-coated graphene; and uniformly mixing the recycled polyester and the modified polythiophene-coated graphene and then performing compression molding to obtain the impact-resistant recycled plastic.
[0006] As an optimization, the waste polyester is one or more of waste polyester plastic bottles, waste polyester plastic sheets, waste polyester fibers, and waste polyester fabrics.
[0007] As an optimization, the ultraviolet absorbing monomer is prepared by reacting 2,5-dimercaptoterephthalic acid with ethylene glycol and 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol in sequence.
[0008] As an optimization, the polythiophene-coated graphene is prepared by polymerizing and depositing thiophene and 3-thiophenesulfonamide on the graphene surface.
[0009] A method for preparing impact-resistant recycled plastics comprises the following preparation steps:
[0010] (1) crushing waste polyester into polyester crumbs with a particle size of 2 to 3 mm, mixing the polyester crumbs, zinc acetate, and ethylene glycol in a mass ratio of 1:(0.03 to 0.05):(3 to 4), stirring and reacting at 180 to 190° C. and 300 to 500 r / min for 2 to 3 hours under a nitrogen atmosphere, cooling to 150 to 160° C., filtering, and drying at 3 to 5 Pa and 50 to 60° C. for 6 to 8 hours to obtain a polyester oligomer;
[0011] (2) 2,5-dimercaptoterephthalic acid and ethylene glycol are uniformly mixed in a molar ratio of 1:2, stirred at 70-80°C for 20-30 minutes, placed in a reaction kettle, stirred and reacted at 230-240°C for 2-3 hours to obtain bis(2-hydroxyethyl) 2,5-dimercaptoterephthalate; bis(2-hydroxyethyl) 2,5-dimercaptoterephthalate, 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)benzene Phenol is added to toluene with a molar ratio of 1:2, and then azobisisobutyronitrile with a mass of 8 to 10 times that of bis(2-hydroxyethyl)2,5-dimercaptoterephthalate is added, and the mixture is stirred at 70 to 80°C and 300 to 500 r / min for 3 to 4 hours under a nitrogen atmosphere, and then dried at 3 to 5 Pa and 50 to 60°C for 7 to 8 hours to obtain an ultraviolet absorbing monomer.
[0012] (3) Mix polyester oligomer, ultraviolet absorption monomer, dimethyl allyl malonate, antimony trioxide, heat stabilizer and matting agent in a mass ratio of 1: (0.2-0.3): (0.2-0.3): (0.02-0.04): (0.05-0.07): (0.05-0.07), place in a polycondensation reaction kettle, stir and react at 270-280° C. and 300-500 r / min for 1-2 h, reduce the pressure to 50-100 Pa, continue stirring and reacting for 1-2 h, cool to room temperature, wash with deionized water for 3-5 times, and dry at 3-5 Pa and 50-60° C. for 7-8 h to obtain recycled polyester;
[0013] (4) Under the stirring conditions of 0-2°C and 300-500 r / min, a thiophene solution of 1-1.2 times the mass of the mixed solution is uniformly added dropwise to the mixed solution within 30 minutes, the stirring reaction is continued for 20-24 hours, the mixture is allowed to stand at 10-30°C for 3-5 hours, filtered, washed with deionized water for 3-5 times, and dried at 3-5 Pa and 60-70°C for 8-10 hours to obtain polythiophene-coated graphene; the polythiophene-coated graphene is Graphene, phenylphosphorous acid, dicyclohexylcarbodiimide and toluene are mixed uniformly in a mass ratio of 1: (1.2-1.4): (0.03-0.05): (10-12), stirred at 60-70°C and 300-500r / min for 3-4h, filtered, washed with anhydrous ethanol and deionized water for 3-5 times respectively, dried at 3-5Pa and 60-70°C for 7-8h to obtain modified polythiophene-coated graphene;
[0014] (5) The recycled polyester, modified polythiophene-coated graphene, and azobisisobutyronitrile are mixed uniformly in a mass ratio of 1: (0.06-0.08): (0.002-0.004), placed in an internal mixer, stirred at 240-250° C. for 10-12 min, placed in a mold for compression molding, and naturally cooled to room temperature before demolding to obtain an impact-resistant recycled plastic.
[0015] As an optimization, the reaction process of the ultraviolet absorbing monomer in step (2) is:
[0016]
[0017] Where R is H or:
[0018] As an optimization, the heat stabilizer in step (3) is trimethyl phosphate and the matting agent is titanium dioxide.
