Electrolyte, preparation method and electrodeposition method of porous nickel-cobalt-tungsten hydrogen evolution catalytic electrode
By using a combination of nickel sulfate, cobalt sulfate, sodium tungstate, sodium citrate, sodium chloride and ammonium chloride in the electrolyte, a constant current DC electrode deposition method is used to solve the complex process of porous hydrogen evolution catalytic electrodes and high power supply requirements. Problem, simple preparation and good hydrogen evolution performance of porous nickel-cobalt-tungsten hydrogen evolution catalytic electrode are achieved.
Patent Information
- Application Number
- CN202411090743.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-09
AI Technical Summary
In the prior art, the electrodeposition process of porous hydrogen evolution catalytic electrodes is complex and has high requirements for electrodeposition power supply. The preparation method of porous nickel-cobalt-tungsten hydrogen evolution catalytic electrodes has not been developed.
Provide an electrolyte and electrodeposition method for porous nickel-cobalt tungsten hydrogen evolution catalytic electrode. The electrolyte consists of water, nickel sulfate, cobalt sulfate, sodium tungstate, sodium citrate, sodium chloride and ammonium chloride, and passes a constant current direct current The preparation of deposition process avoids the problems of high power supply requirements and complex process.
The porous nickel-cobalt tungsten hydrogen evolution catalytic electrode is achieved directly to obtain porous distribution. The electrolyte is simple in composition and easy to prepare, without adding surfactant or adjusting pH value. The electrodeposition process does not require high power supply requirements, and the obtained plating layer has good hydrogen evolution. Catalytic properties.
Smart Images

Figure CN118621378B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the preparation of a hydrogen evolution catalytic electrode, and specifically discloses an electrolyte, a preparation method and an electrodeposition method of a porous nickel-cobalt-tungsten hydrogen evolution catalytic electrode. Background Art
[0002] With the continuous development of industrial technology, electrodeposited metal coatings are widely used in machinery, energy, catalysis and other fields. In order to meet the performance requirements of the industrial field for electrodeposited metal coatings, people have designed and developed metal coatings with various structures. Among them, metal coatings with porous structures can not only improve their wear resistance as surface protective layers, but also have other special properties such as catalytic loading, and have the potential for application as hydrogen evolution catalytic electrodes.
[0003] At present, common electrodeposition methods for porous hydrogen evolution catalytic electrodes include template method, sacrificial material method and pulse electrodeposition method. The template method refers to the use of a template with a specific pore structure (such as porous alumina, polystyrene microspheres, etc.) for electrodeposition when depositing porous electrodes. After the deposition is completed, the template is removed by chemical dissolution or pyrolysis; or a self-assembled structure formed by a surfactant, block copolymer, etc. is used as a template. After the electrodeposition is completed, the template material such as the surfactant is removed to obtain a porous metal. The pulse electrodeposition method usually requires strict control of the pulse period and amplitude of the electrodeposition current or voltage, temperature and other process parameters to ensure the quality and performance of the coating. In contrast, the constant current DC electrodeposition process not only has lower performance requirements for the deposition power supply, but also has simple process operation and is easy to implement.
[0004] Although technicians have already prepared a variety of porous metal layers by electrodeposition, the electrodeposition preparation method of porous nickel-cobalt-tungsten hydrogen evolution catalytic electrode has not yet been developed. Summary of the invention
[0005] In view of this, the purpose of the present invention is to overcome the problem that the porous hydrogen evolution catalytic electrode has complex process or high requirements on the electrodeposition power supply, and to provide an electrolyte, preparation method and electrodeposition method of a porous nickel-cobalt-tungsten hydrogen evolution catalytic electrode.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0007] The first technical purpose of the present invention is to provide an electrolyte for depositing a porous nickel-cobalt-tungsten hydrogen evolution catalytic electrode, wherein the solvent of the electrolyte is water, and the mass percentages of the components in the solute are: 0.62-1.77% nickel sulfate, 0.62-1.77% cobalt sulfate, 2.65-7.96% sodium tungstate, 8.84-18.58% sodium citrate, 0.79-1.77% sodium chloride, and 0.88-4.87% ammonium chloride.
