A hydrophobic coating for car cover and preparation method thereof
By using specific components and reaction processes to form a crosslinking network structure and fluorocarbon side chain, the problems of insufficient mechanical properties and environmentally friendly solvents of the existing car coat coating are solved, and the excellent hydrophobic and waterproofing effect and mechanical properties of the car coat coating are achieved. .
Patent Information
- Application Number
- CN202410712461.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-06-04
AI Technical Summary
The existing car coat coatings have shortcomings in terms of mechanical properties, and the solvents used do not meet environmental protection requirements, making it difficult to achieve excellent hydrophobic and waterproofing effects and good mechanical properties at the same time.
Polytetrahydrofuran glycol, modified terminal hydroxyl polyester, isophorone diisocyanate, 2,2-dihydroxymethylpropionic acid, triethylamine and 3,6-dioxa-1,8-octane di Components such as thiol form crosslinking network structures and fluorocarbon side chains through specific reaction and film formation processes to enhance the hydrophobicity and mechanical properties of the coating.
The prepared hydrophobic coating for car clothes has good hydrophobic and waterproofing effects and mechanical properties, which can effectively improve the waterproof performance and external force resistance of car clothes, and meet environmental protection requirements.
Smart Images

Figure CN118620507B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of coatings, and in particular to a hydrophobic coating for car covers and a preparation method thereof. Background Art
[0002] With the continuous expansion of the family car market in my country, there are more and more private cars in various cities. For car owners, there are fewer people who have private garages. Most of them are placed in open places, such as residential areas, roadsides, etc. However, when it rains and blows, it will cause damage to the surface of the car, so it needs to be protected, and car covers are produced. Car covers generally refer to polymer films attached to the surface of the vehicle's outer coating for protection and decoration. The main film car covers used in the market now are thermoplastic polyurethane, polyvinyl chloride materials, etc.
[0003] For example, the patent with the authorization announcement number CN109504258B discloses a method for making a transparent car cover with heat insulation and super hydrophobic functions. The invention uses water-based polyurethane-nano tin antimony oxide composite emulsion and fluorosilane solution as raw materials, and the prepared car cover has good heat insulation and hydrophobic effects. However, it does not improve the mechanical properties.
[0004] For example, the patent application publication number CN114752293A discloses a coating material for car cover film and a preparation method thereof. The invention uses TPU coating resin, silicone resin, and modified polyethylene wax as raw materials. The coating prepared has a good hydrophobic effect, but it also does not improve its mechanical properties. In addition, the solvents used in the invention are butanone, cyclohexane, etc., which do not meet environmental protection requirements. Summary of the invention
[0005] 1. Technical issues to be resolved
[0006] In view of the deficiencies in the prior art, the present invention provides a hydrophobic coating for a car cover and a preparation method thereof. The hydrophobic coating for a car cover prepared by the present invention has excellent hydrophobic and waterproof effects and good mechanical properties.
[0007] (II) Technical solution
[0008] A hydrophobic coating for a car cover, the hydrophobic coating for a car cover being composed of the following weight components: 100 weight components of polytetramethylene glycol, 50-100 weight components of modified terminal hydroxyl polyester, 60-100 weight components of isophorone diisocyanate, 15-24 weight components of 2,2-dihydroxymethylpropionic acid, 10-15 weight components of triethylamine, and 15-20 weight components of 3,6-dioxa-1,8-octanedithiol.
[0009] Preferably, the preparation method of the hydrophobic coating for car cover is:
[0010] (1) adding polytetrahydrofuran diol and modified terminal hydroxyl polyester into a flask, removing water under vacuum at 110-120° C. for 1-3 hours, reducing the temperature to 45-55° C., adding isophorone diisocyanate thereto under nitrogen conditions, reacting at 75-90° C. for 2-5 hours, then adding 2,2-dimethylol propionic acid thereto, continuing the reaction for 3-5 hours, reducing the temperature to 30-40° C., adding triethylamine thereto, neutralizing for 20-50 minutes, then adding 3,6-dioxa-1,8-octanedithiol thereto, extending the chain for 3-10 minutes, finally adding deionized water thereto, stirring and dispersing, and obtaining a modified polyurethane dispersion;
[0011] (2) The modified polyurethane dispersion is evenly coated on the tinplate sheet and allowed to form a film at room temperature for 2-3 days to obtain a hydrophobic coating for car covers.