[0019] As an optimization, the preparation method of the mixed solution in step (4) is: under a nitrogen atmosphere, graphene, anhydrous ferric chloride, and tetrahydrofuran are uniformly mixed in a mass ratio of 1: (0.1-0.3): (10-12), and ultrasonically treated for 1-2 hours to prepare a mixed solution.
[0020] As an optimization, the preparation method of the thiophene solution in step (4) is: thiophene, 3-thiophenesulfonamide, and tetrahydrofuran are uniformly mixed in a mass ratio of 1: (0.1-0.2): (6-8) to prepare a thiophene solution.
[0021] As an optimization, the process parameters of the compression molding in step (5) are: at 240-250° C., 2-3 MPa, maintaining pressure for 3-5 min, keeping the pressure constant, cooling to 90-100° C. and maintaining heat for 2-3 h.
[0022] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0023] When preparing the impact-resistant recycled plastic, the invention comprises the following steps: using ethylene glycol to alcoholize waste polyester to obtain polyester oligomers; reacting 2,5-dimercaptoterephthalic acid with ethylene glycol and 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propylene)phenol in sequence to obtain ultraviolet absorption monomers; polycondensing the polyester oligomers, the ultraviolet absorption monomers and dimethyl allylmalonate to obtain recycled polyester; polymerizing and depositing thiophene and 3-thiophene sulfonamide on the surface of graphene to obtain polythiophene-coated graphene; reacting the polythiophene-coated graphene with phenylphosphorous acid to obtain modified polythiophene-coated graphene; and uniformly mixing the recycled polyester and the modified polythiophene-coated graphene and then performing compression molding to obtain the impact-resistant recycled plastic.
[0024] Firstly, waste polyester is hydrolyzed with ethylene glycol to obtain polyester oligomers, 2,5-dimercaptoterephthalic acid is reacted with ethylene glycol and 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol in sequence to obtain ultraviolet absorbing monomers; 2,5-dimercaptoterephthalic acid is esterified with ethylene glycol in sequence to generate bis(2-hydroxyethyl)2,5-dimercaptoterephthalate, the thiol group on the bis(2-hydroxyethyl)2,5-dimercaptoterephthalate is reacted with the thiol group on the 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol The carbon-carbon double bond undergoes an addition reaction, and a benzotriazole ultraviolet absorbing group is introduced into the ultraviolet absorbing monomer. The benzotriazole ultraviolet absorbing group initially exists in the form of an ester compound. After absorbing ultraviolet rays, the electron cloud density is transferred from the oxygen atom to the nitrogen atom of the triazole ring, making the nitrogen atom alkaline and the proton transferred to the nitrogen atom, thereby forming an unstable tautomer. Since the tautomer is in an unstable state, it will release the absorbed energy in the form of heat energy or other lower energy, and return to the stable ground state, giving the impact-resistant recycled plastic excellent anti-aging properties.
[0025] Secondly, polyester oligomers, ultraviolet absorbing monomers, and allyl dimethyl malonate are subjected to condensation reaction to obtain recycled polyester, and carbon-carbon double bonds are introduced into the side chains of the recycled polyester molecules. The carbon-carbon double bonds introduced into the side chains of the polyester molecules can undergo addition reaction with the PH bonds on the modified polythiophene-coated graphene to form a cross-linked network, thereby inhibiting the relative slip between the polyester molecular chains and giving the impact-resistant recycled plastics excellent impact resistance.