[0008] It should be noted that nickel sulfate, cobalt sulfate and sodium tungstate in the electrolyte provide metal elements for the alloy, and tungsten is co-deposited under the induction of nickel and cobalt, and cobalt and tungsten elements have hydrogen evolution catalytic properties. Therefore, a porous structure can be formed on the surface of the alloy layer through the hydrogen evolution process during the electrodeposition process to obtain a porous nickel-cobalt-tungsten hydrogen evolution catalytic electrode. Sodium citrate is a complexing agent that plays a role in complexing metal ions, and the adjustment of the content of sodium citrate will change the pH value of the electrolyte. As the pH value of the alkaline electrolyte increases, the hydrogen evolution effect of the electrolyte will increase, so that the pore structure of the prepared alloy layer increases. The appropriate addition of ammonium chloride can improve the stability of the electrolyte, and it will also affect the pH value of the electrolyte. The addition of sodium chloride enhances the conductivity of the electrolyte and can improve the current efficiency.
[0009] The second technical purpose of the present invention is to provide a method for preparing an electrolyte for a porous nickel-cobalt-tungsten hydrogen evolution catalytic electrode, which specifically comprises the following steps:
[0010] Weigh nickel sulfate, cobalt sulfate, sodium tungstate, sodium citrate, sodium chloride and ammonium chloride respectively, dissolve nickel sulfate and cobalt sulfate in water to obtain a mixed aqueous solution of nickel salt-cobalt salt, dissolve sodium tungstate in water to obtain a sodium tungstate aqueous solution, dissolve sodium citrate in water to obtain a sodium citrate aqueous solution, and dissolve sodium chloride and ammonium chloride in water to obtain a chloride aqueous solution;
[0011] First, a sodium tungstate aqueous solution and a sodium citrate aqueous solution are mixed to obtain a mixed solution, and then a nickel salt-cobalt salt mixed aqueous solution and a chloride aqueous solution are added to the mixed solution; water is added to adjust the concentration of the electrolyte used to deposit the porous nickel-cobalt-tungsten hydrogen evolution catalytic electrode as described above, and the electrolyte is obtained by mixing evenly.
[0012] It should be noted that the purpose of adding and mixing in batches is to avoid dissolving multiple reagents together to form precipitation, which would affect the use and performance of the electrolyte.
[0013] The third technical purpose of the present invention is to provide a method for electrodeposition of a porous nickel-cobalt-tungsten hydrogen evolution catalytic electrode, the specific steps of which are as follows:
[0014] S1, polishing the plated substrate, washing it with water, soaking it in 1 mol / L sodium carbonate at room temperature, taking it out, washing it with water, soaking it in 1 mol / L dilute hydrochloric acid at room temperature, taking it out, rinsing it with distilled water and setting it aside;
[0015] S2, using the plated substrate treated in step S1 as the cathode and the pure platinum plate as the anode, immersing them in the electrolyte as described above, and mechanically stirring to perform electrochemical deposition. After the electrodeposition is completed, immersing the plated substrate in deionized water to recover the electrolyte on the surface of the plated substrate, and then rinsing with ethanol and drying to obtain the porous nickel-cobalt-tungsten hydrogen evolution catalytic electrode.
[0016] It should be noted that mechanical stirring or cathode movement can ensure the uniformity of electrolyte composition during the electrochemical deposition process; and soaking and rinsing the surface of the plated part after electrodeposition can ensure that there is no electrolyte residue on the surface of the obtained coating.
[0017] Preferably, the soaking time at room temperature using sodium carbonate is 3 minutes, and the soaking time at room temperature using dilute hydrochloric acid is 10 seconds.
[0018] Preferably, the drying temperature is 30-50° C., the drying time is 1-5 min, and the mechanical stirring speed is 200 rpm.
[0019] Preferably, the electrodeposition is carried out using a constant current, direct current continuous electrodeposition.
