A method for preparing a magnetic spherical catalyst carrier

The multi-layer cladding structure is formed on magnetic particles by the disk granulator method, which solves the size and stability of existing magnetic catalyst support, and realizes the preparation of magnetic spherical catalyst support suitable for industrial-grade catalysis and induction heating catalytic reactions. .

CN118634865BActive Publication Date: 2024-11-08YUAN QIU XIN CAI LIAO (NAN TONG) YOU XIAN GONG SI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411117154.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-08
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

The particle size of existing magnetic catalyst support is too small to be used for industrial-grade catalysis, and the magnetic properties are easily destroyed or affect the catalytic reaction.

Method used

The disk granulator method is used to grow a multi-layered coated structure on the magnetic particles by rolling molding to form a magnetic spherical catalyst support with a particle size of 300-4000 μm. The magnetic core is protected by an inert gas atmosphere to avoid oxidation and excessive heating.

Benefits of technology

Magnetic spherical catalyst support suitable for industrial-grade catalysis is prepared, which improves magnetic isolation and catalytic activity, reduces production costs, and achieves efficient catalytic reactions through induction heating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118634865B_ABST
    Figure CN118634865B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a magnetic spherical catalyst carrier, comprising: step 10, adding magnetic particles, a first precursor powder and a first growth solution to a disc granulator, rolling the disc granulator so that the first precursor powder grows on the surface of the magnetic particles to obtain single-layer coated particles; step 20, adding single-layer coated particles, a second precursor powder and a second growth solution to the disc granulator, rolling the disc granulator so that the second precursor powder grows on the surface of the single-layer coated particles to obtain double-layer coated particles; step 30, calcining the double-layer coated particles under an inert or reducing gas atmosphere, and obtaining a calcined product after cooling; step 40, screening out a magnetic spherical catalyst carrier from the calcined product. The present invention provides a method for preparing a magnetic spherical catalyst carrier, which can prepare a magnetic spherical catalyst carrier with a particle size of submillimeter and above millimeter level, and the magnetism is well isolated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalyst carriers, and particularly relates to a method for preparing a magnetic spherical catalyst carrier. Background Art

[0002] Solid catalyst carriers with magnetic properties have many unique application advantages in heterogeneous catalysis, such as rapid separation, enrichment and recovery of catalysts through external magnetic fields, can be used as catalyst carriers in magnetically stabilized bed reactors, and can also use their magnetic properties to achieve induction heating of catalysts. Induction heating has recently become a unique catalytic heating scheme, in which heat is generated at magnetic sites by using an external alternating magnetic field and immediately transferred outward to the catalytic center to initiate and maintain the catalytic reaction of the reactants adsorbed thereon. Compared with the traditional Joule heating method of heating the entire reactor, the non-contact heating method of induction heating shows significant advantages: on the one hand, due to the selective absorption of radio frequency energy, the magnetic catalyst generates heat almost instantly, significantly reducing thermal inertia and improving the uniformity of temperature distribution in the reaction medium; on the other hand, induction heating only provides the catalyst with the heat energy required for its catalytic active sites to initiate and maintain the catalytic reaction, thereby avoiding overheating of the entire reactor and the reaction medium, greatly reducing heat loss and energy input, and also avoiding the degradation of reactants and the generation of by-products caused by overheating of the medium.

[0003] Commonly used magnetic catalyst carriers are usually required to have a certain specific surface area (usually greater than 80 m 2 / g), pore volume (usually required to be greater than 0.4 cm 3 / g), pore size (except for molecular sieve carriers, which are usually required to be greater than 5 nm) and / or activity (such as acidic or basic sites). However, common magnetic catalyst carriers are composed of a coating layer covering a magnetic center. Due to the presence of pores in the coating layer, the degree of isolation between the coated magnetic center and the outside world is poor, making it easy to be oxidized. Moreover, the poorly isolated magnetic center reacts and / or participates in the catalytic reaction during the catalytic reaction, resulting in the destruction of magnetism or affecting the catalytic reaction.

[0004] Moreover, the existing methods for preparing magnetic catalysts and carrier particles usually adopt methods such as hydrothermal method and sol-gel method which are mainly suitable for generating nanometer or micrometer-sized particles, and the particle size of the prepared particles is usually nanometer-sized and less than 100 micrometers. However, industrial-grade catalysis often requires particles in the sub-millimeter or millimeter scale. The magnetic catalysts and carrier particles obtained by the existing methods are too small in size and can only be used for laboratory-scale catalytic reactions, and cannot be truly used for industrial-grade catalysis. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for preparing a magnetic spherical catalyst carrier, which can prepare a magnetic spherical catalyst carrier with a particle size of submillimeter level and above millimeter level, and the magnetism is well isolated.

[0006] In order to solve the above technical problems, the present invention provides a method for preparing a magnetic spherical catalyst carrier, comprising the following steps:

[0007] Step 10, adding magnetic particles, a first precursor powder and a first growth solution into a disc granulator, and rolling the disc granulator to make the first precursor powder grow on the surface of the magnetic particles to obtain single-layer coated particles;

[0008] Step 20, adding the single-layer coated particles, the second precursor powder and the second growth solution into the disc granulator, and rolling the disc granulator so that the second precursor powder grows on the surface of the single-layer coated particles to obtain double-layer coated particles;

[0009] Step 30, calcining the double-layer coated particles in an inert or reducing gas atmosphere, and obtaining a calcined product after cooling;

[0010] Step 40, screening out the magnetic spherical catalyst carrier from the calcined product;

[0011] The magnetic spherical catalyst carrier comprises a magnetic core, a first wrapping layer covering the magnetic core, and a second wrapping layer covering the first wrapping layer.

[0012] As a further improvement of the embodiment of the present invention, the particle size of the magnetic spherical catalyst carrier is 300 to 4000 μm.

[0013] As a further improvement of the embodiment of the present invention, the particle size of the magnetic particles is 20 to 300 μm.

[0014] As a further improvement of the embodiment of the present invention, the ratio of the particle size of the magnetic particles to the target thickness of the first encapsulating layer is 1:0.5-3.

[0015] As a further improvement of the embodiment of the present invention, in step 10, the mass of the first precursor powder to be added is obtained using formula (1) according to the mass of the added magnetic particles, the particle size of the magnetic particles and the target thickness of the first coating layer:

[0016] m 11,烧前 = m 10 ρ 11,烧后 [( L 11 + r 10 ) 3 –r 10 3 ] / (ρ 10 r 10 3 w 11,烧后 ) Formula (1)

[0017] In the formula, m 11,烧前 represents the mass of the first precursor powder, in grams; m 10 Indicates the mass of magnetic particles, unit: gram; ρ 11,烧后 It indicates the tap density of the first coating layer after calcination, unit: g / cm3; L 11 Indicates the target thickness of the first wrapping layer, in microns; r 10 Represents the radius of the magnetic particle, unit: micrometer; ρ 10 Indicates the tap density of magnetic particles, unit: g / cm3; w 11,烧后 It indicates the residual mass percentage of the first precursor powder after calcination.

[0018] As a further improvement of the embodiment of the present invention, the particle size of the first precursor powder is less than 0.2 μm.

[0019] As a further improvement of the embodiment of the present invention, the pore volume of the first precursor powder is less than 0.3 cm 3 / g.

[0020] As a further improvement of the embodiment of the present invention, in the step 20, before adding the single-layer coated particles into the disc granulator, the single-layer coated particles are first calcined in an inert or reducing gas atmosphere.

[0021] As a further improvement of the embodiment of the present invention, the calcination temperature of the single-layer coated particles is 500 to 900 o C.

[0022] As a further improvement of the embodiment of the present invention, the calcination temperature of the double-layer coated particles is 300 to 700 o C.

[0023] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0024] (1) The method of the present invention is based on a rolling forming method, using magnetic particles with a particle size of 20 to 300 μm as growth nuclei. With the assistance of a growth solution, the precursor powder is adsorbed, coated and grown on the magnetic particles, thereby obtaining a magnetic spherical catalyst carrier with a particle size of 300 to 4000 μm for industrial-grade catalysis.

[0025] (2) The method of the present invention uses magnetic particles as growth nuclei, first allowing the first precursor powder to grow on the magnetic particles to obtain single-layer coated particles, and then allowing the second precursor powder to grow on the single-layer coated particles to obtain double-layer coated particles, which are then calcined in an inert gas atmosphere to form a multilayer structure. After calcination, the second precursor powder forms a second outermost coating layer, which serves as a catalyst carrier layer for loading the catalyst. After calcination, the first precursor powder forms a first coating layer between the magnetic core and the second coating layer, which serves as a protective layer for isolating the magnetic core to prevent the magnetic core from directly contacting the reactant and causing the magnetism to be broken or affecting the catalytic reaction. Calcination in an inert gas atmosphere protects the magnetic core, especially the magnetic core composed of Fe or Fe3O4, to prevent it from being over-oxidized at high temperatures.