[0012] Preferably, the preparation method of the modified hydroxyl-terminated polyester is:
[0013] S1. Add nano-silicon dioxide to a flask filled with 70-85% ethanol aqueous solution, ultrasonically disperse for 5-15 minutes, add 10-20% hydrochloric acid aqueous solution to adjust the pH to 3-5, add mercaptopropyl triethoxysilane to it, ultrasonically disperse, heat to 75-85° C., react for 8-12 hours, and after the reaction is completed, cool to room temperature, filter, wash, and dry to obtain intermediate 1;
[0014] S2, adding intermediate 1 and maleic anhydride into a flask filled with tetrahydrofuran solvent, stirring and dispersing, then adding benzoin dimethyl ether thereto, reacting under ultraviolet light at 365 nm for 20-40 minutes, and after the reaction is completed, rotary evaporation to obtain intermediate 2;
[0015] S3. Under nitrogen conditions, 3,5-di(hydroxymethyl)aniline is added to a flask containing chloroform solvent, stirred and dispersed, and triethylamine is added thereto. At 0-5°C, hexafluoropropylene oxide polymer is added thereto, stirred and dispersed, and the temperature is raised to 20-30°C. The reaction is carried out for 2-5 hours. After the reaction is completed, the mixture is washed with 5% sodium bicarbonate and dried to obtain a fluorinated diol;
[0016] S4. Under nitrogen conditions, add phthalic anhydride, intermediate 2, and fluorinated diol into a flask, stir and disperse, heat to 180-210°C, stir and react for 6-12 hours, and after the reaction is completed, cool to room temperature and dry to obtain a modified hydroxyl-terminated polyester.
[0017] Preferably, in S1, the mass ratio of nano-silica to mercaptopropyltriethoxysilane is 100:10-30.
[0018] Preferably, in S2, the mass ratio of intermediate 1, maleic anhydride and benzoin dimethyl ether is 100:40-60:0.3-0.5.
[0019] Preferably, in S3, the mass ratio of 3,5-di(hydroxymethyl)aniline, triethylamine and hexafluoropropylene oxide polymer is 1:0.65-0.8:2-3.
[0020] Preferably, in S4, the mass ratio of phthalic anhydride, intermediate 2, and fluorinated diol is 1:0.45-0.6:3-4.
[0021] (III) Beneficial technical effects
[0022] The present invention uses nano silicon dioxide, mercaptopropyl triethoxysilane and maleic anhydride as raw materials, and obtains intermediate 2 through hydrolysis condensation reaction and click reaction. The amino group contained in 3,5-di(hydroxymethyl)aniline is used to react with hexafluoropropylene oxide polymer under the catalysis of triethylamine to obtain fluorinated diol, which is used as a raw material to undergo ring-opening polymerization with phthalic anhydride and intermediate 2 to obtain modified terminal hydroxyl polyester. Finally, polytetrahydrofuran diol, modified terminal hydroxyl polyester, isophorone diisocyanate and the like are used as raw materials, and a modified polyurethane dispersion is obtained through reaction, which is applied on a tinplate sheet to form a film to obtain a hydrophobic coating for car covers.
[0023] The hydrophobic coating for car covers prepared by the present invention contains a large number of branched structures, which can be interlaced to form a cross-linked network structure. When subjected to external force, the force can be dispersed along the network structure, thereby improving the mechanical properties of the coating. In addition, when subjected to external force, the nano-silicon dioxide particles contained therein dispersed in the matrix can concentrate stress and cause the surrounding matrix to yield. In this process, a large amount of energy is absorbed, further improving the mechanical properties of the coating.