[0020] Furthermore, the current density of the cathode is 7-50 A / dm 2 The temperature of electrochemical deposition is 40-60 °C, and the time of DC continuous electrodeposition is 0.5-5 h.
[0021] Preferably, no surfactant is added in the electrodeposition method and no pH value of the electrolyte needs to be adjusted.
[0022] In summary, the electrolyte, preparation method and electrodeposition method of the porous nickel-cobalt-tungsten hydrogen evolution catalytic electrode provided by the present invention have the following advantages:
[0023] The porous nickel-cobalt-tungsten hydrogen evolution catalytic electrode with a porous structure can be directly obtained by the present invention. Not only is the electrolyte composition simple and easy to prepare, but no other surfactant is added to the electrolyte, and the pH value of the electrolyte does not need to be additionally adjusted. The present invention adopts constant current and direct current continuous electrodeposition, does not need to change parameters during the electrodeposition process, and has low requirements on the power supply used for electrodeposition. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0025] Figure 1 This is the SEM image of Example 1 of the present invention;
[0026] Figure 2 1 is a cyclic voltammetry scanning curve diagram of Example 1 of the present invention;
[0027] Figure 3 It is a double-layer capacitance fitting diagram of Example 1 of the present invention;
[0028] Figure 4 This is a linear sweep voltammetry curve of Example 1 of the present invention;
[0029] Figure 5 This is the SEM image of Example 2 of the present invention;
[0030] Figure 6 1 is a cyclic voltammetry scanning curve diagram of Example 2 of the present invention;
[0031] Figure 7 It is a double-layer capacitance fitting diagram of Example 2 of the present invention;
[0032] Figure 8 This is a linear sweep voltammetry curve diagram of Example 2 of the present invention;
[0033] Fig. 9 This is the SEM image of Example 3 of the present invention;
[0034] Fig.10 1 is a cyclic voltammetry scanning curve diagram of Example 3 of the present invention;
[0035] Fig.11 It is a double-layer capacitance fitting diagram of Example 3 of the present invention;
[0036] Fig.12 This is a linear sweep voltammetry curve diagram of Example 3 of the present invention;
[0037] Fig.13 This is the SEM image of Example 4 of the present invention;
[0038] Fig.14 4 is a cyclic voltammetry scanning curve diagram of Example 4 of the present invention;
[0039] Fig.15 It is a double-layer capacitance fitting diagram of Example 4 of the present invention;
[0040] Fig.16 This is a linear sweep voltammetry curve diagram of Example 4 of the present invention;
[0041] Fig.17 This is the SEM image of Example 5 of the present invention;
[0042] Fig.18 1 is a cyclic voltammetry scanning curve diagram of Example 5 of the present invention;
[0043] Fig.19 It is a double-layer capacitance fitting diagram of Example 5 of the present invention;
[0044] Fig. 20 This is a linear sweep voltammetry curve of Example 5 of the present invention;
[0045] Fig.21 This is the SEM image of Example 6 of the present invention;
[0046] Fig. 22 : is a cyclic voltammetry scanning curve diagram of Example 6 of the present invention;
[0047] Fig.23 It is a double-layer capacitance fitting diagram of Example 6 of the present invention;
[0048] Fig.24 This is a linear sweep voltammetry curve diagram of Example 6 of the present invention;
[0049] Fig.25 This is the SEM image of Example 7 of the present invention;
[0050] Fig.26 is a cyclic voltammetry scanning curve diagram of Example 7 of the present invention;
[0051] Fig. 27 It is a double-layer capacitance fitting diagram of Example 7 of the present invention;
[0052] Fig.28 This is a linear sweep voltammetry curve diagram of Example 7 of the present invention;
[0053] Fig.29 This is the SEM image of Example 8 of the present invention;
[0054] Fig.30 is a cyclic voltammetry scanning curve diagram of Example 8 of the present invention;
[0055] Fig.31 It is a double-layer capacitance fitting diagram of Example 8 of the present invention;