[0026] (3) The method of the present invention uses a first precursor powder with ultrafine particle size and low pore volume. After calcination in an inert environment, the first coating layer obtained is more dense, further strengthening the isolation and protection of the magnetic core.

[0027] (4) The method of the present invention sets the ratio of the particle size of the magnetic particles to the target thickness of the first coating layer to 1:0.5-3. The first coating layer should not be too thin, otherwise it will not provide sufficient protection for the magnetic core. Although the first coating layer after calcination has a weak shielding effect on the magnetic field and a high heat transfer efficiency, the first coating layer should not be too thick, otherwise a large number of carrier particles that do not contain a magnetic core will be easily formed during the preparation process, and the thickness of the second coating layer with high catalytic activity can be limited, affecting the catalytic efficiency.

[0028] (5) The method of the present invention adds magnetic particles with uniform particle size as growth nuclei during rolling forming and granulation. Due to the affinity between the precursor powder and the growth nuclei, the precursor powder mainly grows on the basis of the growth nuclei. From the perspective of the speed of change of the particle size distribution with the preparation time, the speed difference of growth based on the growth nuclei is significantly smaller than the speed difference of self-nucleation and growth, so the method of the present invention can improve the uniformity of particle size. The method of the present invention can control the size of the product and improve the controllability of particle size by controlling the amount of precursor powder added according to the particle size of the magnetic particles, the target thickness of the first coating layer and the target thickness of the second coating layer.

[0029] (6) The method of the present invention is based on the rolling molding method, which uses a small amount of cheap raw materials and has low energy consumption. The output of a single batch can be increased by simply using a larger disc granulator, which can reach tens or even hundreds of kilograms at a time, and a single rolling molding does not exceed 30 minutes at most, which is time-saving, so the production cost per ton is low. Compared with the method of the present invention, the spray fluidization method is complicated, requires multiple rounds of growth, has a long preparation cycle (a single batch requires several hours, and multiple rounds of growth are required to reach the target size), and the energy consumption of evaporating the solvent is high, and the loss of raw materials is significant, resulting in high production costs. The oil (ammonia) column molding method and the water phase molding method have high energy consumption, slow curing speed, low efficiency, and high overall production costs. The spray drying method not only cannot obtain catalyst carriers in the range of 300 to 4000 μm, but also has a low single batch output (the spray process requires several hours to obtain tens of kilograms of product), and the energy cost caused by evaporating the solvent is also significant.

[0030] (7) The magnetic spherical catalyst carrier obtained by the method of the present invention can be used in catalytic reactions that use induction heating to provide heat. A magnetic catalyst is obtained by loading catalytically active substances such as Pd, Ni, and Fe on a magnetic spherical catalyst carrier, and placing the magnetic catalyst under an alternating magnetic field of 50 to 1000 kHz, so that the temperature of the catalyst surface can reach 50 to 1000 kHz. o C high temperature, triggering and maintaining Pd, Ni, Fe and other catalytic active substances catalyzing carbon-carbon coupling, hydrocarbon hydrogenation, hydrocarbon dehydrogenation, hydrocarbon reforming and other catalytic reactions; during the reaction process, the catalyst surface can be maintained at the required temperature, and the catalytic reaction medium, that is, the dispersed solution of the liquid-solid multiphase catalytic reaction or the reaction gas of the gas-solid multiphase catalytic reaction, has a medium temperature that is always equal to or less than the catalyst surface temperature; in this way, the catalytic reactor temperature occurring on the catalyst surface Pd, Ni, Fe and other catalytic active substances is always maintained at the most suitable reaction temperature, and the medium temperature will not be higher than the most suitable reaction temperature, thereby reducing the possibility of side reactions. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a schematic diagram of the structure of a magnetic spherical catalyst carrier prepared by the preparation method of an embodiment of the present invention.

[0032] The figure includes: a magnetic spherical catalyst carrier 1, a magnetic core 10, a first wrapping layer 11, and a second wrapping layer 12. DETAILED DESCRIPTION

[0033] The technical solution of the present invention is described in detail below with reference to the accompanying drawings.

[0034] The present invention provides a method for preparing a magnetic spherical catalyst carrier, comprising the following steps:

[0035] Step 10, adding magnetic particles, a first precursor powder and a first growth solution into a disc granulator, and rolling the disc granulator to make the first precursor powder grow on the surface of the magnetic particles to obtain single-layer coated particles.

[0036] Step 20, adding the single-layer coated particles, the second precursor powder and the second growth solution into the disc granulator, rolling the disc granulator to make the second precursor powder grow on the surface of the single-layer coated particles to obtain double-layer coated particles.

[0037] Step 30, calcining the double-layer coated particles in an inert or reducing gas atmosphere, and obtaining a calcined product after cooling.

[0038] Step 40, screening out the magnetic spherical catalyst carrier from the calcined product. Specifically, the magnetic spherical catalyst carrier can be sucked out from the calcined product using a magnet.

[0039] like Figure 1 As shown, the magnetic spherical catalyst carrier 1 includes a magnetic core 10 , a first wrapping layer 11 covering the magnetic core 10 , and a second wrapping layer 12 covering the first wrapping layer 11 .

[0040] The magnetic particles include at least one of elemental iron particles, γ-phase ferric oxide particles, and ferroferric oxide particles. Preferably, the average particle size D of the magnetic particles is 50 20 to 300 μm. Magnetic particles can be obtained by the following methods: (1) directly purchasing and using particles with a narrow particle size distribution; (2) further size screening the purchased particles; (3) grinding large particles and then further size screening; (4) synthesizing by chemical methods (such as sol-gel method). In this embodiment, method (2) is preferably used because commercially available iron powder and ferroferric oxide powder are available in various size ranges at low prices, and simple physical screening can further improve the particle size uniformity of the magnetic particles. Particle size uniformity is often characterized by the particle size distribution span (PDS), which is defined as (D 90 -D 10 ) / D 50 The smaller the value, the higher the uniformity of the particle size, where D is the particle diameter and the subscript number indicates the percentage of particles smaller than this diameter, calculated by volume fraction. 50 It represents the particle size when the volume of particles smaller than this particle size accounts for 50% in the particle distribution, and is often called the average particle size. 50 For example, for magnetic particles with a narrow particle size distribution of 50μm, it is only necessary to re-screen the purchased 200 to 400 mesh ferroferric oxide powder (250 mesh and 325 mesh sieves), and retain the particles larger than 325 mesh and smaller than 250 mesh. The actual D 50 = 49μm, PDS = 14%.

[0041] The first precursor powder includes at least one of aluminum hydroxide, pseudo-boehmite, boehmite, anhydrous alumina, and bauxite, and the first encapsulation layer 11 formed after calcination is an aluminum oxide layer. Alternatively, the first precursor powder includes at least one of silicon oxide powder, silicon oxide aerogel, and silicon oxide sol, and the first encapsulation layer 11 formed after calcination is a silicon oxide layer. Preferably, the first precursor powder includes at least one of aluminum oxide, pseudo-boehmite, and aluminum hydroxide. On the one hand, the first encapsulation layer 11 formed after calcination is an aluminum oxide layer, and the aluminum oxide layer has a low porosity and a high degree of density, so it has a good protective effect on the magnetic core and does not affect the overall mechanical strength. On the other hand, the price of aluminum oxide, pseudo-boehmite, and aluminum hydroxide is low, which is conducive to improving the economy of the catalyst. The second precursor powder includes at least one of aluminum hydroxide, pseudo-boehmite, boehmite, anhydrous alumina, and bauxite, or at least one of silicon oxide powder, silicon oxide aerogel, and silicon oxide sol. The components of the second precursor powder and the first precursor powder may be the same or different.

[0042] The first growth solution includes a binder, and the binder includes at least one of water, ethanol solution, and methanol solution; or, the binder includes at least one of ether, acetone, pyridine, tetrahydrofuran, chloroform, benzene, toluene, hexane, cyclohexane, and acetonitrile. Usually, water, ethanol solution, and methanol solution are more widely used because of low cost, low pollution, and good bonding effect, among which water is the best choice. The first growth solution also includes an auxiliary agent, and the auxiliary agent includes at least one of nitric acid, hydrochloric acid, acetic acid, formic acid, starch, dextrin, polyvinyl alcohol, and polyethyleneimine. The mass ratio of the auxiliary agent to the binder is 0.01 to 0.25:1. The second growth solution includes a binder, and the binder includes at least one of water, ethanol solution, and methanol solution; or, the binder includes at least one of ether, acetone, pyridine, tetrahydrofuran, chloroform, benzene, toluene, hexane, cyclohexane, and acetonitrile. Usually, water, ethanol solution, and methanol solution are more widely used because of low cost, low pollution, and good bonding effect, among which water is the best choice. The first growth solution also includes an additive, which includes at least one of nitric acid, hydrochloric acid, acetic acid, formic acid, starch, dextrin, polyvinyl alcohol, and polyethyleneimine. The mass ratio of the additive to the binder is 0.01 to 0.25:1. The main function of the additive is to enhance the affinity between particles and powders, and between powders. The additive can be selected according to the composition of the precursor powder. For example, if the first precursor powder and the second precursor powder are both pseudo-boehmite, when the second precursor powder grows on a single layer of coated particles, a small amount of acid (such as nitric acid, acetic acid) in the second growth solution can enhance the interaction of pseudo-boehmite and make growth easier. During the two disc granulator growth processes, a small amount of polyvinyl alcohol or polyethyleneimine can act as a bonding glue, making it easier for particles and powders, and powders to bond together. The components of the second growth solution and the first growth solution may be the same or different. The mass ratio of the first growth solution to the first precursor powder may be equal to or different from the mass ratio of the second growth solution to the second precursor powder.