[0026] Finally, thiophene and 3-thiophenesulfonamide are polymerized and deposited on the surface of graphene to obtain polythiophene-coated graphene, and amino groups are introduced into the polythiophene-coated graphene; the polythiophene-coated graphene is reacted with phenylphosphite to obtain modified polythiophene-coated graphene, and the amino groups on the polythiophene-coated graphene react with the phosphate groups on the phenylphosphite to generate phosphoramide, and phosphorus element and PH bond are introduced into the modified polythiophene-coated graphene. The introduction of phosphorus element can give the impact-resistant recycled plastic excellent flame retardant properties, and the PH bond introduced into the modified polythiophene-coated graphene can It reacts with the carbon-carbon double bonds introduced on the side chains of recycled polyester molecules to form a cross-linked network, which inhibits the relative slip between polyester molecular chains and gives the impact-resistant recycled plastic excellent impact resistance. Graphene is a two-dimensional layered carbon material with a conjugated system that makes it have strong electron conduction ability and excellent conductivity, which can give the impact-resistant recycled plastic excellent antistatic properties. Polythiophene is a conductive polymer material that can form a conductive path inside the impact-resistant recycled plastic, further improving the antistatic properties of the impact-resistant recycled plastic. DETAILED DESCRIPTION
[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0028] Example 1
[0029] A method for preparing impact-resistant recycled plastics, the method comprising the following preparation steps:
[0030] (1) Waste polyester was crushed into polyester crumbs with a particle size of 2 mm, the polyester crumbs, zinc acetate, and ethylene glycol were mixed uniformly at a mass ratio of 1:0.03:3, stirred at 180°C and 300 r / min for 3 h under a nitrogen atmosphere, cooled to 150°C, filtered, and dried at 3 Pa and 50°C for 8 h to obtain polyester oligomers;
[0031] (2) 2,5-dimercaptoterephthalic acid and ethylene glycol were mixed uniformly in a molar ratio of 1:2, stirred at 70°C for 30 minutes, placed in a reactor, and stirred and reacted at 230°C for 3 hours to obtain bis(2-hydroxyethyl) 2,5-dimercaptoterephthalate; bis(2-hydroxyethyl) 2,5-dimercaptoterephthalate and 2-(2H-benzotriazol-2-yl)-4-methyl-6-(2-propenyl)phenol were added in a molar ratio of 1:2 to toluene with a mass of 8 times that of bis(2-hydroxyethyl) 2,5-dimercaptoterephthalate, and then azobisisobutyronitrile with a mass of 0.03 times that of bis(2-hydroxyethyl) 2,5-dimercaptoterephthalate was added, and the mixture was stirred and reacted at 70°C and 300 r / min for 4 hours under a nitrogen atmosphere, and dried at 3Pa and 50°C for 8 hours to obtain a UV absorbing monomer;
[0032] (3) The polyester oligomer, the ultraviolet absorption monomer, the dimethyl allyl malonate, the antimony trioxide, the trimethyl phosphate, and the titanium dioxide were mixed uniformly in a mass ratio of 1:0.2:0.2:0.02:0.05:0.05, placed in a polycondensation reactor, stirred and reacted at 270°C and 300 r / min for 2 h, the pressure was reduced to 50 Pa, the stirring reaction was continued for 2 h, cooled to room temperature, washed with deionized water for 3 times, and dried at 3 Pa and 50°C for 8 h to obtain a recycled polyester;
[0033] (4) Under a nitrogen atmosphere, graphene, anhydrous ferric chloride, and tetrahydrofuran were mixed at a mass ratio of 1:0.1:10, and ultrasonically treated for 1 hour to prepare a mixed solution. Thiophene, 3-thiophenesulfonamide, and tetrahydrofuran were mixed at a mass ratio of 1:0.1:6 to prepare a thiophene solution. Under stirring conditions of 0°C and 300 r / min, a thiophene solution with a mass that is 1 times the mass of the mixed solution was uniformly added dropwise to the mixed solution within 30 minutes. The stirring reaction was continued for 24 hours. The mixture was allowed to stand at 10°C for 5 h, filtered, washed with deionized water for 3 times, and dried at 3Pa and 60°C for 10 h to obtain polythiophene-coated graphene; polythiophene-coated graphene, phenylphosphorous acid, dicyclohexylcarbodiimide, and toluene were uniformly mixed in a mass ratio of 1:1.2:0.03:10, stirred at 60°C and 300 r / min for 4 h, filtered, washed with anhydrous ethanol and deionized water for 3 times each, and dried at 3Pa and 60°C for 8 h to obtain modified polythiophene-coated graphene;
[0034] (5) The recycled polyester, modified polythiophene-coated graphene, and azobisisobutyronitrile were mixed evenly in a mass ratio of 1:0.06:0.002, placed in an internal mixer, stirred at 240°C for 12 min, placed in a mold, maintained at 240°C and 2 MPa for 5 min, kept the pressure constant, cooled to 90°C and kept warm for 3 h, naturally cooled to room temperature, and then demolded to obtain an impact-resistant recycled plastic.