[0056] Fig.32 This is a linear sweep voltammetry curve diagram of Example 8 of the present invention;
[0057] Fig.33 This is the SEM image of Example 9 of the present invention;
[0058] Fig.34 is a cyclic voltammetry scanning curve diagram of Example 9 of the present invention;
[0059] Fig.35 It is a double-layer capacitance fitting diagram of Example 9 of the present invention;
[0060] Fig.36 This is a linear sweep voltammetry curve of Example 9 of the present invention;
[0061] Fig.37 is the SEM image of Example 10 of the present invention;
[0062] Fig.38 1 is a cyclic voltammetry scanning curve diagram of Example 10 of the present invention;
[0063] Fig.39It is a double-layer capacitance fitting diagram of Example 10 of the present invention;
[0064] Fig.40 is a linear sweep voltammetry curve diagram of Example 10 of the present invention;
[0065] Fig.41 This is the SEM image of Example 11 of the present invention;
[0066] Fig.42 1 is a cyclic voltammetry scanning curve diagram of Example 11 of the present invention;
[0067] Fig.43 It is a double-layer capacitance fitting diagram of Example 11 of the present invention;
[0068] Fig.44 This is a linear sweep voltammetry curve of Example 11 of the present invention. DETAILED DESCRIPTION
[0069] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0070] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this application are performed using conventional test methods in the art. It should be understood that the terms described in this application are only used to describe specific implementation methods and are not used to limit the content disclosed in this application.
[0071] Unless otherwise specified, the technical and scientific terms used in this document have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs; other experimental methods and technical means not specifically specified in this application refer to experimental methods and technical means commonly used by ordinary technicians in this field.
[0072] In order to better illustrate the content of the present application, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the main purpose of the present application.
[0073] Under the premise of no conflict, the technical features disclosed in the embodiments of the present application can be combined arbitrarily, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present application.
[0074] The invention discloses an electrolyte, a preparation method and an electrodeposition method of a porous nickel-cobalt-tungsten hydrogen evolution catalytic electrode.
[0075] In order to better understand the present invention, the present invention is further specifically described below through the following examples, but it should not be understood as a limitation of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the protection scope of the present invention.
[0076] Example 1
[0077] This embodiment discloses an electrolyte for a porous nickel-cobalt-tungsten hydrogen evolution catalytic electrode. The solvent of the electrolyte is water, and the mass percentages of the components in the solute are: 1.77% nickel sulfate, 0.62% cobalt sulfate, 4.42% sodium tungstate, 13.27% sodium citrate, 0.88% sodium chloride, and 2.65% ammonium chloride.
[0078] A method for preparing 1L of an electrolyte having the above composition for depositing a porous nickel-cobalt-tungsten hydrogen evolution catalytic electrode specifically comprises:
[0079] Dissolve 20 g of nickel sulfate and 7 g of cobalt sulfate in water to obtain a mixed aqueous solution of nickel salt and cobalt salt;
[0080] Take 50 g of sodium tungstate and dissolve it in water to obtain a sodium tungstate aqueous solution;
[0081] 150 g of sodium citrate was dissolved in water to obtain a sodium citrate aqueous solution;
[0082] Dissolve 30 g of ammonium chloride and 10 g of sodium chloride in water to obtain a chloride aqueous solution;
[0083] The sodium tungstate aqueous solution and the sodium citrate aqueous solution are mixed, the mixed aqueous solution of nickel salt-cobalt salt and the chloride aqueous solution are added to the mixed aqueous solution of sodium tungstate and sodium citrate, and water is added to 1 L to obtain the final desired electrolyte.