[0043] The method of the present invention is based on a rolling forming method, and uses magnetic particles as growth nuclei. Under the auxiliary action of a growth solution, the precursor powder is adsorbed to coat and grow on the magnetic particles. By selecting magnetic particles of different particle sizes, spherical particles of different particle sizes can be grown to form magnetic spherical catalyst carriers of different particle sizes, and the particle size range of the prepared magnetic spherical catalyst carrier is large. By selecting magnetic particles with a particle size of 20 to 300 μm and selecting an appropriate mass ratio of magnetic particles to precursor powder, a magnetic spherical catalyst carrier with a particle size of 300 to 4000 μm can be prepared for industrial-grade catalysis, and has high particle size uniformity and a small particle size distribution span.

[0044] The method of the invention is based on a rolling forming method, using a particle size of as a growth nucleus, and with the assistance of a growth solution, adsorbing precursor powder to coat and grow on magnetic particles to obtain a magnetic spherical catalyst carrier with a particle size of 300 to 4000 μm.

[0045] The method of the present invention uses magnetic particles as growth cores, first allowing the first precursor powder to grow on the magnetic particles to obtain single-layer coated particles, and then allowing the second precursor powder to grow on the single-layer coated particles to obtain double-layer coated particles, and then forming a multilayer structure after calcining in an inert gas atmosphere. After calcining, the second precursor powder forms a second outermost coating layer, which serves as a catalyst carrier layer for loading the catalyst. After calcining, the first precursor powder forms a first coating layer between the magnetic core and the second coating layer, which serves as a protective layer for isolating the magnetic core to prevent the magnetic core from directly contacting the reactant and causing the magnetism to be broken or affecting the catalytic reaction. The inert gas is calcined to protect the magnetic core, especially the magnetic core composed of Fe or Fe3O4, from being over-oxidized at high temperatures.

[0046] The method of the present invention adds magnetic particles with uniform particle size as growth nuclei during rolling molding and granulation, and adopts a growth solution as an auxiliary to enhance the interaction between the precursor powder and the magnetic particles, so that the precursor powder is easier to coat and grow on the magnetic particles, while reducing the tendency of the precursor powder to self-nucleate growth, thereby obtaining a magnetic spherical catalyst carrier with high particle size uniformity and a small particle size distribution span.

[0047] The method of the present invention is based on the rolling molding method, which uses a small amount of cheap raw materials and has low energy consumption; the output of a single batch can be increased by simply using a larger disc granulator, which can reach tens or even hundreds of kilograms at a time, and a single rolling molding does not exceed one hour at most, which consumes less time, so the production cost per ton is low. Compared with the method of the present invention, the spray fluidization method has a complex process, requires multiple rounds of growth, and has a long preparation cycle (a single batch requires several hours, and multiple rounds of growth are required to reach the target size), and the energy consumption of evaporating solvent is high, and the loss of raw materials is significant, resulting in high production costs. The oil (ammonia) column molding method and the water phase molding method have high energy consumption, slow curing speed, low efficiency, and high overall production cost. The spray drying method not only cannot obtain a catalyst carrier in the range of 300 to 4000 μm, but also has a low single batch output (the spray process requires several hours to obtain tens of kilograms of product), and the energy cost caused by evaporating solvent is also significant.

[0048] The magnetic spherical catalyst carrier obtained by the method of the present invention can be used in catalytic reactions that use induction heating to provide heat. The magnetic catalyst is obtained by loading catalytically active substances such as Pd, Ni, and Fe on the magnetic catalyst carrier, and the magnetic catalyst is placed in an alternating magnetic field of 50 to 1000 kHz, so that the temperature of the catalyst surface can reach 500 to 1000 kHz. oC high temperature, triggering and maintaining Pd, Ni, Fe and other catalytic active substances catalyzing carbon-carbon coupling, hydrocarbon hydrogenation, hydrocarbon dehydrogenation, hydrocarbon reforming and other catalytic reactions; during the reaction process, the catalyst surface can be maintained at the required temperature, and the catalytic reaction medium, that is, the dispersed solution of the liquid-solid multiphase catalytic reaction or the reaction gas of the gas-solid multiphase catalytic reaction, has a medium temperature that is always equal to or less than the catalyst surface temperature; in this way, the catalytic reactor temperature occurring on the catalyst surface Pd, Ni, Fe and other catalytic active substances is always maintained at the most suitable reaction temperature, and the medium temperature will not be higher than the most suitable reaction temperature, thereby reducing the possibility of side reactions.

[0049] Preferably, the average particle size D of the first precursor powder is 50 The particle size of the alumina, pseudo-boehmite or aluminum hydroxide is less than 0.2 μm. The ultra-fine particle size of alumina and pseudo-boehmite is selected, especially the ultra-fine particle size of alumina and pseudo-boehmite, compared with the conventional raw materials (D 50 >5μm), which can greatly reduce the macropores formed by particle accumulation, reduce the porosity of the first coating layer, and strengthen the isolation and protection of the magnetic core. Experiments show that the particles (including the magnetic core and the first coating layer) obtained by using ultrafine particles of aluminum oxide as the first precursor to grow the first coating layer are only 0.01 cm 3 / g of pores, and conventional pseudo-boehmite was selected as the first precursor to grow the first coating layer to obtain particles with a pore size of 0.08 cm 3 / g hole.

[0050] Preferably, the pore volume of the first precursor powder is less than 0.3 cm 3 / g. The use of low-pore-volume first precursor powder can significantly reduce the pore volume of mesopores (2-50 nm), further reducing the porosity of the first coating layer. For example, the use of low-pore-volume pseudo-boehmite (pore volume PV = 0.28 cm 3 / g) and alumina (0.17 cm 3 / g) as the first precursor, the mesoporous volumes of the particles were 0.12 cm 3 / g and 0.10 cm 3 / g; in contrast, high pore volume pseudo-boehmite (pore volume PV = 1.01 cm 3 / g) as the raw material, the particles obtained by calcining have a mesopore volume of 0.58 cm 3 / g.

[0051] Preferably, in step 10, a sintering aid is also added to the disc granulator to increase the density of the first coating layer and reduce the porosity. For example, adding 2% titanium oxide powder or 1.5% zirconium oxide powder to the alumina powder can reduce the sintering temperature of the alumina. At the same sintering temperature (e.g., 650 °C), the sintering temperature of the alumina powder can be reduced.o C) can increase the sintering degree and reduce the porosity.

[0052] Considering that if the second precursor powder uses silicon oxide powder, silicon oxide aerogel or silicon oxide sol, the temperature for calcining to form a silicon oxide layer is only 340°C, while the first precursor powder uses aluminum oxide, pseudo-boehmite or aluminum hydroxide, the temperature for calcining to form an aluminum oxide layer is above 600°C, the calcining temperature in step 30 cannot form a dense first coating layer. As a preferred example, in step 20, before adding the single-layer coated particles to the disc granulator, the single-layer coated particles are first calcined in an inert or reducing gas atmosphere. Preferably, the calcining temperature for calcining the single-layer coated particles is 500-900°C. o C. In this embodiment, the single-layer coated particles are first calcined, and after calcination, a dense first coating layer is formed outside the magnetic core to isolate and protect the magnetic core, thereby preventing the magnetic core from contacting the reactants during the catalytic reaction, participating in the reaction, and affecting the catalytic effect. The calcination in an inert or reducing gas atmosphere is to protect the magnetic core, especially the magnetic core composed of Fe or Fe3O4, from being over-oxidized at high temperatures.

[0053] Preferably, in step 30, the calcination temperature of the double-layer coated particles is 300 to 700 o C.

[0054] As a preferred example, the ratio of the particle size of the magnetic particles to the target thickness of the first coating layer is 1:0.5 to 3. The first coating layer should not be too thin, otherwise it will not provide sufficient protection for the magnetic core. However, the first coating layer should not be too thick, otherwise it will easily form a large number of carrier particles that do not contain the magnetic core, and also limit the thickness that can be achieved by the second coating layer with high catalytic activity, affecting the catalytic efficiency.