[0035] Example 2
[0036] A method for preparing impact-resistant recycled plastics, the method comprising the following preparation steps:
[0037] (1) Waste polyester was crushed into polyester crumbs with a particle size of 2.5 mm, the polyester crumbs, zinc acetate, and ethylene glycol were mixed evenly in a mass ratio of 1:0.04:3.5, stirred and reacted at 185°C and 400 r / min for 2.5 h in a nitrogen atmosphere, cooled to 155°C, filtered, and dried at 4 Pa and 55°C for 7 h to obtain polyester oligomers;
[0038] (2) 2,5-dimercaptoterephthalic acid and ethylene glycol were mixed in a molar ratio of 1:2, stirred at 75°C for 25 minutes, placed in a reactor, and stirred at 235°C for 2.5 hours to obtain bis(2-hydroxyethyl) 2,5-dimercaptoterephthalate; bis(2-hydroxyethyl) 2,5-dimercaptoterephthalate and 2-(2H-benzotriazol-2-yl)-4-methyl-6-(2-propenyl)phenol were added in a molar ratio of 1:2 to toluene with a mass of 9 times that of bis(2-hydroxyethyl) 2,5-dimercaptoterephthalate, and then azobisisobutyronitrile with a mass of 0.04 times that of bis(2-hydroxyethyl) 2,5-dimercaptoterephthalate was added, and the mixture was stirred at 75°C and 400 r / min for 3.5 hours under a nitrogen atmosphere, and dried at 4Pa and 55°C for 7.5 hours to obtain a UV absorbing monomer;
[0039] (3) The polyester oligomer, ultraviolet absorption monomer, dimethyl allyl malonate, antimony trioxide, trimethyl phosphate, and titanium dioxide were mixed uniformly in a mass ratio of 1:0.25:0.25:0.03:0.06:0.06, placed in a polycondensation reactor, stirred and reacted at 275°C and 400 r / min for 1.5 hours, the pressure was reduced to 75 Pa, the stirring reaction was continued for 1.5 hours, cooled to room temperature, washed with deionized water for 4 times, and dried at 4 Pa and 55°C for 7.5 hours to obtain recycled polyester;
[0040] (4) Under nitrogen atmosphere, graphene, anhydrous ferric chloride, and tetrahydrofuran were mixed in a mass ratio of 1:0.2:11, and ultrasonically treated for 1.5 h to prepare a mixed solution. Thiophene, 3-thiophenesulfonamide, and tetrahydrofuran were mixed in a mass ratio of 1:0.15:7 to prepare a thiophene solution. Under stirring conditions of 1°C and 400 r / min, 1.1 times the mass of the mixed solution of thiophene solution was uniformly added dropwise to the mixed solution within 30 min, and the stirring reaction was continued for 22 h. The mixture was allowed to stand at 20°C for 4 hours, filtered, washed with deionized water for 4 times, and dried at 4Pa and 65°C for 9 hours to obtain polythiophene-coated graphene; polythiophene-coated graphene, phenylphosphorous acid, dicyclohexylcarbodiimide, and toluene were uniformly mixed in a mass ratio of 1:1.3:0.04:11, stirred at 65°C and 400r / min for 3.5 hours, filtered, washed with anhydrous ethanol and deionized water for 4 times respectively, and dried at 4Pa and 65°C for 7.5 hours to obtain modified polythiophene-coated graphene;
[0041] (5) The recycled polyester, modified polythiophene-coated graphene, and azobisisobutyronitrile were mixed evenly in a mass ratio of 1:0.07:0.003, placed in an internal mixer, stirred at 245°C for 11 minutes, placed in a mold, maintained at 245°C and 2.5 MPa for 4 minutes, kept the pressure constant, cooled to 95°C and kept warm for 2.5 hours, naturally cooled to room temperature, and then demolded to obtain an impact-resistant recycled plastic.
[0042] Example 3
[0043] A method for preparing impact-resistant recycled plastics, the method comprising the following preparation steps:
[0044] (1) Waste polyester was crushed into polyester crumbs with a particle size of 3 mm, the polyester crumbs, zinc acetate, and ethylene glycol were mixed uniformly in a mass ratio of 1:0.05:4, stirred and reacted at 190°C and 500 r / min for 2 h in a nitrogen atmosphere, cooled to 160°C, filtered, and dried at 5 Pa and 60°C for 6 h to obtain polyester oligomers;
[0045] (2) 2,5-dimercaptoterephthalic acid and ethylene glycol were mixed in a molar ratio of 1:2, stirred at 80°C for 20 minutes, placed in a reactor, and stirred at 240°C for 2 hours to obtain bis(2-hydroxyethyl) 2,5-dimercaptoterephthalate; bis(2-hydroxyethyl) 2,5-dimercaptoterephthalate and 2-(2H-benzotriazol-2-yl)-4-methyl-6-(2-propenyl)phenol were added in a molar ratio of 1:2 to toluene with a mass of 10 times that of bis(2-hydroxyethyl) 2,5-dimercaptoterephthalate, and then azobisisobutyronitrile with a mass of 0.05 times that of bis(2-hydroxyethyl) 2,5-dimercaptoterephthalate was added, and the mixture was stirred at 80°C and 500 r / min for 3 hours under a nitrogen atmosphere, and dried at 5 Pa and 60°C for 7 hours to obtain a UV absorbing monomer;