[0024] The hydrophobic coating for car cover prepared by the present invention contains more fluorocarbon side chains, and the polar groups of the main chain and the side chain are wrapped and shielded by the fluorocarbon side chains, so the free energy of the coating surface is small and the hydrophobicity is strong. The hydrophobic coating for car cover prepared by the present invention has good hydrophobic effect and mechanical properties, and its application in car cover can improve its hydrophobic and waterproof effect and its mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the preparation route of intermediate 2;
[0026] Figure 2 It is a preparation route for modified hydroxyl-terminated polyester. DETAILED DESCRIPTION
[0027] The following examples can enable professionals in this field to more fully understand the present invention, but do not limit the present invention in any way.
[0028] Example 1
[0029] (1) 10 g of nano-silica was added to a flask containing 100 mL of 80% ethanol aqueous solution, and ultrasonically dispersed for 12 min. A 20% hydrochloric acid aqueous solution was added thereto to adjust the pH to 5. 2 g of mercaptopropyltriethoxysilane was added thereto and ultrasonically dispersed. The temperature was raised to 80° C. and the reaction was carried out for 10 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed, and dried to obtain an intermediate 1.
[0030] (2) 3 g of intermediate 1 and 1.6 g of maleic anhydride were added to a flask containing 150 mL of tetrahydrofuran solvent, stirred and dispersed, and then 0.015 g of benzoin dimethyl ether was added thereto. The mixture was reacted under ultraviolet light at 365 nm for 30 min. After the reaction was completed, the mixture was rotary evaporated to obtain intermediate 2.
[0031] (3) Under nitrogen conditions, 5 g of 3,5-di(hydroxymethyl)aniline was added to a flask containing 100 mL of chloroform solvent, and the mixture was stirred and dispersed. Then, 3.6 g of triethylamine was added thereto. At 0° C., 12 g of hexafluoropropylene oxide polymer was added thereto, and the mixture was stirred and dispersed. The mixture was heated to 25° C. and reacted for 4 h. After the reaction was completed, the mixture was washed with 5% sodium bicarbonate and dried to obtain a fluorinated diol.
[0032] (4) Under nitrogen conditions, 8 g of phthalic anhydride, 4 g of intermediate 2, and 30 g of fluorinated diol were added to a flask, stirred and dispersed, and the temperature was raised to 190° C. and stirred for reaction for 12 h. After the reaction was completed, the mixture was cooled to room temperature and dried to obtain a modified hydroxyl-terminated polyester.
[0033] (5) 20 g of polytetrahydrofuran diol and 10 g of modified terminal hydroxyl polyester were added to a flask, and the temperature was reduced to 55° C. at 120° C. under vacuum to remove water for 2.5 h. 20 g of isophorone diisocyanate was added under nitrogen and reacted at 90° C. for 5 h. 3 g of 2,2-dimethylolpropionic acid was added and the reaction was continued for 3 h. The temperature was reduced to 30° C. 2 g of triethylamine was added and neutralized for 40 min. 3 g of 3,6-dioxa-1,8-octanedithiol was added and chain extended for 10 min. 90 g of deionized water was added and the mixture was stirred and dispersed to obtain a modified polyurethane dispersion.
[0034] (6) The modified polyurethane dispersion is evenly coated on a tinplate sheet and allowed to form a film at room temperature for 3 days to obtain a hydrophobic coating for car covers.
[0035] Example 2
[0036] (1) 10 g of nano-silica was added to a flask containing 100 mL of 85% ethanol aqueous solution, and ultrasonically dispersed for 5 min. A 20% hydrochloric acid aqueous solution was added thereto to adjust the pH to 4. 2 g of mercaptopropyltriethoxysilane was added thereto and ultrasonically dispersed. The temperature was raised to 80° C. and the reaction was carried out for 12 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed, and dried to obtain an intermediate 1.
[0037] (2) 3 g of intermediate 1 and 1.5 g of maleic anhydride were added to a flask containing 150 mL of tetrahydrofuran solvent, stirred and dispersed, and then 0.01 g of benzoin dimethyl ether was added thereto. The mixture was reacted under ultraviolet light at 365 nm for 40 min. After the reaction was completed, the mixture was rotary evaporated to obtain intermediate 2.