[0055] As a preferred example, in step 10, the mass of the first precursor powder to be added is obtained using formula (1) according to the mass of the added magnetic particles, the particle size of the magnetic particles and the target thickness of the first coating layer:

[0056] m 11,烧前 = m 10 ρ 11,烧后 [( L 11 + r 10 ) 3 – r 10 3 ] / (ρ 10 r 10 3 w 11,烧后) Formula (1)

[0057] In the formula, m 11,烧前 represents the mass of the first precursor powder, in grams (g); m 10 Indicates the mass of magnetic particles, unit: gram (g); ρ 11,烧后 Indicates the tap density of the first coating layer after sintering, unit: g / cm3 3 ); L 11 Indicates the target thickness of the first wrapping layer, in micrometers (μm); r 10 Indicates the radius of the magnetic particle, unit: micrometer (μm); ρ 10 Indicates the tap density of magnetic particles, unit: g / cm 3 ); w 11,烧后 It indicates the residual mass percentage of the first precursor powder after calcination.

[0058] In formula (1), ρ 11,烧后 and ρ 10 Theoretically, it should be the material density to exclude the influence of the voids in the particle stacking on the density. In practice, the target thickness of the first coating layer is similar to the actual thickness of the first coating layer, and this embodiment assumes that the density of the magnetic particles and the first precursor after sintering is similar. For example, the stacking void ratio of Fe3O4 (or Fe, γ-Fe2O3) and γ-Al2O3 powder ( V %), then ρ in formula (1) 11,烧后 / ρ 10 Approximately 11材料,烧后 / ρ 10材料 , that is [ρ 11,烧后 / (1- V % 11 )] / [ρ 10 / (1- V % 10 )]. It should be noted that if the purchased magnetic particles are of high purity, the impurity content is usually below 2%, and the water content is also below 2%. Under an inert atmosphere and with proper protection, the density and quality changes before and after calcination are not significant, so ρ 10 =ρ 10,烧前 ≈ρ 10,烧后 , m 10 = m 10,烧前 ≈ m 10,烧后 ρ 11,烧后 After the first precursor powder is calcined to a corresponding temperature (usually 500-900o C) The obtained powder is measured after manual tapping, or the first precursor powder is measured by a tap density meter. 10 It is obtained by directly measuring the tap density of magnetic particles. w 11,烧后 By comparing the mass of the first precursor powder before and after calcination, w 11,烧后 = m 11,烧后 / m 11,烧前 .

[0059] Target thickness of the second wrapping layer L 12 It is calculated by the following formula: L 12 = RL 11 - r 10 ,in R Indicates the target carrier particle size.

[0060] In step 20, the mass of the second precursor powder to be added is obtained using formula (2) according to the mass of the added single-layer coated particles, the particle size of the magnetic particles, the target thickness of the first coating layer and the target thickness of the second coating layer:

[0061] m 12,烧前 = m 10+11,烧后 ρ 12,烧后 [( L 12 + L 11 + r 10 ) 3 –( L 11 + r 10 ) 3 ] / [ρ 10+11,烧后 ( L 11 + r 10 ) 3 w 12,烧后 Formula (2)

[0062] In the formula, m 12,烧前 represents the mass of the second precursor powder, in grams (g); m 10+11,烧后 It represents the mass of the single-layer coated particles or the residual mass of the single-layer coated particles after calcination, in grams (g); ρ12,烧后 It indicates the tap density of the second precursor powder after calcination, unit: g / cm3 3 );ρ 10+11,烧后 It indicates the tap density of the single-layer coated particles after calcination, unit: g / cm3 (g / cm 3 ); L 12 Indicates the target thickness of the second wrapping layer, unit: micrometer (μm); w 12,烧后 It represents the residual mass percentage of the second precursor powder after calcination.

[0063] If the single-layer coated particles are calcined and then added to the disc granulator, m 10+11,烧后 Take the actual added mass. If the single-layer coated particles are added to the disc granulator without being roasted, m 10+11,烧后 Take the residual mass after roasting of the added amount. For example, if the single-layer coated particles are added to the disc granulator without roasting, and it is planned to add 50g, and it is measured that the residual mass of each 50g of single-layer coated particles after roasting is 40g, then m 10+11,烧后 Take 40g. 12,烧后 By calcining the second precursor powder to a corresponding temperature (300-700 o C) and measure the tap density of the powder obtained. 10+11,烧后 By calcining the single-layer coated particles to the corresponding temperature (500-900 o C) and then directly measure the tap density. w 12,烧后 By comparing the mass of the second precursor powder before and after calcination, w 12,烧后 = m 12,烧后 / m 12,烧前 .

[0064] In the embodiment of the present invention, magnetic particles of appropriate particle size are first selected according to the target particle size of the carrier particles; the target thickness of the first coating layer is determined according to the ratio of the particle size of the magnetic particles to the target thickness of the first coating layer, and then the target thickness of the second coating layer is determined; then, according to the relationship between the mass of the magnetic particles-the particle size of the magnetic particles-the target thickness of the first coating layer-the mass of the first precursor powder as shown in the established formula (1), the mass of the first precursor powder to be added is determined according to the mass of the added magnetic particles, the particle size of the magnetic particles and the target thickness of the first coating layer; then, according to the relationship between the mass of the single-layer coated particles-the particle size of the magnetic particles-the target thickness of the first coating layer-the target thickness of the second coating layer-the mass of the second precursor powder as shown in the established formula (2), the mass of the second precursor powder to be added is determined according to the mass of the single-layer coated particles, the particle size of the magnetic particles, the target thickness of the first coating layer and the target thickness of the second coating layer, thereby controlling the size of the product and improving the controllability of the particle size.

[0065] Eight examples are provided below to verify the performance of the magnetic spherical catalyst carrier prepared by the method of the embodiments of the present invention.

[0066] Example 1 (Target particle size of magnetic spherical catalyst carrier 350 μm)

[0067] The magnetic particles are Fe3O4 powder with an average particle size of D 50 The particle size of Fe3O4 is 49 μm, the PDS is 14%, and the mass is 23.1 g. The magnetic properties of Fe3O4 were tested under a vibrating sample magnetometer (MPMS-SQUID, VSM-094, the same below), and the magnetization intensity was 73.5 emu / g, and there was no hysteresis in the magnetic field range of ±20000 Oe, indicating that Fe3O4 has good superparamagnetism. The first precursor powder is pseudo-boehmite with an average particle size of D 50 The pore volume PV is 0.28 cm 3 / g; the second precursor powder is pseudo-boehmite, with an average particle size of D 50 The pore volume PV is 1.01 cm 3 / g.

[0068] According to the particle size of the magnetic particles, the target thickness of the first coating layer is determined to be 50 μm, and the target thickness of the second coating layer is 100 μm. According to the mass of the added magnetic particles, the particle size of the magnetic particles and the target thickness of the first coating layer, the mass of the first precursor powder to be added is determined to be 319 g. According to the mass of the added single-layer coated particles, the particle size of the magnetic particles, the target thickness of the first coating layer and the target thickness of the second coating layer, the mass of the second precursor powder to be added is determined to be 217 g.

[0069] Add 319 g of ultrafine pseudo-boehmite powder into the disc granulator and turn on the disc. 50 23.1 g of Fe3O4 powder with a diameter of 49 μm and a PDS content of 14% was added with 20 g of an aqueous solution containing 0.4% polyvinyl alcohol by mass. After ultrasonic treatment for 3 minutes, the suspension was dripped into a disc granulator. Subsequently, 118 g of water was gradually sprayed in. After all the powders were bonded into balls, the granulator was stopped. The single-layer coated particles were tested using a particle size distribution meter to obtain the particle size D 50 = 158 μm.

[0070] Add 217 g of conventional pseudo-boehmite powder into the disc granulator and start the disc to rotate. Take 40 g of single-layer coated particles as the growth nucleus for the second round of growth, and then evenly spray 25 g of an aqueous solution containing 0.4% mass fraction of polyvinyl alcohol on the small balls, and then slowly add them to the disc granulator. Subsequently, 178 g of water is gradually sprayed in, and the granulator is stopped after all the powders are bonded into balls. The obtained spherical particles are dried in an oven at 120°C, and then calcined at 650°C for 4 hours under nitrogen protection to obtain the calcined product. Use a magnet to absorb the magnetic particles, remove the non-magnetic particles (accounting for 2.7% by mass), and obtain the final product. The final product is tested using a particle size distribution meter to obtain the particle size D 50 = 344μm, PDS = 38%, D 50 The deviation is (D 50实际 -D 50目标 ) / D 50目标 = (344-350) / 350 = -2%.

[0071] The magnetic properties of the carrier product were tested using a vibrating sample magnetometer, and the overall magnetization intensity was 1.08emu / g. The magnetization intensity calculated based on the mass of the magnetic core was 70.6 emu / g-magnetic core (magnetization intensity change of the magnetic core was -4%), and there was no hysteresis within the magnetic field range of ±20000 Oe, indicating that the first wrapping layer had a perfect protective effect on the magnetic core and retained good superparamagnetism after inert gas calcination.