[0084] Furthermore, the electrodeposition method of the porous nickel-cobalt-tungsten hydrogen evolution catalytic electrode specifically comprises the following steps:
[0085] S1, polish the substrate, wash it with water, put it in 1 mol / L sodium carbonate, soak it at room temperature for 3 min, take it out, wash it with water again, put it in 1 mol / L dilute hydrochloric acid, soak it at room temperature for 10 s, take it out and rinse it with distilled water for later use;
[0086] S2, the plated part treated in step S1 is used as the cathode and the pure platinum plate is used as the anode, and is immersed in the electrolyte obtained above, the electrolyte temperature is maintained at 50 °C, and the cathode current density is 7 A / dm 2, DC electrodeposition time is 5 h, mechanical stirring speed is 200 rpm, constant current, DC continuous electrodeposition is adopted; after deposition is completed, the plated parts are immersed in deionized water to recover the electrolyte on the surface of the plated parts, after soaking for 20 s, rinsed with ethanol for 10 s and then dried.
[0087] Example 2
[0088] The cathode current density is 10 A / dm 2 , DC deposition time is 3 h, and other conditions are the same as those in Example 1.
[0089] Example 3
[0090] The cathode current density is 50 A / dm 2 , DC deposition time is 0.6 h, and other conditions are the same as those in Example 1.
[0091] Example 4
[0092] The mass percentages of the components in the electrolyte solute are: nickel sulfate 1.32%, cobalt sulfate 1.32%, sodium tungstate 4.42%, sodium citrate 13.27%, sodium chloride 0.88%, ammonium chloride 2.65%; the cathode current density is 10 A / dm 2 , DC deposition time is 3 h, and other conditions are the same as those in Example 1.
[0093] Example 5
[0094] The mass percentages of the components in the electrolyte solute are: nickel sulfate 1.32%, cobalt sulfate 1.32%, sodium tungstate 4.42%, sodium citrate 13.27%, sodium chloride 0.88%, ammonium chloride 2.65%; the cathode current density is 50 A / dm 2 , DC deposition time is 0.6 h, and other conditions are the same as those in Example 1.
[0095] Example 6
[0096] The mass percentages of the components in the electrolyte solute are: nickel sulfate 0.62%, cobalt sulfate 1.77%, sodium tungstate 4.42%, sodium citrate 13.27%, sodium chloride 0.88%, and ammonium chloride 2.65%; other conditions are the same as in Example 1.
[0097] Example 7
[0098] The mass percentages of the components in the electrolyte solute are: nickel sulfate 0.62%, cobalt sulfate 1.77%, sodium tungstate 4.42%, sodium citrate 13.27%, sodium chloride 0.88%, ammonium chloride 2.65%; the cathode current density is 10 A / dm 2 , DC deposition time is 3 h, and other conditions are the same as those in Example 1.
[0099] Example 8
[0100] The mass percentages of the components in the electrolyte solute are: nickel sulfate 0.62%, cobalt sulfate 1.77%, sodium tungstate 4.42%, sodium citrate 13.27%, sodium chloride 0.88%, ammonium chloride 2.65%; the cathode current density is 50 A / dm 2 , DC deposition time is 0.6 h, and other conditions are the same as those in Example 1.
[0101] Example 9
[0102] The mass percentages of the components in the electrolyte solute are: sodium tungstate 7.96%, nickel sulfate 1.77%, cobalt sulfate 0.62%, sodium citrate 13.27%, sodium chloride 0.88%, ammonium chloride 2.65%; the cathode current density is 50 A / dm 2 , DC deposition time is 0.6 h, and other conditions are the same as those in Example 1.
[0103] Example 10
[0104] The mass percentages of the components in the electrolyte solute are: sodium citrate 18.58%, nickel sulfate 1.77%, cobalt sulfate 0.62%, sodium tungstate 4.42%, sodium chloride 0.88%, ammonium chloride 2.65%; the cathode current density is 50 A / dm 2 , DC deposition time is 0.6 h, and other conditions are the same as those in Example 1.
[0105] Embodiment 11
[0106] The mass percentages of the components in the electrolyte solute are: ammonium chloride 4.86%, nickel sulfate 1.77%, cobalt sulfate 0.62%, sodium tungstate 4.42%, sodium citrate 13.27%, sodium chloride 0.88%; the cathode current density is 50 A / dm 2 , DC deposition time is 0.6 h, and other conditions are the same as those in Example 1.