[0038] (3) Under nitrogen conditions, 5 g of 3,5-di(hydroxymethyl)aniline was added to a flask containing 100 mL of chloroform solvent, and the mixture was stirred and dispersed. Then, 3.5 g of triethylamine was added thereto. At 0° C., 12 g of hexafluoropropylene oxide polymer was added thereto, and the mixture was stirred and dispersed. The mixture was heated to 30° C. and reacted for 2 h. After the reaction was completed, the mixture was washed with 5% sodium bicarbonate and dried to obtain a fluorinated diol.
[0039] (4) Under nitrogen conditions, 8 g of phthalic anhydride, 4.8 g of intermediate 2, and 32 g of fluorinated diol were added to a flask, stirred and dispersed, heated to 210° C., and stirred for reaction for 10 h. After the reaction was completed, the mixture was cooled to room temperature and dried to obtain a modified hydroxyl-terminated polyester.
[0040] (5) 20 g of polytetrahydrofuran diol and 12 g of modified terminal hydroxyl polyester were added to a flask, and the temperature was reduced to 45 ° C. at 115 ° C. for 2 h under vacuum to remove water. Under nitrogen conditions, 12 g of isophorone diisocyanate was added thereto, and the temperature was reacted at 75 ° C. for 3 h. Then, 4.5 g of 2,2-dimethylolpropionic acid was added thereto, and the reaction was continued for 5 h. The temperature was reduced to 40 ° C., 2.5 g of triethylamine was added thereto, and the reaction was neutralized for 50 min. Then, 4 g of 3,6-dioxa-1,8-octanedithiol was added thereto, and the chain was extended for 5 min. Finally, 60 g of deionized water was added thereto, and the mixture was stirred and dispersed to obtain a modified polyurethane dispersion.
[0041] (6) The modified polyurethane dispersion is evenly coated on a tinplate sheet and allowed to form a film at room temperature for 3 days to obtain a hydrophobic coating for car covers.
[0042] Example 3
[0043] (1) 10 g of nano-silica was added to a flask containing 100 mL of 80% ethanol aqueous solution, and ultrasonically dispersed for 10 min. A 15% hydrochloric acid aqueous solution was added thereto to adjust the pH to 5. 2 g of mercaptopropyltriethoxysilane was added thereto and ultrasonically dispersed. The temperature was raised to 80° C. and the reaction was carried out for 10 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed, and dried to obtain an intermediate 1.
[0044] (2) 3 g of intermediate 1 and 1.5 g of maleic anhydride were added to a flask containing 150 mL of tetrahydrofuran solvent, and the mixture was stirred and dispersed. Then, 0.015 g of benzoin dimethyl ether was added thereto, and the mixture was reacted under ultraviolet light at 365 nm for 40 min. After the reaction was completed, the mixture was rotary evaporated to obtain intermediate 2.
[0045] (3) Under nitrogen conditions, 5 g of 3,5-di(hydroxymethyl)aniline was added to a flask containing 100 mL of chloroform solvent, and the mixture was stirred and dispersed. Then, 3.25 g of triethylamine was added thereto. At 5° C., 10 g of hexafluoropropylene oxide polymer was added thereto, and the mixture was stirred and dispersed. The mixture was heated to 20° C. and reacted for 5 h. After the reaction was completed, the mixture was washed with 5% sodium bicarbonate and dried to obtain a fluorinated diol.
[0046] (4) Under nitrogen conditions, 8 g of phthalic anhydride, 3.6 g of intermediate 2, and 24 g of fluorinated diol were added to a flask, stirred and dispersed, and the temperature was raised to 180° C. and stirred for reaction for 6 h. After the reaction was completed, the mixture was cooled to room temperature and dried to obtain a modified hydroxyl-terminated polyester.