[0072] Example 2 (Target particle size of magnetic spherical catalyst carrier 500 μm)

[0073] The magnetic particles are Fe3O4 powder with an average particle size of D 50 The particle size of Fe3O4 is 98 μm, the PDS is 16%, and the mass is 150 g. The magnetic properties of Fe3O4 were tested under a vibrating sample magnetometer, and the magnetization intensity was 71.8 emu / g, and there was no hysteresis in the magnetic field range of ±20000 Oe, indicating that Fe3O4 has good superparamagnetism. The first precursor powder is alumina with an average particle size of D 50The pore volume PV is 0.17 cm 3 / g; the second precursor powder is silicon oxide, with an average particle size of D 50 The pore volume PV is 0.77 cm 3 / g.

[0074] According to the particle size of the magnetic particles, the target thickness of the first coating layer is determined to be 50 μm, and the target thickness of the second coating layer is determined to be 150 μm. According to the mass of the added magnetic particles, the particle size of the magnetic particles and the target thickness of the first coating layer, the mass of the first precursor powder to be added is determined to be 438 g. According to the mass of the added single-layer coated particles, the particle size of the magnetic particles, the target thickness of the first coating layer and the target thickness of the second coating layer, the mass of the second precursor powder to be added is determined to be 385 g.

[0075] Add 438 g of ultrafine γ-alumina powder into the disc granulator and turn on the disc. 50 150g of Fe3O4 powder with a diameter of 98μm and a PDS content of 16% was added with 80g of an aqueous solution containing 0.4% polyvinyl alcohol by mass, and ultrasonicated for 3 minutes. The suspension was then dripped into a disc granulator. Subsequently, 42g of water was gradually sprayed in. After all the powders were bonded into balls, the granulator was stopped. The single-layer coated particles were tested using a particle size distribution meter to obtain the particle size D 50 = 212 μm.

[0076] Add 150 g of SiO2 powder to the disc granulator and start the disc rotation. Take 40 g of the first calcined product pellets as the growth nuclei for the second round of growth. After evenly spraying 5 g of an aqueous solution containing 0.4% by mass fraction of polyvinyl alcohol on the pellets, slowly add them to the disc granulator. Subsequently, 127 g of water is gradually sprayed in, and the granulator is stopped after all the powders are bonded into balls. After drying the obtained spherical particles in an oven at 120°C, they are calcined at 600°C for 4 hours under nitrogen protection to obtain a calcined product. Use a magnet to absorb the magnetic particles, remove the non-magnetic particles (4.1% by mass), and obtain the final product. The final product is tested using a particle size distribution meter to obtain the particle size D 50 = 515μm, PDS = 26%, D 50 The deviation is (D 50实际 -D 50目标 ) / D 50目标 = (515-500) / 500 = +3%.

[0077] The magnetic properties of the carrier product were tested using a vibrating sample magnetometer, and the overall magnetization intensity was 5.66emu / g. The magnetization intensity calculated based on the mass of the magnetic core was 70.0 emu / g-magnetic core (magnetization intensity change of the magnetic core was -5.3%), and there was no hysteresis within the magnetic field range of ±20000 Oe, indicating that the first wrapping layer had a perfect protective effect on the magnetic core and retained good superparamagnetism after inert gas calcination.

[0078] Example 3 (Target particle size of magnetic spherical catalyst carrier 1000 μm)

[0079] The magnetic particles are Fe3O4 powder with an average particle size of D 50 The first precursor powder is pseudo-boehmite with an average particle size of D 50 The pore volume PV is 0.28 cm 3 / g; the second precursor powder is TiO2, with an average particle size of D 50 The pore volume is 3.5 μm and the pore volume PV is 0.38 cm 3 / g.

[0080] According to the particle size of the magnetic particles, the target thickness of the first coating layer is determined to be 100 μm, and the target thickness of the second coating layer is determined to be 300 μm. According to the mass of the added magnetic particles, the particle size of the magnetic particles and the target thickness of the first coating layer, the mass of the first precursor powder to be added is determined to be 178 g. According to the mass of the added single-layer coated particles, the particle size of the magnetic particles, the target thickness of the first coating layer and the target thickness of the second coating layer, the mass of the second precursor powder to be added is determined to be 508 g.

[0081] Add 178 g of ultrafine pseudo-boehmite powder into the disc granulator and turn on the disc. 50 50g of Fe3O4 powder with a diameter of 205μm and a PDS content of 16% was added with 30g of an aqueous solution containing 0.4% polyvinyl alcohol by mass, and ultrasonicated for 3 minutes. The suspension was then dripped into a disc granulator. Subsequently, 65g of water was gradually sprayed in, and the granulator was stopped after all the powders were bonded into balls. The obtained spherical particles were dried in an oven at 120℃, and then calcined at 600℃ for 4 hours under nitrogen protection to obtain the first calcined product. The first calcined product was tested using a particle size distribution measuring instrument to obtain the particle size D 50 = 388 μm.

[0082] Add 531g TiO2 powder into the disc granulator and start the disc to rotate. Take 40g of the first calcined product pellets as the growth nuclei for the second round of growth. After evenly spraying 5g of an aqueous solution containing 0.5% mass fraction of polyethyleneimine on the pellets, slowly add them to the disc granulator. Subsequently, 247g of water is gradually sprayed in, and the granulator is stopped after all the powders are bonded into balls. After drying the obtained spherical particles in an oven at 120°C, they are calcined at 340°C for 4 hours under nitrogen protection to obtain a secondary calcination product. Use a magnet to absorb the magnetic particles, remove the non-magnetic particles (0.9% by mass), and obtain the final product. The final product is tested using a particle size distribution meter to obtain the particle size D 50 = 1032μm, PDS = 21%, D 50 The deviation is (D 50实际 -D 50目标 ) / D 50目标 = (1043-1000) / 1000 = +4%.

[0083] Example 4 (the target particle size of the magnetic spherical catalyst carrier is 300 μm, and the magnetic core particle size is selected to be about 20 μm)

[0084] The magnetic particles are Fe3O4 powder. The average particle size D of the initial raw material Fe3O4 50 The particle size of the powder was 18.4 μm and the PDS was 37%. The 800-mesh sieve was used as the top sieve and the 2000-mesh sieve was used as the bottom sieve to obtain a powder with a particle size between 800 and 2000 mesh. The powder was used as the magnetic core and the average particle size D of the powder was measured at the same time. 50 The first precursor powder is pseudo-boehmite with an average particle size of D 50 The pore volume PV is 0.28 cm 3 / g; the second precursor powder is pseudo-boehmite, with an average particle size of D 50 The pore volume PV is 1.01 cm 3 / g.

[0085] According to the particle size of the magnetic particles, the target thickness of the first coating layer is determined to be 30 μm, and the target thickness of the second coating layer is determined to be 110 μm. According to the mass of the added magnetic particles, the particle size of the magnetic particles and the target thickness of the first coating layer, the mass of the first precursor powder to be added is determined to be 321 g. According to the mass of the added single-layer coated particles, the particle size of the magnetic particles, the target thickness of the first coating layer, and the target thickness of the second coating layer, the mass of the second precursor powder to be added is determined to be 557 g.

[0086] Add 321 g of ultrafine pseudo-boehmite powder into the disc granulator and turn on the disc.50 10 g of Fe3O4 powder with a diameter of 22.4 μm and a PDS content of 24% was added with 8 g of an aqueous solution containing 0.4% polyvinyl alcohol by mass. After ultrasonic treatment for 3 minutes, the suspension was dripped into a disc granulator. Subsequently, 115 g of water was gradually sprayed in. After all the powders were bonded into balls, the granulator was stopped. The single-layer coated particles were tested using a particle size distribution meter to obtain the particle size D 50 = 91 μm.

[0087] Add 557 g of conventional pseudo-boehmite powder into the disc granulator and start the disc to rotate. Take 40 g of single-layer coated particles as the growth nucleus for the second round of growth, and then evenly spray 25 g of an aqueous solution containing 0.4% mass fraction of polyvinyl alcohol on the small balls, and then slowly add it to the disc granulator. Subsequently, 103 g of water is gradually sprayed in, and the granulator is stopped after all the powders are bonded into balls. The obtained spherical particles are dried in an oven at 120°C, and then calcined at 650°C for 4 hours under nitrogen protection to obtain the calcined product. Use a magnet to absorb the magnetic particles, remove the non-magnetic particles (6.7% by mass), and obtain the final product. The final product is tested using a particle size distribution meter to obtain the particle size D 50 = 312 μm, PDS = 42%, D 50 The deviation is (D 50实际 -D 50目标 ) / D 50目标 = (312-300) / 300 = +4%.

