Micron-sized carbon nitride and its preparation method and application

The preparation of micron-scale carbon nitride with porous thin-walled structures through hydrothermal method has solved the problem of insufficient hydrogen production activity of existing carbon nitride in photocatalytic decomposition of water, and achieved the improvement of efficient photocatalytic performance and green and economical catalyst preparation .

CN118637568BActive Publication Date: 2024-12-03SHANDONG PETROCHEMICAL INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411102582.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-12-03
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

The existing carbon nitride has weak activity in the process of photocatalytic decomposition of water and hydrogen production, making it difficult to effectively utilize its internal active sites, and the method of preparing high-efficiency photocatalysts has problems of high cost and high complexity.

Method used

Rod-shaped precursors were obtained by hydrothermal method, and then calcined in argon atmosphere and thermally stripped in the air to prepare micron-scale carbon nitride with a porous thin-walled structure, which simplifies the preparation process, reduces the raw material price, and increases the catalyst specific surface area and photocatalytic properties.

Benefits of technology

It achieves efficient photocatalytic performance improvement, accelerates the transfer and separation of photogenerated charges through the porous structure, effectively exposes the active sites inside the tube, improves the photocatalytic performance of the catalyst, and provides a green, efficient metal-free photocatalyst. Preparation scheme.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118637568B_ABST
    Figure CN118637568B_ABST
Patent Text Reader

Abstract

This invention proposes a micron-sized carbon nitride, its preparation method, and its applications, belonging to the field of inorganic materials technology. The micron-sized carbon nitride has a length of 10-20 μm, a maximum cross-sectional diameter of 2-10 μm, a wall thickness of 5-30 nm, and internal hollow granular pores with a diameter of 30-150 nm and a wall thickness of 5-15 nm. The carbon nitride obtained by this invention can be composited with other semiconductor materials and its surface modified to promote interfacial charge transfer, optimize the band structure, and further improve the photocatalytic activity of the catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inorganic materials, and in particular to micron-sized carbon nitride and a preparation method and application thereof. Background Art

[0002] Carbon nitride is a metal-free organic polymer semiconductor material with inherent advantages such as low cost, simple preparation, and stable physical and chemical properties. However, due to the low density of active sites in bulk carbon nitride, it is easily affected by photogenerated charge-hole recombination, so its activity in the photocatalytic decomposition of water to produce hydrogen is relatively weak. Catalyst surface engineering strategies can provide abundant surface active sites for photocatalytic hydrogen production reactions.

[0003] Constructing carbon nitride polymers with abundant surface active sites is an effective strategy to improve the performance of photocatalytic hydrogen production. Among them, the special morphology and the construction of nanosheets can effectively increase the specific surface area of ​​carbon nitride, expose more active sites, and shorten the diffusion path of photogenerated charges. Due to the quantum confinement effect, the electronic band gap of carbon nitride with a thin layer structure will move in the opposite direction to obtain a larger conduction band potential, thereby providing a stronger reduction ability for the photocatalytic hydrogen production reaction. At the same time, carbon nitride with a one-dimensional tubular structure has received increasing attention in recent years. The thin layer of the tube wall can shorten the transmission distance of the photogenerated charge to the surface, which can effectively increase the migration rate of the photogenerated charge, thereby improving the separation efficiency of electrons and holes. Constructing a porous structure on tubular carbon nitride can effectively increase the active sites on its surface. However, even carbon nitride with a porous tubular structure is difficult to effectively utilize the active sites inside the tube (patent CN115845894A). Therefore, it is of great significance to prepare a carbon nitride tube with a structure. Summary of the invention

[0004] The purpose of the present invention is to provide a micron-sized carbon nitride and its preparation method and application. A rod-shaped precursor is obtained by hydrothermal method, and hexagonal graphite phase tubular carbon nitride is obtained after calcination in argon atmosphere, and carbon nitride is further obtained after thermal stripping in air. The synthesis method is simple and repeatable, and the raw material price is low, which provides a green and efficient preparation scheme for the preparation of metal-free high-efficiency photocatalyst.

[0005] The technical solution of the present invention is achieved in this way:

[0006] The invention provides a micron-sized carbon nitride, wherein the length of the micron-sized carbon nitride is 10-20 μm, the diameter of the maximum cross section is 2-10 μm, the tube wall thickness is 5-30 nm, the diameter of the hollow particle pore structure inside the micron-sized carbon nitride is 30-150 nm, and the wall thickness is 5-15 nm.

[0007] The present invention further protects a method for preparing the above-mentioned micron-sized carbon nitride, comprising the following steps:

[0008] (1) Dispersing a carbon-nitrogen-containing precursor in deionized water, placing the mixture in a reactor, and subjecting the mixture to a hydrothermal reaction. After the reactor is cooled to room temperature, the reactor is opened to separate a white precursor.