[0047] (5) 20 g of polytetrahydrofuran diol and 15 g of modified terminal hydroxyl polyester were added to a flask, and the temperature was reduced to 50 ° C. at 110 ° C. for 1 h under vacuum to remove water. Under nitrogen conditions, 12 g of isophorone diisocyanate was added thereto, and the temperature was reacted at 75 ° C. for 2 h. Then 3.8 g of 2,2-dimethylolpropionic acid was added thereto, and the reaction was continued for 3 h. The temperature was reduced to 30 ° C., 2 g of triethylamine was added thereto, and the reaction was neutralized for 20 min. Then 4 g of 3,6-dioxa-1,8-octanedithiol was added thereto, and the chain was extended for 3 min. Finally, 50 g of deionized water was added thereto, and the mixture was stirred and dispersed to obtain a modified polyurethane dispersion.
[0048] (6) The modified polyurethane dispersion is evenly coated on a tinplate sheet and allowed to form a film at room temperature for 2 days to obtain a hydrophobic coating for car covers.
[0049] Example 4
[0050] (1) 10 g of nano-silica was added to a flask containing 100 mL of 85% ethanol aqueous solution, and ultrasonically dispersed for 15 min. A 10% hydrochloric acid aqueous solution was added thereto to adjust the pH to 3. 1 g of mercaptopropyltriethoxysilane was added thereto and ultrasonically dispersed. The temperature was raised to 85° C. and the reaction was carried out for 8 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed, and dried to obtain an intermediate 1.
[0051] (2) 3 g of intermediate 1 and 1.2 g of maleic anhydride were added to a flask containing 150 mL of tetrahydrofuran solvent, stirred and dispersed, and then 0.009 g of benzoin dimethyl ether was added thereto. The mixture was reacted under ultraviolet light at 365 nm for 20 min. After the reaction was completed, the mixture was rotary evaporated to obtain intermediate 2.
[0052] (3) Under nitrogen conditions, 5 g of 3,5-di(hydroxymethyl)aniline was added to a flask containing 100 mL of chloroform solvent, and the mixture was stirred and dispersed. Then, 4 g of triethylamine was added thereto. At 0° C., 15 g of hexafluoropropylene oxide polymer was added thereto, and the mixture was stirred and dispersed. The mixture was heated to 25° C. and reacted for 4 h. After the reaction was completed, the mixture was washed with 5% sodium bicarbonate and dried to obtain a fluorinated diol.
[0053] (4) Under nitrogen conditions, 8 g of phthalic anhydride, 4.5 g of intermediate 2, and 25 g of fluorinated diol were added to a flask, stirred and dispersed, and the temperature was raised to 200° C. and stirred for reaction for 12 h. After the reaction was completed, the mixture was cooled to room temperature and dried to obtain a modified hydroxyl-terminated polyester.
[0054] (5) 20 g of polytetrahydrofuran diol and 18 g of modified terminal hydroxyl polyester were added to a flask, and the temperature was reduced to 45 ° C. at 120 ° C. for 3 h under vacuum to remove water. 15 g of isophorone diisocyanate was added thereto under nitrogen conditions, and the reaction was carried out at 90 ° C. for 5 h. 4.8 g of 2,2-dimethylol propionic acid was added thereto, and the reaction was continued for 4 h. The temperature was reduced to 35 ° C. 3 g of triethylamine was added thereto and neutralized for 30 min. 3.5 g of 3,6-dioxa-1,8-octanedithiol was added thereto and chain extended for 10 min. Finally, 100 g of deionized water was added thereto and the mixture was stirred and dispersed to obtain a modified polyurethane dispersion.
[0055] (6) The modified polyurethane dispersion is evenly coated on a tinplate sheet and allowed to form a film at room temperature for 3 days to obtain a hydrophobic coating for car covers.
[0056] Example 5
[0057] (1) 10 g of nano-silica was added to a flask containing 100 mL of 70% ethanol aqueous solution, and ultrasonically dispersed for 8 min. A 15% hydrochloric acid aqueous solution was added thereto to adjust the pH to 4. 3 g of mercaptopropyltriethoxysilane was added thereto and ultrasonically dispersed. The temperature was raised to 75° C. and the reaction was carried out for 12 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed, and dried to obtain an intermediate 1.