[0088] Example 5 (the target particle size of the magnetic spherical catalyst carrier is 4000 μm, and the magnetic core particle size is selected to be about 300 μm)

[0089] The magnetic particles are Fe3O4 powder. The average particle size D of the initial raw material Fe3O4 50 The first precursor powder is pseudo-boehmite with an average particle size of D 50 The pore volume PV is 0.28 cm 3 / g; the second precursor powder is pseudo-boehmite, with an average particle size of D 50 The pore volume PV is 1.01 cm 3 / g.

[0090] According to the particle size of the magnetic particles, the target thickness of the first coating layer is determined to be 350 μm, and the target thickness of the second coating layer is determined to be 1500 μm. According to the mass of the added magnetic particles, the particle size of the magnetic particles and the target thickness of the first coating layer, the mass of the first precursor powder to be added is determined to be 367 g. According to the mass of the added single-layer coated particles, the particle size of the magnetic particles, the target thickness of the first coating layer and the target thickness of the second coating layer, the mass of the second precursor powder to be added is determined to be 603 g.

[0091] Add 367 g of ultrafine pseudo-boehmite powder to the disc granulator and turn on the disc. Add 16 g of aqueous solution containing 0.4% mass fraction of polyvinyl alcohol to 20 g of powder, and add the suspension dropwise into the disc granulator after ultrasonic treatment for 3 minutes. Then gradually spray 147 g of water, and stop the granulator after all the powders are bonded into balls. Use a particle size distribution meter to test the single-layer coated particles and obtain the particle size D 50 = 1088 μm.

[0092] Add 603 g of conventional pseudo-boehmite powder into the disc granulator and start the disc to rotate. Take 20 g of single-layer coated particles as the growth nucleus for the second round of growth, and then evenly spray 15 g of an aqueous solution containing 0.4% mass fraction of polyvinyl alcohol on the small balls, and then slowly add it to the disc granulator. Subsequently, 486 g of water is gradually sprayed in, and the granulator is stopped after all the powders are bonded into balls. The obtained spherical particles are dried in an oven at 120°C, and then calcined at 650°C for 4 hours under nitrogen protection to obtain the calcined product. Use a magnet to absorb the magnetic particles, remove the non-magnetic particles (1.3% by mass), and obtain the final product. The final product is tested using a particle size distribution meter to obtain the particle size D 50 = 3923 μm, PDS = 15%, D 50 The deviation is (D 50实际 -D 50目标 ) / D 50目标 = (3923-4000) / = -2%.

[0093] Example 6 (Target particle size of magnetic spherical catalyst carrier 350 μm)

[0094] The magnetic particles are Fe3O4 powder with an average particle size of D 50 The particle size of Fe3O4 is 49 μm, the PDS is 14%, and the mass is 23.1 g. The magnetic properties of Fe3O4 were tested under a vibrating sample magnetometer, and the magnetization intensity was 73.5 emu / g, and there was no hysteresis in the magnetic field range of ±20000 Oe, indicating that Fe3O4 has good superparamagnetism. The first precursor powder is a conventional particle size pseudo-boehmite with an average particle size of D 50The pore volume PV is 1.01 cm 3 / g; The second precursor powder uses conventional particle size pseudo-boehmite, with an average particle size of D 50 The pore volume PV is 1.01 cm 3 / g.

[0095] According to the particle size of the magnetic particles, the target thickness of the first coating layer is determined to be 50 μm, and the target thickness of the second coating layer is 100 μm. According to the mass of the added magnetic particles, the particle size of the magnetic particles and the target thickness of the first coating layer, the mass of the first precursor powder to be added is determined to be 262 g. According to the mass of the added single-layer coated particles, the particle size of the magnetic particles, the target thickness of the first coating layer and the target thickness of the second coating layer, the mass of the second precursor powder to be added is determined to be 282 g.

[0096] Add 262 g of conventional pseudo-boehmite powder into the disc granulator and turn on the disc. 50 50 g of Fe3O4 powder with a diameter of 49 μm and a PDS content of 14% was added with 35 g of an aqueous solution containing 0.4% polyvinyl alcohol by mass. After ultrasonic treatment for 3 minutes, the suspension was dripped into a disc granulator. Subsequently, 202 g of water was gradually sprayed in. After all the powders were bonded into balls, the granulator was stopped. The single-layer coated particles were tested using a particle size distribution meter to obtain the particle size D 50 = 173 μm.

[0097] Add 282 g of conventional pseudo-boehmite powder into the disc granulator and start the disc to rotate. Take 40 g of single-layer coated particles as the growth nucleus for the second round of growth, and then evenly spray 6 g of an aqueous solution containing 0.4% mass fraction of polyvinyl alcohol on the small balls, and then slowly add it to the disc granulator. Subsequently, 214 g of water is gradually sprayed in, and the granulator is stopped after all the powders are bonded into balls. The obtained spherical particles are dried in an oven at 120°C, and then calcined at 650°C for 4 hours under nitrogen protection to obtain the calcined product. Use a magnet to absorb the magnetic particles, remove the non-magnetic particles (8.7% by mass), and obtain the final product. The final product is tested using a particle size distribution meter to obtain the particle size D 50 = 362 μm, PDS = 31%, D 50 The deviation is (D 50实际 -D 50目标 ) / D 50目标 = (362-350) / 350 = +4%.

[0098] The magnetic properties of the carrier product were tested using a vibrating sample magnetometer, and the overall magnetization intensity was 1.29emu / g. The magnetization intensity calculated based on the magnetic core mass was 46.4 emu / g-magnetic core (magnetization intensity change of the magnetic core was -37%), and there was significant hysteresis within the magnetic field range of ±20000 Oe, indicating that the superparamagnetism of the core was significantly lost after calcination in an inert gas atmosphere due to the weak protection of the first wrapping layer on the magnetic core.

[0099] Example 7 (Target particle size of magnetic spherical catalyst carrier 350 μm)

[0100] The magnetic particles are Fe3O4 powder with an average particle size of D 50 The particle size of Fe3O4 is 49 μm, the PDS is 14%, and the mass is 23.1 g. The magnetic properties of Fe3O4 were tested under a vibrating sample magnetometer, and the magnetization intensity was 73.5 emu / g, and there was no hysteresis in the magnetic field range of ±20000 Oe, indicating that Fe3O4 has good superparamagnetism. The first precursor powder is pseudo-boehmite with an average particle size of D 50 The pore volume PV is 0.28 cm 3 / g; the second precursor powder is pseudo-boehmite, with an average particle size of D 50 The pore volume PV is 1.01 cm 3 / g.

[0101] According to the particle size of the magnetic particles, the target thickness of the first coating layer is determined to be 20 μm, and the target thickness of the second coating layer is 100 μm. According to the mass of the added magnetic particles, the particle size of the magnetic particles and the target thickness of the first coating layer, the mass of the first precursor powder to be added is determined to be 254 g. According to the mass of the added single-layer coated particles, the particle size of the magnetic particles, the target thickness of the first coating layer and the target thickness of the second coating layer, the mass of the second precursor powder to be added is determined to be 549 g.

[0102] Add 254 g of ultrafine pseudo-boehmite powder into the disc granulator and turn on the disc. 50 150 g of Fe3O4 powder with a diameter of 49 μm and a PDS content of 14% was added with 120 g of an aqueous solution containing 0.4% polyvinyl alcohol by mass. After ultrasonic treatment for 3 minutes, the suspension was dripped into a disc granulator. Subsequently, 95 g of water was gradually sprayed in. After all the powders were bonded into balls, the granulator was stopped. The single-layer coated particles were tested using a particle size distribution meter to obtain the particle size D 50 = 97 μm.

[0103] Add 549 g of conventional pseudo-boehmite powder into the disc granulator and start the disc to rotate. Take 40 g of single-layer coated particles as the growth nucleus for the second round of growth, and then evenly spray 25 g of an aqueous solution containing 0.4% mass fraction of polyvinyl alcohol on the small balls, and then slowly add them to the disc granulator. Subsequently, 450 g of water is gradually sprayed in, and the granulator is stopped after all the powders are bonded into balls. The obtained spherical particles are dried in an oven at 120°C, and then calcined at 650°C for 4 hours under nitrogen protection to obtain the calcined product. Use a magnet to absorb the magnetic particles, remove the non-magnetic particles (3.1% by mass), and obtain the final product. The final product is tested using a particle size distribution meter to obtain the particle size D 50 = 351 μm, PDS = 36%, D 50 The deviation is (D 50实际 -D 50目标 ) / D 50目标 = (351-350) / 350 = +0.3%.

[0104] The magnetic properties of the carrier product were tested using a vibrating sample magnetometer, and the overall magnetization intensity was 1.92emu / g. The magnetization intensity calculated based on the mass of the magnetic core was 61.3 emu / g-magnetic core (magnetization intensity change of the magnetic core was -17%), and there was hysteresis within the magnetic field range of ±20000 Oe, indicating that due to the insufficient thickness of the first wrapping layer, its protective effect on the magnetic core was weak, and the superparamagnetism of the core was lost to a certain extent after calcination in an inert gas atmosphere.