[0009] (2) drying the white precursor obtained in step (1), and calcining under the protection of an inert gas to obtain yellow hexagonal graphite phase tubular carbon nitride;

[0010] (3) Stack the openings of the corundum crucibles relative to each other to form a space, place the hexagonal tubular carbon nitride obtained in step (2) on the aluminum foil of the lower crucible, and cover it with another crucible. At this time, the sample is in the middle of the two corundum crucibles. Wrap a layer of aluminum foil on the outside of the two crucibles, then place them in a muffle furnace for calcination and cool them down to obtain micron-sized carbon nitride.

[0011] As a further improvement of the present invention, the temperature of the hydrothermal reaction is 180-210°C, and the time is 10-12h. During the hydrothermal reaction, a precursor solution of a certain concentration is fully dissolved under high temperature and high pressure, and self-assembles to form a precursor after cooling. If the precursor concentration is too high, it is not conducive to self-assembly to form a rod-shaped precursor. Too low temperature or too short hydrothermal reaction time is not conducive to the dissolution and reaction of the precursor. Too high temperature will cause certain damage to the inner tank of the reactor, and will also cause excessive decomposition of the precursor, which is not conducive to the precipitation of the product.

[0012] As a further improvement of the present invention, the carbon-nitrogen-containing precursor is melamine.

[0013] As a further improvement of the present invention, the concentration of the carbon-nitrogen-containing precursor is 8-33 mg / mL.

[0014] As a further improvement of the present invention, the cooling is natural cooling. The cooling rate will affect the morphology of the precursor.

[0015] As a further improvement of the present invention, during the calcination process in step (2), the heating rate is selected between 5-8°C / min, the calcination temperature is between 550-570°C, and the calcination time is selected between 3-5h.

[0016] As a further improvement of the present invention, the heating rate of the muffle furnace calcination in step (3) is selected between 5-8°C / min, the calcination temperature is selected between 450-520°C, and the calcination time is selected between 0.5-1.5h.

[0017] The present invention further protects an application of the above-mentioned micron-sized carbon nitride in the field of photocatalytic hydrogen production.

[0018] The present invention has the following beneficial effects:

[0019] The present invention obtains a rod-shaped precursor by hydrothermal method, and obtains hexagonal graphite phase tubular carbon nitride after calcination in argon atmosphere, and further obtains carbon nitride after thermal exfoliation in air. The synthesis method is simple and repeatable, and the raw material price is low, which provides a green and efficient preparation scheme for the preparation of metal-free high-efficiency photocatalyst.

[0020] The present invention develops a carbon nitride photocatalyst, the porous thin-wall structure accelerates the transfer and separation of photogenerated charges, while the half-tube structure effectively increases the specific surface area of ​​the catalyst, fully exposes the active sites inside the tube, and effectively improves the photocatalytic performance of the catalyst.

[0021] The specific thermal stripping device of the present invention provides more options for synthesizing thin-layer structure materials. At the same time, the carbon nitride obtained by the present invention can be compounded with other semiconductor materials and its surface can be modified to promote interface charge transfer, optimize the energy band structure, and further improve the photocatalytic activity of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0023] Figure 1 This is a scanning electron microscope (SEM) photo of carbon nitride;

[0024] Figure 2 This is a scanning electron microscope (SEM) photo of carbon nitride;

[0025] Figure 3 This is a scanning electron microscope (SEM) image of hexagonal tubular carbon nitride for comparison;

[0026] Figure 4 is the X-ray diffraction spectrum (XRD) of carbon nitride;

[0027] Figure 5 These are the test results of the photocatalytic hydrogen production performance of carbon nitride. DETAILED DESCRIPTION

[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Example 1

[0030] This embodiment provides a method for preparing micron-sized carbon nitride, comprising the following steps:

[0031] (1) Ultrasonic dispersion of melamine in deionized water at a concentration of 8 mg / mL was performed, and the mixture was placed in a reactor for hydrothermal reaction at 180°C for 10 h. After the reactor was naturally cooled to room temperature, the reactor was opened and a white precursor was separated;

[0032] (2) drying the white precursor obtained in step (1), and calcining under the protection of an inert gas to obtain yellow hexagonal graphite phase tubular carbon nitride;

[0033] During the calcination process, the heating rate is selected at 5°C / min, the calcination temperature is 550°C, and the calcination time is selected at 3h;

[0034] The openings of the corundum crucibles are stacked together to form a space, and the hexagonal tubular carbon nitride obtained in step (2) is placed on the aluminum foil of the lower crucible, and covered with another crucible. At this time, the sample is in the middle of the two corundum crucibles. A layer of aluminum foil is wrapped on the outside of the two crucibles. Then, it is placed in a muffle furnace for calcination. The heating rate is selected at 5°C / min, the calcination temperature is selected at 450°C, the calcination time is selected at 0.5h, and the temperature is naturally lowered to obtain micron-sized carbon nitride.