[0058] (2) 3 g of intermediate 1 and 1.8 g of maleic anhydride were added to a flask containing 150 mL of tetrahydrofuran solvent, stirred and dispersed, and then 0.015 g of benzoin dimethyl ether was added thereto. The mixture was reacted under ultraviolet light at 365 nm for 40 min. After the reaction was completed, the mixture was rotary evaporated to obtain intermediate 2.
[0059] (3) Under nitrogen conditions, 5 g of 3,5-di(hydroxymethyl)aniline was added to a flask containing 100 mL of chloroform solvent, and the mixture was stirred and dispersed. Then, 3.5 g of triethylamine was added thereto. At 0° C., 14 g of hexafluoropropylene oxide polymer was added thereto, and the mixture was stirred and dispersed. The mixture was heated to 25° C. and reacted for 4 h. After the reaction was completed, the mixture was washed with 5% sodium bicarbonate and dried to obtain a fluorinated diol.
[0060] (4) Under nitrogen conditions, 8 g of phthalic anhydride, 4.8 g of intermediate 2, and 32 g of fluorinated diol were added to a flask, stirred and dispersed, heated to 210° C., and stirred for reaction for 10 h. After the reaction was completed, the mixture was cooled to room temperature and dried to obtain a modified hydroxyl-terminated polyester.
[0061] (5) 20 g of polytetrahydrofuran diol and 20 g of modified terminal hydroxyl polyester were added to a flask, and the temperature was reduced to 55° C. at 120° C. for 2 h under vacuum to remove water. 20 g of isophorone diisocyanate was added thereto under nitrogen and the temperature was reacted at 80° C. for 4 h. 3 g of 2,2-dimethylolpropionic acid was added thereto and the temperature was reduced to 35° C. 3 g of triethylamine was added thereto and the reaction was continued for 4 h. The temperature was reduced to 35° C. 3 g of triethylamine was added thereto and the reaction was neutralized for 40 min. 3.5 g of 3,6-dioxa-1,8-octanedithiol was added thereto and the chain was extended for 5 min. Finally, 80 g of deionized water was added thereto and the mixture was stirred and dispersed to obtain a modified polyurethane dispersion.
[0062] (6) The modified polyurethane dispersion is evenly coated on a tinplate sheet and allowed to form a film at room temperature for 3 days to obtain a hydrophobic coating for car covers.
[0063] Comparative Example 1
[0064] The difference between this comparative example and Example 1 is that step (5) does not contain modified hydroxyl-terminated polyester.
[0065] The contact angle meter was used to test the hydrophobicity of the coating.
[0066] Refer to GB / T9286-1998, use a knife to do a scratch test to test adhesion. Adhesion levels are divided into 0-5 levels, with 0 being the best.
[0067] Table 1: Hydrophobicity and adhesion performance tests of various embodiments and comparative examples
[0068] Contact angle (°) Adhesion grade (grade) Example 1 94.3 Level 0 Example 2 119.1 Level 0 Example 3 123.8 Level 0 Example 4 132.4 Level 0 Example 5 130.9 Level 0 Comparative Example 1 80.1 Level 2
[0069] The larger the contact angle, the worse the hydrophilicity and the better the hydrophobicity. As can be seen from the table, the coating prepared by the present invention has a good hydrophobic effect.
[0070] Referring to GB / T1720-79, a paint film impactor was used to conduct the coating impact resistance test experiment.
[0071] Refer to GB / T528-2009 and use an electronic universal testing machine to test the tensile properties.
[0072] Table 2: Mechanical properties test results of various embodiments and comparative examples
[0073] Impact strength / kg·cm Tensile strength / MPa Example 1 62 0.726 Example 2 68 0.792 Example 3 74 0.843 Example 4 78 0.914 Example 5 75 0.890 Comparative Example 1 48 0.512
[0074] It can be seen from the table that the coating prepared by the present invention has good mechanical properties.