[0046] (3) The polyester oligomer, the ultraviolet absorption monomer, the dimethyl allyl malonate, the antimony trioxide, the trimethyl phosphate, and the titanium dioxide were mixed uniformly in a mass ratio of 1:0.3:0.3:0.04:0.07:0.07, placed in a polycondensation reactor, stirred and reacted at 280°C and 500 r / min for 1 hour, the pressure was reduced to 100 Pa, the stirring reaction was continued for 1 hour, cooled to room temperature, washed with deionized water for 5 times, and dried at 5 Pa and 60°C for 7 hours to obtain a recycled polyester;
[0047] (4) Under a nitrogen atmosphere, graphene, anhydrous ferric chloride, and tetrahydrofuran were mixed at a mass ratio of 1:0.3:12, and ultrasonically treated for 2 h to prepare a mixed solution. Thiophene, 3-thiophenesulfonamide, and tetrahydrofuran were mixed at a mass ratio of 1:0.2:8 to prepare a thiophene solution. Under the stirring conditions of 2°C and 500 r / min, a thiophene solution with a mass 1.2 times that of the mixed solution was uniformly added dropwise to the mixed solution within 30 min, and the stirring reaction was continued for 20 h. , standing at 30°C for 3h, filtered, washed with deionized water 5 times, dried at 5Pa, 70°C for 8h, to obtain polythiophene-coated graphene; polythiophene-coated graphene, phenylphosphorous acid, dicyclohexylcarbodiimide, and toluene were mixed evenly in a mass ratio of 1:1.4:0.05:12, stirred at 70°C, 500r / min for 3h, filtered, washed with anhydrous ethanol and deionized water 5 times each, and dried at 5Pa, 70°C for 7h to obtain modified polythiophene-coated graphene;
[0048] (5) The recycled polyester, modified polythiophene-coated graphene, and azobisisobutyronitrile were mixed evenly in a mass ratio of 1:0.08:0.004, placed in an internal mixer, stirred at 250°C for 10 min, placed in a mold, and maintained at 250°C and 3 MPa for 3 min. The pressure was kept constant, cooled to 100°C and kept warm for 2 h, and then naturally cooled to room temperature and demolded to obtain an impact-resistant recycled plastic.
[0049] Comparative Example 1
[0050] The difference between the preparation method of the impact-resistant recycled plastic of Comparative Example 1 and Example 2 is that step (2) is not performed, and step (3) is modified as follows: polyester oligomer, dimethyl allyl malonate, antimony trioxide, trimethyl phosphate, and titanium dioxide are uniformly mixed in a mass ratio of 1:0.25:0.03:0.06:0.06, placed in a polycondensation reactor, stirred and reacted at 275°C and 400r / min for 1.5h, the pressure is reduced to 75Pa, the stirring reaction is continued for 1.5h, cooled to room temperature, washed with deionized water 4 times, and dried at 4Pa and 55°C for 7.5h to obtain recycled polyester. The remaining steps are the same as those of Example 2.
[0051] Comparative Example 2
[0052] The difference between the preparation method of the impact-resistant recycled plastic of Comparative Example 2 and Example 2 lies in the difference in step (3), which is modified as follows: polyester oligomer, ultraviolet absorption monomer, antimony trioxide, trimethyl phosphate, and titanium dioxide are uniformly mixed in a mass ratio of 1:0.25:0.03:0.06:0.06, placed in a polycondensation reactor, stirred and reacted at 275°C and 400r / min for 1.5h, the pressure is reduced to 75Pa, the stirring reaction is continued for 1.5h, cooled to room temperature, washed with deionized water 4 times, and dried at 4Pa and 55°C for 7.5h to obtain recycled polyester. The remaining steps are the same as those of Example 2.
[0053] Comparative Example 3
[0054] The preparation method of the impact-resistant recycled plastic of Comparative Example 3 is different from that of Example 2 in that step (4) is not performed, and step (5) is modified as follows: the recycled polyester is placed in an internal mixer, stirred at 245° C. for 11 min, placed in a mold, maintained at 245° C. and 2.5 MPa for 4 min, the pressure is kept constant, the temperature is reduced to 95° C. and maintained for 2.5 h, and the impact-resistant recycled plastic is removed from the mold after naturally cooling to room temperature. The remaining steps are the same as those of Example 2.