[0105] Example 8 (Target particle size of magnetic spherical catalyst carrier is 4000 μm, and magnetic core particle size is selected to be about 300 μm)

[0106] The magnetic particles are Fe3O4 powder. The average particle size D of the initial raw material Fe3O4 50 The magnetic properties of Fe3O4 were tested under a vibrating sample magnetometer, and the magnetization intensity was 67.3 emu / g, and there was no hysteresis in the magnetic field range of ±20000 Oe, indicating that Fe3O4 has good superparamagnetism. The first precursor powder was pseudo-boehmite with an average particle size of D 50 The pore volume PV is 0.28 cm 3 / g; the second precursor powder is pseudo-boehmite, with an average particle size of D 50 The pore volume PV is 1.01 cm 3 / g.

[0107] According to the particle size of the magnetic particles, the target thickness of the first coating layer is determined to be 1000 μm, and the target thickness of the second coating layer is determined to be 850 μm. According to the mass of the added magnetic particles, the particle size of the magnetic particles and the target thickness of the first coating layer, the mass of the first precursor powder to be added is determined to be 1146 g. According to the mass of the added single-layer coated particles, the particle size of the magnetic particles, the target thickness of the first coating layer and the target thickness of the second coating layer, the mass of the second precursor powder to be added is determined to be 228 g.

[0108] Add 1146 g of ultrafine pseudo-boehmite powder to the disc granulator and turn on the disc. Add 8 g of aqueous solution containing 0.4% mass fraction of polyvinyl alcohol to 10 g of Fe3O4 powder, and add the suspension dropwise into the disc granulator after ultrasonic treatment for 3 minutes. Then gradually spray 503 g of water, and stop the granulator after all the powders are bonded into balls. Use a particle size distribution meter to test the single-layer coated particles and obtain the particle size D 50 = 2505 μm.

[0109] Add 850 g of conventional pseudo-boehmite powder into the disc granulator and start the disc to rotate. Take 100 g of single-layer coated particles as the growth nucleus for the second round of growth, and then evenly spray 75 g of an aqueous solution containing 0.4% mass fraction of polyvinyl alcohol on the small balls, and then slowly add it to the disc granulator. Subsequently, 636 g of water is gradually sprayed in, and the granulator is stopped after all the powders are bonded into balls. The obtained spherical particles are dried in a 120°C oven and calcined at 650°C for 4 hours under nitrogen protection to obtain the calcined product. Use a magnet to absorb the magnetic particles, remove the non-magnetic particles (accounting for 21.7% by mass), and obtain the final product. The final product is tested using a particle size distribution meter to obtain the particle size D 50 = 3923 μm, PDS = 15%, D 50 The deviation is (D 50实际 -D 50目标 ) / D 50目标 = (3923-4000) / = -2%.

[0110] As can be seen from Examples 1 to 8, the method of the present invention can be used to prepare submillimeter and millimeter-level magnetic particles, and the magnetic core, the first encapsulation layer and the second encapsulation layer can have different components and different crystal phases. The thickness and particle size of the first encapsulation layer and the second encapsulation layer can also be adjusted within a large range. From the comparison between Example 1 and Example 6, it can be seen that since the first encapsulation layer in Example 6 is obtained using conventional pseudo-boehmite as a raw material, its protective effect on the magnetic core is weak, the proportion of non-magnetic particles in the product is significantly higher than that in Example 1, and the paramagnetism has a significant loss. From the comparison between Example 1 and Example 7, it can be seen that if the thickness of the first encapsulation layer is insufficient, its protective effect on the magnetic core is weak, and the superparamagnetism of the core after calcination in an inert gas atmosphere has a certain loss. From Example 8, it can be seen that if the thickness of the first encapsulation layer is too large, the proportion of the raw material of the first encapsulation layer is too large, and it is easy to form a ball by itself during growth rather than being wrapped on the magnetic core, resulting in a significantly higher proportion of non-magnetic particles in the product than in other embodiments.

[0111] The performance of the product in the embodiment is verified below.

[0112] 1. The products of Example 1, Example 2, Example 6 and Example 8 were respectively used for catalyst loading and the magnetic properties were tested.

[0113] Test 1: 2.11 g of palladium acetate was dissolved in 100 mL of acetone to obtain a palladium acetate solution; then, the obtained palladium acetate solution was added to a glass beaker containing 100 g of a magnetic catalyst carrier (the product of Example 1), and the mixture of the magnetic catalyst carrier and the palladium acetate solution was stirred with a glass rod for 5 minutes to fully mix the two; the obtained beaker containing the mixture of solid and liquid was placed in an oven at 30 o C for 72 hours to evaporate most of the acetone in the beaker to obtain a dried magnetic catalyst loaded with palladium acetate; the obtained magnetic catalyst loaded with palladium acetate was further heated at 700 o C in a hydrogen atmosphere (10% H2, balanced by N2) to obtain a magnetic catalyst loaded with elemental palladium.

[0114] The catalyst was tested for magnetic properties using a vibrating sample magnetometer, and the results showed that the magnetic core magnetization intensity changed by -2.1%, and there was no hysteresis within the magnetic field range of ±20,000 Oe, indicating that the first coating layer had a perfect protective effect on the magnetic core and retained good superparamagnetism after calcination in a hydrogen atmosphere.

[0115] Test 2: 31.13 g of nickel nitrate was dissolved in 100 g of water to obtain a nickel nitrate aqueous solution; then, the obtained nickel nitrate aqueous solution was added dropwise to a glass beaker containing 100 g of the magnetic catalyst carrier (the product of Example 2), and the mixture of the magnetic catalyst carrier and the nickel nitrate solution was stirred with a glass rod for 5 minutes to fully mix the two; the obtained beaker containing the mixture of solid and liquid was placed in an oven at 40 o C for 72 hours to evaporate most of the water in the beaker to obtain a dried magnetic catalyst loaded with nickel nitrate; the obtained magnetic catalyst loaded with nickel nitrate was further heated at 700 o C was calcined in a hydrogen atmosphere (10% H2, balanced by N2) to obtain a magnetic catalyst loaded with elemental nickel; the mass fraction of Ni in the magnetic catalyst was 10%.

[0116] The catalyst was tested for magnetic properties using a vibrating sample magnetometer, and the results showed that the magnetic core magnetization intensity changed by -1.8%, and there was no hysteresis within the magnetic field range of ±20,000 Oe, indicating that the first coating layer had a perfect protective effect on the magnetic core and retained good superparamagnetism after calcination in a hydrogen atmosphere.

[0117] Test 3: 31.13 g of nickel nitrate was dissolved in 100 g of water to obtain a nickel nitrate aqueous solution; then, the obtained nickel nitrate aqueous solution was added dropwise to a glass beaker containing 100 g of the catalyst carrier (the product of Example 6), and the mixture of the non-magnetic catalyst carrier and the nickel nitrate solution was stirred with a glass rod for 5 minutes to fully mix the two; the obtained beaker containing the mixture of solid and liquid was placed in an oven at 40 o C for 72 hours to evaporate most of the water in the beaker to obtain a dried non-magnetic catalyst loaded with nickel nitrate; the obtained non-magnetic catalyst loaded with nickel nitrate was further heated at 700 o C was calcined in a hydrogen atmosphere (10% H2, balanced by N2) to obtain a magnetic catalyst loaded with elemental nickel; the mass fraction of Ni in the non-magnetic catalyst was 10%.

[0118] The catalyst was tested for magnetic properties under a vibrating sample magnetometer, and the magnetic core magnetization intensity changed by -17%, and the hysteresis became wider within the magnetic field range of ±20000 Oe. Compared with test 2, it shows that due to the porous first coating layer, the protection of the magnetic core is weak, and the superparamagnetism of the magnetic core is further lost after calcination in a hydrogen atmosphere.

[0119] Test 4: 31.13 g of nickel nitrate was dissolved in 100 g of water to obtain a nickel nitrate aqueous solution; then, the obtained nickel nitrate aqueous solution was added dropwise to a glass beaker containing 100 g of the catalyst carrier (the product of Example 8), and the mixture of the non-magnetic catalyst carrier and the nickel nitrate solution was stirred with a glass rod for 5 minutes to fully mix the two; the obtained beaker containing the mixture of solid and liquid was placed in an oven at 40 o C for 72 hours to evaporate most of the water in the beaker to obtain a dried non-magnetic catalyst loaded with nickel nitrate; the obtained non-magnetic catalyst loaded with nickel nitrate was further heated at 700 o C was calcined in a hydrogen atmosphere (10% H2, balanced by N2) to obtain a magnetic catalyst loaded with elemental nickel; the mass fraction of Ni in the non-magnetic catalyst was 10%.