[0075] Finally, it should be noted that the above examples are only specific embodiments of the present invention. Obviously, the present invention is not limited to the above examples, and many variations are possible. All variations that can be directly derived or associated with the content disclosed by a person skilled in the art should be considered as the protection scope of the present invention.
Claims
1. A hydrophobic coating for car cover, characterized in that: The hydrophobic coating for car covers is composed of the following components by weight: 100 components by weight of polytetramethylene glycol, 50-100 components by weight of modified terminal hydroxyl polyester, 60-100 components by weight of isophorone diisocyanate, 15-24 components by weight of 2,2-dimethylolpropionic acid, 10-15 components by weight of triethylamine, and 15-20 components by weight of 3,6-dioxa-1,8-octanedithiol; The preparation method of the modified hydroxyl-terminated polyester is: S1. Add nano-silica to a flask containing 70-85% ethanol aqueous solution, ultrasonically disperse for 5-15 minutes, add 10-20% hydrochloric acid aqueous solution to adjust the pH to 3-5, add mercaptopropyltriethoxysilane, ultrasonically disperse, heat to 75-85°C, react for 8-12 hours, and after the reaction is completed, cool to room temperature, filter, wash, and dry to obtain intermediate 1; S2, adding intermediate 1 and maleic anhydride to a flask containing tetrahydrofuran solvent, stirring and dispersing, then adding benzoin dimethyl ether, reacting under ultraviolet light at 365nm for 20-40min, and after completion of the reaction, rotary evaporation to obtain intermediate 2; S3. Under nitrogen conditions, 3,5-di(hydroxymethyl)aniline was added to a flask containing chloroform solvent, stirred and dispersed, and triethylamine was added thereto. Hexafluoropropylene oxide polymer was added thereto at 0-5°C, stirred and dispersed, and the temperature was raised to 20-30°C. The reaction was carried out for 2-5 hours. After the reaction was completed, the mixture was washed with 5% sodium bicarbonate and dried to obtain a fluorinated diol; S4. Under nitrogen conditions, add phthalic anhydride, intermediate 2, and fluorinated diol into a flask, stir and disperse, heat to 180-210°C, stir and react for 6-12 hours. After the reaction is completed, cool to room temperature and dry to obtain a modified hydroxyl-terminated polyester.
2. The hydrophobic coating for car cover according to claim 1, characterized in that: The preparation method of the hydrophobic coating for car cover is: (1) adding polytetrahydrofuran diol and modified hydroxyl-terminated polyester to a flask, removing water in vacuo at 110-120° C. for 1-3 hours, reducing the temperature to 45-55° C., adding isophorone diisocyanate thereto under nitrogen, reacting at 75-90° C. for 2-5 hours, then adding 2,2-dimethylolpropionic acid thereto, continuing the reaction for 3-5 hours, reducing the temperature to 30-40° C., adding triethylamine thereto, neutralizing for 20-50 minutes, then adding 3,6-dioxa-1,8-octanedithiol thereto, carrying out chain extension for 3-10 minutes, finally adding deionized water thereto, stirring and dispersing, and obtaining a modified polyurethane dispersion; (2) The modified polyurethane dispersion is evenly coated on the tinplate sheet and formed into a film at room temperature for 2-3 days to obtain a hydrophobic coating for car cover.
3. The hydrophobic coating for car cover according to claim 1, characterized in that: In the S1, the mass ratio of nano-silica to mercaptopropyltriethoxysilane is 100:10-30.
4. The hydrophobic coating for car cover according to claim 1, characterized in that: In the above-mentioned S2, the mass ratio of the intermediate 1, maleic anhydride and benzoin dimethyl ether is 100:40-60:0.3-0.
5.
5. The hydrophobic coating for car cover according to claim 1, characterized in that: In the S3, the mass ratio of 3,5-di(hydroxymethyl)aniline, triethylamine, and hexafluoropropylene oxide polymer is 1:0.65-0.8:2-3.
6. The hydrophobic coating for car cover according to claim 1, characterized in that: In the above-mentioned S4, the mass ratio of phthalic anhydride, intermediate 2, and fluorinated diol is 1:0.45-0.6:3-4.