[0055] Comparative Example 4
[0056] The preparation method of the impact-resistant recycled plastic of Comparative Example 4 is different from that of Example 2 only in step (4), and step (4) is modified as follows: in a nitrogen atmosphere, graphene, anhydrous ferric chloride, and tetrahydrofuran are mixed uniformly in a mass ratio of 1:0.2:11, and ultrasonically treated for 1.5 hours to prepare a mixed solution; thiophene, 3-thiophenesulfonamide, and tetrahydrofuran are mixed uniformly in a mass ratio of 1:0.15:7 to prepare a thiophene solution; under the stirring conditions of 1°C and 400 r / min, a thiophene solution with a mass of 1.1 times the mass of the mixed solution is uniformly added dropwise to the mixed solution within 30 minutes, and the stirring reaction is continued for 22 hours, and the mixture is allowed to stand at 20°C for 4 hours, filtered, washed with deionized water 4 times, and dried at 4Pa and 65°C for 9 hours to obtain modified polythiophene-coated graphene. The remaining steps are the same as those of Example 2.
[0057] Comparative Example 5
[0058] The preparation method of the impact-resistant recycled plastic of Comparative Example 5 is different from that of Example 2 in that step (4) is not performed, and step (5) is modified as follows: the recycled polyester and graphene are uniformly mixed in a mass ratio of 1:0.07, placed in an internal mixer, stirred at 245°C for 11 minutes, placed in a mold, maintained at 245°C, 2.5 MPa for 4 minutes, the pressure is kept constant, the temperature is reduced to 95°C and kept warm for 2.5 hours, and the mold is demolded and taken out after natural cooling to room temperature to obtain the impact-resistant recycled plastic.
[0059] Test Example 1
[0060] Impact resistance and anti-aging performance testing
[0061] Test method: According to GB / T1843, the impact strength of the embodiment and the comparative example was tested on an impact tester, and then the original sample without impact test was irradiated with a xenon arc lamp for 72 hours. According to GB / T1843, the impact strength of the embodiment and the comparative example after UV aging treatment was tested on an impact tester, and the impact strength change rate of the embodiment and the comparative example before and after UV aging treatment was calculated, and the impact strength change rate = (original impact strength of the sample - impact strength after UV aging treatment) / original impact strength of the sample × 100%. The results are shown in Table 1.
[0062] Table 1
[0063]
[0064]
[0065] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 5 in Table 1, it can be found that the impact-resistant recycled plastic prepared by the present invention has good impact resistance and anti-aging properties.
[0066] By comparison, the impact strength of Examples 1 to 3 is greater than that of Comparative Example 2, indicating that the recycled polyester is prepared by the condensation reaction of polyester oligomers, ultraviolet absorbing monomers, and allyl dimethyl malonate, and carbon-carbon double bonds are introduced into the side chains of the recycled polyester molecules. The carbon-carbon double bonds introduced into the side chains of the polyester molecules can undergo addition reaction with the PH bonds on the modified polythiophene-coated graphene to form a cross-linked network, thereby inhibiting the relative slip between the polyester molecular chains and giving the impact-resistant recycled plastics excellent impact resistance.
[0067] By comparison, the impact strength of Examples 1 to 3 is greater than that of Comparative Examples 3 to 5, indicating that thiophene and 3-thiophenesulfonamide are polymerized and deposited on the surface of graphene to obtain polythiophene-coated graphene, and amino groups are introduced into the polythiophene-coated graphene; the polythiophene-coated graphene is reacted with phenylphosphite to obtain modified polythiophene-coated graphene, the amino groups on the polythiophene-coated graphene react with the phosphate groups on the phenylphosphite to generate phosphoramide, and PH bonds are introduced into the modified polythiophene-coated graphene. The PH bonds introduced into the modified polythiophene-coated graphene can undergo addition reaction with the carbon-carbon double bonds introduced into the side chains of the recycled polyester molecules to form a cross-linked network, thereby inhibiting the relative slip between the polyester molecular chains and giving the impact-resistant recycled plastics excellent impact resistance.
[0068] By comparison, the impact strength change rate of Examples 1 to 3 is less than that of Comparative Example 1, indicating that 2,5-dimercaptoterephthalic acid is sequentially reacted with ethylene glycol and 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol to prepare an ultraviolet absorbing monomer; 2,5-dimercaptoterephthalic acid is sequentially esterified with ethylene glycol to produce bis(2-hydroxyethyl) 2,5-dimercaptoterephthalate; the thiol group on the bis(2-hydroxyethyl) 2,5-dimercaptoterephthalate is reacted with 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2 -propylene)phenol undergoes an addition reaction on the carbon-carbon double bond, and introduces a benzotriazole ultraviolet absorbing group into the ultraviolet absorbing monomer. The benzotriazole ultraviolet absorbing group initially exists in the form of an ester compound. After absorbing ultraviolet rays, the electron cloud density is transferred from the oxygen atom to the nitrogen atom of the triazole ring, making the nitrogen atom alkaline and the proton transferred to the nitrogen atom, thereby forming an unstable tautomer. Since the tautomer is in an unstable state, it will release the absorbed energy in the form of heat or other lower energy, and return to the stable ground state, giving the impact-resistant recycled plastic excellent anti-aging properties.