[0107] In order to further demonstrate the beneficial effects of the present invention and to better understand the present invention, the following experimental examples and comparative examples are used to further illustrate the technical features disclosed in the present invention, but they should not be understood as limiting the present invention. Other improvements made by those skilled in the art based on the above invention content without creative work are also considered to fall within the scope of protection of the present invention.
[0108] (1) The electrocatalytic hydrogen evolution performance of the coatings prepared in Examples 1-11 was tested. Before the test, the samples were fixed with a test device so that the coatings were exposed for 1 cm. 2The circular area. The test parameters of the cyclic voltammetry curve are: open circuit potential of plus or minus 50 mV, scanning rate of 10 mV / s-100 mV / s, and 20 test cycles. The half of the absolute value of the difference between the two current densities corresponding to the intermediate potential value (i.e., the open circuit potential value) at different scanning rates is obtained respectively, and the slope obtained by linear fitting at the corresponding scanning rate is the double layer capacitance value. The test parameters of the linear scanning voltammetry curve are: initial potential: -0.7 V (relative to mercuric oxide electrode), termination voltage is -1.5 V (relative to mercuric oxide electrode), scanning rate is 5 mV / s, and the cathode polarization curve of the sample is recorded, taking 10 mA / cm 2 The potential corresponding to the current density is the hydrogen evolution overpotential.
[0109] As can be seen from the attached figure, the nickel-cobalt-tungsten coating with a porous structure can be obtained by electrodeposition under the conditions of the present invention. The prepared coating has a certain hydrogen evolution performance, and the lowest hydrogen evolution overpotential is 98 mV. In the cyclic voltammetry test of the deposited coating at different scan rates, it can be observed that as the deposition current density increases, the pore structure of the coating becomes denser and more complex, and the double-layer capacitance value measured for the corresponding coating is relatively higher, that is, there are more electrocatalytic active sites; at the 10 mA / cm obtained in the linear sweep voltammetry test, the 2 The potential corresponding to the current density shows a law similar to that of the double-layer capacitance.
[0110] (2) Scanning electron microscopy (SEM) test was performed on the surface of the prepared nickel-cobalt-tungsten hydrogen evolution catalytic electrode. It can be seen that the electrode surface presents a porous distribution structure. The porous structure of the coating surface gradually increases with the increase of current density. The change of electrolyte composition has little effect on the coating structure. Electrochemical tests show that the electrode has certain hydrogen evolution catalytic performance.
[0111] In the three groups of Examples 1, 2, 3 and 4, 5 and 6, 7, 8, the electrolyte composition in the group remains unchanged, only the cathode current density and deposition time are changed. The SEM image of the obtained coating shows that as the current density increases, the number of micropores on the coating surface increases and the distribution is more dense. The double electric layer capacitance value of the obtained coating also shows an upward trend as the current density increases accordingly. The content of nickel sulfate in these three groups of electrolytes decreases successively, and the content of cobalt sulfate increases successively. When under the same cathode current density, the number and distribution of pores on the surface of the obtained coating are closer, and as the nickel sulfate content decreases and the cobalt sulfate content increases, the colony-like structure of the obtained coating is more obvious.
[0112] The electrolyte composition of Example 9 increases the content of sodium tungstate compared with Example 1, and the surface of the obtained coating has a finer colony structure than that of Example 1. The double layer capacitance and hydrogen evolution overpotential of the coating of Example 9 are also significantly improved compared with those of Example 1.
[0113] The electrolyte composition of Example 10 increases the content of sodium citrate compared to Example 1, thereby causing the pH value of the electrolyte to increase, intensifying the hydrogen evolution reaction accompanying the deposition process, resulting in more pores and microgaps on the surface of the coating, thereby increasing the double layer capacitance of the coating, and reducing the hydrogen evolution overpotential to a certain extent, thereby improving the hydrogen evolution performance of the coating.