[0120] The magnetic properties of the catalyst were tested under a vibrating sample magnetometer. The results showed that the magnetic core magnetization intensity changed by -0.3%, and there was no hysteresis in the magnetic field range of ±20000 Oe, indicating that the first wrapping layer had a perfect protective effect on the magnetic core and retained good superparamagnetism after calcination in a hydrogen atmosphere.

[0121] 2. The products of Example 1, Example 2 and Example 8 were respectively used to test the catalytic reaction performance by induction heating under an external magnetic field.

[0122] Test 5: Using induction heating to provide heat for CO catalytic oxidation reaction.

[0123] 1 g of magnetic catalyst (the product of Example 1 was loaded in Test 1) was loaded in a fixed bed quartz tube reactor, and the fixed bed quartz tube was vertically placed in a magnetic induction coil, keeping the catalyst loading position in the middle of the upper and lower edges of the magnetic induction coil; the catalyst in the fixed bed quartz tube reactor was protected by N2, the N2 flow rate was 100 mL / min, the alternating magnetic field was turned on, the frequency was set to 800 kHz, and the power was 0.2 kW; when the catalyst bed temperature rose to 80 o C, the catalyst bed temperature was kept at 80 o C is constant, and the alternating magnetic field power is 0.11kW; the fixed bed quartz tube reactor is set at a catalyst bed temperature of 80 o After keeping at 80 °C for 10 min, the N2 protective gas was switched to a mixture of CO and air, i.e., the reaction gas. The volume ratio of CO to air was 1:1, and the reaction gas space velocity was 1000 mL / g / h. o C and flowed through the catalyst bed. After 10 hours of reaction, the concentrations of the product components were monitored by gas chromatography and the conversion rate of the reactants was calculated. The conversion rate of CO was found to be 99%.

[0124] The catalyst after the reaction was heated at 120 o C to remove the adsorbed moisture and gas molecules, and then the magnetic properties were tested under a vibrating sample magnetometer, and the magnetic nuclear magnetization intensity changed by +0.8%, and there was no hysteresis within the magnetic field range of ±20000 Oe. This indicates that after a long period of low-temperature reaction (80 o C) The magnetic properties of the nucleus are not affected.

[0125] Test 6: Using induction heating to provide heat, catalytic dry reforming of CO2 and CH4 was performed.

[0126] 1 g of magnetic catalyst (the product of Example 2 was loaded in Test 2) was loaded in a fixed bed quartz tube reactor, and the fixed bed quartz tube was vertically placed in a magnetic induction coil, keeping the catalyst loading position in the middle of the upper and lower edges of the magnetic induction coil; the catalyst in the fixed bed quartz tube reactor was protected by N2, the N2 flow rate was 100 mL / min, the alternating magnetic field was turned on, the frequency was set to 800 kHz, and the power was 3 kW; after 20 minutes, when the catalyst bed temperature rose to 650 o C, by adjusting the alternating magnetic field power, the catalyst bed temperature is kept at 650 o C is constant, and the alternating magnetic field power is 2.1 kW; the fixed bed quartz tube reactor is set at a catalyst bed temperature of 650 o After keeping at 650 °C for 10 min, the N2 protective gas was switched to a mixture of CO2 and CH4, i.e., the reaction gas. The volume ratio of CO2 to CH4 was 1:1, and the reaction gas space velocity was 300 mL / g / h. o C and flowed through the catalyst bed. After 10 hours of reaction, the concentrations of the product components were monitored by gas chromatography and the conversion rates of the reactants were calculated. The results showed that the conversion rates of CO2 and CH4 were 75% and 73%, respectively.

[0127] The catalyst after the reaction was heated at 120 o C to remove the adsorbed moisture and gas molecules, and then the magnetic properties were tested under a vibrating sample magnetometer, and the magnetic nuclear magnetization intensity changed by -0.7%, and there was no hysteresis within the magnetic field range of ±20000 Oe. This shows that even after a long high temperature reaction (650 o C), the superparamagnetism of the core is still well preserved.

[0128] Test 7: Using induction heating to provide heat, catalytic dry reforming of CO2 and CH4 was performed.

[0129] 1 g of magnetic catalyst (the product of Example 8 was loaded in Test 4) was loaded in a fixed bed quartz tube reactor, and the fixed bed quartz tube was vertically placed in a magnetic induction coil, keeping the catalyst loading position in the middle of the upper and lower edges of the magnetic induction coil; the catalyst in the fixed bed quartz tube reactor was protected by N2, the N2 flow rate was 100 mL / min, the alternating magnetic field was turned on, the frequency was set to 800 kHz, and the power was 5 kW; after 40 minutes, when the catalyst bed temperature rose to 650 o C, by adjusting the alternating magnetic field power, the catalyst bed temperature is kept at 650 o C is constant, and the alternating magnetic field power is 3.4 kW; the fixed bed quartz tube reactor is set at a catalyst bed temperature of 650 o After keeping at 650 °C for 10 min, the N2 protective gas was switched to a mixture of CO2 and CH4, i.e., the reaction gas. The volume ratio of CO2 to CH4 was 1:1, and the reaction gas space velocity was 300 mL / g / h. o C and flowed through the catalyst bed. After 10 hours of reaction, the concentrations of the product components were monitored by gas chromatography and the conversion rates of the reactants were calculated. The results showed that the conversion rates of CO2 and CH4 were 73% and 69%, respectively.

[0130] The catalyst after the reaction was heated at 120 o C to remove the adsorbed moisture and gas molecules, and then the magnetic properties were tested under a vibrating sample magnetometer, and the magnetic nuclear magnetization intensity changed by -0.4%, and there was no hysteresis in the magnetic field range of ±20000 Oe. This shows that even after a long high temperature reaction (650 o C), the superparamagnetism of the core is still well preserved. On the other hand, the magnetic field power and heating time required to reach the target temperature for the catalyst with too thick a first coating layer are significantly increased, and the conversion rates of CO2 and CH4 are also reduced, indicating that the low proportion of magnetic core particle size affects the catalytic effect.

[0131] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by a technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A method for preparing a magnetic spherical catalyst carrier, It is characterized in that The following steps are involved: Step 10, adding magnetic particles, a first precursor powder and a first growth solution into a disc granulator, and rolling the disc granulator to make the first precursor powder grow on the surface of the magnetic particles to obtain single-layer coated particles; Step 20, adding the single-layer coated particles, the second precursor powder and the second growth solution into the disc granulator, and rolling the disc granulator so that the second precursor powder grows on the surface of the single-layer coated particles to obtain double-layer coated particles; Step 30, calcining the double-layer coated particles in an inert or reducing gas atmosphere, and obtaining a calcined product after cooling; Step 40, screening out the magnetic spherical catalyst carrier from the calcined product; The magnetic spherical catalyst carrier (1) comprises a magnetic core (10), a first wrapping layer (11) wrapping the magnetic core (10), and a second wrapping layer (12) wrapping the first wrapping layer (11); In step 10, the mass of the first precursor powder to be added is obtained using formula (1) according to the mass of the added magnetic particles, the particle size of the magnetic particles and the target thickness of the first coating layer: m 11,烧前 = m 10 r 11,烧后 [( L 11 + r 10 ) 3 – r 10 3 ] / (p 10 r 10 3 w 11,烧后 ) formula (1) In the formula, m 11,烧前 represents the mass of the first precursor powder, in grams; m 10 Indicates the mass of magnetic particles, unit: gram; ρ 11,烧后 It indicates the tap density of the first coating layer after calcination, unit: g / cm3; L 11 Indicates the target thickness of the first wrapping layer, in microns; r 10 Indicates the radius of the magnetic particle, unit: micrometer; ρ 10 Indicates the tap density of magnetic particles, unit: g / cm3; w 11,烧后 It indicates the residual mass percentage of the first precursor powder after calcination.

2. The method for preparing a magnetic spherical catalyst carrier according to claim 1, It is characterized in that The particle size of the magnetic spherical catalyst carrier is 300 to 4000 μm.

3. The method for preparing a magnetic spherical catalyst carrier according to claim 1, It is characterized in that The particle size of the magnetic particles is 20 to 300 μm.

4. The method for preparing a magnetic spherical catalyst carrier according to claim 1, It is characterized in that The ratio of the particle size of the magnetic particles to the target thickness of the first coating layer is 1:0.5-3.

5. The method for preparing a magnetic spherical catalyst carrier according to claim 1, It is characterized in that The particle size of the first precursor powder is less than 0.2 μm.

6. The method for preparing a magnetic spherical catalyst carrier according to claim 1, It is characterized in that The pore volume of the first precursor powder is less than 0.3 cm 3 / g.

7. The method for preparing a magnetic spherical catalyst carrier according to claim 1, It is characterized in that In the step 20, before the single-layer coated particles are added to the disc granulator, the single-layer coated particles are first calcined in an inert or reducing gas atmosphere.

8. The method for preparing a magnetic spherical catalyst carrier according to claim 7, It is characterized in that The calcination temperature for the single-layer coated particles is 500 to 900 o C.