[0069] Test Example 2
[0070] Flame retardant performance test
[0071] Test method: The examples and comparative examples were prepared into standard specimens according to GB / T2406.2, and the limiting oxygen index of the standard specimens was tested. The results are shown in Table 2
[0072] Table 2
[0073] Limiting oxygen index (%) Limiting oxygen index (%) Example 1 29.56 Comparative Example 1 28.86 Example 2 30.17 Comparative Example 2 29.44 Example 3 29.14 Comparative Example 3 21.37 Comparative Example 4 20.49 Comparative Example 5 21.18
[0074] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 5 in Table 2, it can be found that the impact-resistant recycled plastic prepared by the present invention has good flame retardant properties.
[0075] By comparison, the limiting oxygen index of Examples 1 to 3 is greater than that of Comparative Examples 3 to 5, indicating that thiophene and 3-thiophenesulfonamide are polymerized and deposited on the surface of graphene to obtain polythiophene-coated graphene, and amino groups are introduced into the polythiophene-coated graphene; the polythiophene-coated graphene is reacted with phenylphosphite to obtain modified polythiophene-coated graphene, the amino groups on the polythiophene-coated graphene react with the phosphate groups on the phenylphosphite to generate phosphoramide, and phosphorus element is introduced into the modified polythiophene-coated graphene, and the introduction of phosphorus element can give the impact-resistant recycled plastic excellent flame retardant properties.
[0076] Test Example 3
[0077] Antistatic performance test
[0078] Test method: According to GB / T 12703, the half-life method is used to discharge the sample placed on the rotating metal platform with a 10KV high voltage for 30 seconds. When the static voltage is stable, the time and half-life when the induced voltage decays to half are detected. The antistatic effects of the embodiments and comparative examples are evaluated based on the half-life. The results are shown in Table 3.
[0079] Table 3
[0080] Half-life(s) Half-life(s) Example 1 7.17 Comparative Example 1 7.47 Example 2 7.29 Comparative Example 2 7.82 Example 3 7.25 Comparative Example 3 15.37 Comparative Example 4 7.53 Comparative Example 5 11.32
[0081] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 5 in Table 3, it can be found that the impact-resistant recycled plastic prepared by the present invention has good antistatic performance.
[0082] By comparison, the half-lives of Examples 1 to 3 are shorter than those of Comparative Examples 3 and 5, and the half-life of Comparative Example 5 is shorter than that of Comparative Example 3, indicating that thiophene and 3-thiophenesulfonamide are polymerized and deposited on the graphene surface to obtain polythiophene-coated graphene. Graphene is a two-dimensional layered carbon material with a conjugated system that makes its electron conduction ability very strong and has excellent conductivity, which can give the impact-resistant recycled plastic excellent antistatic properties; polythiophene is a conductive polymer material that can form a conductive path inside the impact-resistant recycled plastic, further improving the antistatic properties of the impact-resistant recycled plastic.
[0083] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. An impact-resistant recycled plastic, characterized in that: The impact-resistant recycled plastic is prepared by alcoholyzing waste polyester with ethylene glycol to obtain polyester oligomers; polycondensing polyester oligomers, ultraviolet absorption monomers and dimethyl allyl malonate to obtain recycled polyester; reacting polythiophene-coated graphene with phenylphosphite to obtain modified polythiophene-coated graphene; and uniformly mixing recycled polyester and modified polythiophene-coated graphene and then performing compression molding to obtain impact-resistant recycled plastic. The ultraviolet absorption monomer is prepared by sequentially reacting 2,5-dimercaptoterephthalic acid with ethylene glycol and 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)phenol; The polythiophene-coated graphene is prepared by polymerizing thiophene and 3-thiophenesulfonamide and depositing them on the surface of graphene.
2. The impact-resistant recycled plastic according to claim 1, characterized in that: The waste polyester is one or more of waste polyester plastic bottles, waste polyester plastic sheets, waste polyester fibers, and waste polyester fabrics.