[0114] The electrolyte composition of Example 11 increases the content of ammonium chloride compared to Example 1, thereby causing the pH value of the electrolyte to decrease, reducing the hydrogen evolution reaction accompanying the deposition process, and in addition, chloride ions can inhibit the grain growth during the metal deposition process, resulting in the formed coating having a denser and smoother surface than that of Example 1.
[0115] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for electrodeposition of a porous nickel-cobalt-tungsten hydrogen evolution catalytic electrode, characterized in that: The specific steps of the method are as follows: S1, polishing the plated substrate, washing it with water, soaking it in 1 mol / L sodium carbonate at room temperature, taking it out, washing it with water, soaking it in 1 mol / L dilute hydrochloric acid at room temperature, taking it out, rinsing it with distilled water and setting it aside; S2, using the plated substrate treated in step S1 as a cathode and a pure platinum plate as an anode, immersing them in an electrolyte, and mechanically stirring them for electrochemical deposition. After the electrodeposition is completed, immersing the plated substrate in deionized water to recover the electrolyte on the surface of the plated substrate, and then rinsing with ethanol and drying to obtain the porous nickel-cobalt-tungsten hydrogen evolution catalytic electrode; The electrochemical deposition adopts constant current, direct current continuous electrodeposition, and the current density of the cathode is 7-50A / dm 2 , the temperature of electrochemical deposition is 40-60 °C, and the time of DC continuous electrodeposition is 0.5-5 h; The solvent of the electrolyte is water, and the mass percentages of the components in the solute are as follows: Nickel sulfate 0.62-1.77%, cobalt sulfate 0.62-1.77%, sodium tungstate 2.65-7.96%, sodium citrate 8.84-18.58%, sodium chloride 0.79-1.77%, ammonium chloride 0.88-4.87%.
2. The method for electrodeposition of a porous nickel-cobalt-tungsten hydrogen evolution catalytic electrode according to claim 1, characterized in that: The immersion time at room temperature using sodium carbonate was 3 min, and the immersion time at room temperature using dilute hydrochloric acid was 10 s.
3. The method for electrodeposition of a porous nickel-cobalt-tungsten hydrogen evolution catalytic electrode according to claim 1, characterized in that: The drying temperature is 30-50°C, the drying time is 1-5 min, and the mechanical stirring rate is 200 rpm.
4. The method for electrodeposition of a porous nickel-cobalt-tungsten hydrogen evolution catalytic electrode according to claim 1, characterized in that: The preparation method of the electrolyte specifically comprises the following steps: Weigh nickel sulfate, cobalt sulfate, sodium tungstate, sodium citrate, sodium chloride and ammonium chloride respectively, dissolve nickel sulfate and cobalt sulfate in water to obtain a mixed aqueous solution of nickel salt-cobalt salt, dissolve sodium tungstate in water to obtain a sodium tungstate aqueous solution, dissolve sodium citrate in water to obtain a sodium citrate aqueous solution, and dissolve sodium chloride and ammonium chloride in water to obtain a chloride aqueous solution; first mix the sodium tungstate aqueous solution and the sodium citrate aqueous solution to obtain a mixed solution, then add the mixed aqueous solution of nickel salt-cobalt salt and the chloride aqueous solution to the mixed solution; add water to adjust the concentration of the electrolyte used to deposit a porous nickel-cobalt-tungsten hydrogen evolution catalytic electrode, and mix evenly to obtain an electrolyte.
Citation Information
Patent Citations
Preparation method of porous nickel-based copper rhenium composite hydrogen evolution electrode
CN109750317A
Porous nickel-based hydrogen evolution electrode composite material
CN112680744A
Plating solution of nickel-cobalt-tungsten gradient plating layer, preparation method and electroplating method
CN114196997A
Porous nickel-molybdenum-cobalt hydrogen evolution electrode and preparation method and application thereof
CN114318393A
Nickel-cobalt-tungsten alloy electro-deposition solution for electroplating sintered neodymium-iron-boron permanent magnet and application of nickel-cobalt-tungsten alloy electro-deposition solution
CN117702205A