[0035] Example 2

[0036] This embodiment provides a method for preparing micron-sized carbon nitride, comprising the following steps:

[0037] (1) Ultrasonic dispersion of melamine in deionized water at a concentration of 33 mg / mL was performed, and the mixture was placed in a reactor for hydrothermal reaction at 210 °C for 12 h. After the reactor was naturally cooled to room temperature, the reactor was opened and a white precursor was separated;

[0038] (2) drying the white precursor obtained in step (1), and calcining under the protection of an inert gas to obtain yellow hexagonal graphite phase tubular carbon nitride;

[0039] During the calcination process, the heating rate is selected at 8°C / min, the calcination temperature is 570°C, and the calcination time is selected at 5h;

[0040] (3) Stack the openings of the corundum crucibles relative to each other to form a space, place the hexagonal tubular carbon nitride obtained in step (2) on the aluminum foil of the lower crucible, and cover it with another crucible. At this time, the sample is in the middle of the two corundum crucibles. Wrap a layer of aluminum foil on the outside of the two crucibles, and then place it in a muffle furnace for calcination. The heating rate is selected at 8°C / min, the calcination temperature is selected at 520°C, the calcination time is selected at 1.5h, and the temperature is naturally lowered to obtain micron-sized carbon nitride.

[0041] Example 3

[0042] This embodiment provides a method for preparing micron-sized carbon nitride, comprising the following steps:

[0043] (1) Melamine was ultrasonically dispersed in deionized water at a concentration of 20 mg / mL, and the mixture was placed in a reactor for hydrothermal reaction at 200 °C for 11 h. After the reactor was naturally cooled to room temperature, the reactor was opened and a white precursor was separated;

[0044] (2) drying the white precursor obtained in step (1), and calcining under the protection of an inert gas to obtain yellow hexagonal graphite phase tubular carbon nitride;

[0045] During the calcination process, the heating rate is selected at 6°C / min, the calcination temperature is 560°C, and the calcination time is selected at 4h;

[0046] The openings of the corundum crucibles are stacked together to form a space, and the hexagonal tubular carbon nitride obtained in step (2) is placed on the aluminum foil of the lower crucible, and covered with another crucible. At this time, the sample is in the middle of the two corundum crucibles. A layer of aluminum foil is wrapped on the outside of the two crucibles. Then, it is placed in a muffle furnace for calcination. The heating rate is selected at 6°C / min, the calcination temperature is selected at 480°C, the calcination time is selected at 1h, and the temperature is naturally lowered to obtain micron-sized carbon nitride. Figure 1 and Figure 2 This is a scanning electron microscope (SEM) image of carbon nitride. Figure 4 This is the X-ray diffraction pattern (XRD) of carbon nitride.

[0047] Figure 3 This is a scanning electron microscope (SEM) image of hexagonal tubular carbon nitride for comparison. Figure 1 , 2 and Figure 3 It can be seen that compared with hexagonal tubular carbon nitride, carbon nitride provides a richer surface structure, which will help improve its performance.

[0048] Figure 5 The photocatalytic hydrogen production performance test results of carbon nitride are shown in Figure 2. From the results, it can be seen that the photocatalytic hydrogen production performance of carbon nitride is significantly better than that of hexagonal tubular carbon nitride.

[0049] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A micron-sized carbon nitride, characterized in that: The length of the micron-sized carbon nitride is 10-20 μm, the diameter of the maximum cross section is 2-10 μm, the wall thickness is 5-30 nm, the diameter of the hollow particle pore structure inside the micron-sized carbon nitride is 30-150 nm, and the wall thickness is 5-15 nm. The preparation method comprises the following steps: (1) Dispersing melamine in deionized water, placing the mixture in a reactor, and subjecting the mixture to a hydrothermal reaction. After the reactor is cooled to room temperature, the reactor is opened to separate a white precursor. (2) drying the white precursor obtained in step (1), and calcining under the protection of an inert gas to obtain yellow hexagonal graphite phase tubular carbon nitride; (3) stacking the openings of the corundum crucibles relative to each other to form a space, placing the hexagonal tubular carbon nitride obtained in step (2) on the aluminum foil of the lower crucible, and covering it with another crucible. At this time, the sample is in the middle of the two corundum crucibles, and a layer of aluminum foil is wrapped on the outside of the two crucibles. Then, the crucibles are placed in a muffle furnace for calcination and cooled to obtain micron-sized carbon nitride; the heating rate of the muffle furnace calcination is selected between 5-8°C / min, the calcination temperature is selected between 450-520°C, and the calcination time is selected between 0.5-1.5h.

2. The micron-sized carbon nitride according to claim 1, characterized in that: The temperature of the hydrothermal reaction is 180-210° C. and the time is 10-12 hours.

3. The micron-sized carbon nitride according to claim 1, characterized in that: The concentration of melamine is 8-33 mg / mL.

4. The micron-sized carbon nitride according to claim 1, characterized in that: The cooling is natural cooling.

5. Use of the micron-sized carbon nitride as claimed in any one of claims 1 to 4 in the field of photocatalytic hydrogen production.