3. A method for preparing impact-resistant recycled plastics, characterized in that: The method comprises the following preparation steps: (1) The waste polyester is crushed into polyester crumbs with a particle size of 2-3 mm, and the polyester crumbs, zinc acetate, and ethylene glycol are mixed uniformly in a mass ratio of 1:(0.03-0.05):(3-4), and stirred at 180-190°C and 300-500 r / min for 2-3 h under a nitrogen atmosphere, cooled to 150-160°C, filtered, and dried at 3-5 Pa and 50-60°C for 6-8 h to obtain a polyester oligomer; (2) 2,5-dimercaptoterephthalic acid and ethylene glycol were mixed uniformly in a molar ratio of 1:2, stirred at 70-80°C for 20-30 min, placed in a reactor, stirred and reacted at 230-240°C for 2-3 h to obtain bis(2-hydroxyethyl) 2,5-dimercaptoterephthalate; bis(2-hydroxyethyl) 2,5-dimercaptoterephthalate, 2-(2H-benzotriazole-2-yl)-4-methyl-6-(2-propenyl)benzene Phenol is added to toluene with a molar ratio of 1:2, which is 8 to 10 times the mass of bis(2-hydroxyethyl) 2,5-dimercaptoterephthalate, and then azobisisobutyronitrile with a mass of 0.03 to 0.05 times the mass of bis(2-hydroxyethyl) 2,5-dimercaptoterephthalate is added, and the mixture is stirred at 70 to 80°C and 300 to 500 r / min for 3 to 4 hours under a nitrogen atmosphere, and then dried at 3 to 5 Pa and 50 to 60°C for 7 to 8 hours to obtain an ultraviolet absorbing monomer; (3) Mix polyester oligomer, ultraviolet absorption monomer, dimethyl allyl malonate, antimony trioxide, heat stabilizer and matting agent in a mass ratio of 1:(0.2~0.3):(0.2~0.3):(0.02~0.04):(0.05~0.07):(0.05~0.07), place in a polycondensation reactor, stir and react at 270~280℃, 300~500r / min for 1~2h, reduce the pressure to 50~100Pa, continue stirring and reacting for 1~2h, cool to room temperature, wash with deionized water 3~5 times, dry at 3~5Pa, 50~60℃ for 7~8h, to obtain recycled polyester; (4) Under the stirring conditions of 0-2°C and 300-500 r / min, a thiophene solution of 1-1.2 times the mass of the mixed solution is uniformly added dropwise to the mixed solution within 30 min, and the stirring reaction is continued for 20-24 h. The mixture is allowed to stand at 10-30°C for 3-5 h, filtered, washed with deionized water for 3-5 times, and dried at 3-5 Pa and 60-70°C for 8-10 h to obtain polythiophene-coated graphene. Graphene, phenylphosphorous acid, dicyclohexylcarbodiimide and toluene are mixed uniformly in a mass ratio of 1:(1.2-1.4):(0.03-0.05):(10-12), stirred at 60-70°C and 300-500r / min for 3-4h, filtered, washed with anhydrous ethanol and deionized water for 3-5 times respectively, dried at 3-5Pa and 60-70°C for 7-8h to obtain modified polythiophene-coated graphene; (5) The recycled polyester, modified polythiophene-coated graphene, and azobisisobutyronitrile are mixed uniformly in a mass ratio of 1:(0.06-0.08):(0.002-0.004), placed in an internal mixer, stirred at 240-250°C for 10-12 minutes, placed in a mold for compression molding, and naturally cooled to room temperature before demolding to obtain an impact-resistant recycled plastic.
4. The method for preparing impact-resistant recycled plastic according to claim 3, characterized in that: The reaction process of the ultraviolet absorbing monomer in step (2) is: ; Where R is: .
5. The method for preparing impact-resistant recycled plastic according to claim 3, characterized in that: In step (3), the heat stabilizer is trimethyl phosphate and the matting agent is titanium dioxide.
6. The method for preparing impact-resistant recycled plastic according to claim 3, characterized in that: The preparation method of the mixed solution in step (4) is as follows: in a nitrogen atmosphere, graphene, anhydrous ferric chloride and tetrahydrofuran are uniformly mixed in a mass ratio of 1:(0.1-0.3):(10-12), and ultrasonically treated for 1-2 hours to prepare a mixed solution.
7. The method for preparing impact-resistant recycled plastic according to claim 3, characterized in that: The preparation method of the thiophene solution in step (4) is: thiophene, 3-thiophenesulfonamide, and tetrahydrofuran are uniformly mixed in a mass ratio of 1:(0.1-0.2):(6-8) to prepare a thiophene solution.
8. The method for preparing impact-resistant recycled plastic according to claim 3, characterized in that: The process parameters of the compression molding in step (5) are: at 240-250° C., 2-3 MPa, maintaining pressure for 3-5 min, keeping the pressure constant, cooling to 90-100° C. and maintaining the temperature for 2-3 h.