A method for in-situ preparation of sodium vanadium fluorophosphate using vanadium-containing leaching solution

Through the in-situ preparation method of vanadium-containing leaching solution, the problems of many processes and high energy consumption in the existing technology are solved, process simplification and efficient utilization of vanadium resources are achieved, production costs and energy consumption are reduced, and vanadium is extended. Chemical industry chain.

CN118637588BActive Publication Date: 2024-11-15NORTHEASTERN UNIV CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411097507.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-15
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

In the prior art, there are many processes, high energy consumption and low efficiency in the preparation of sodium vanadium fluorine phosphate, resulting in low vanadium resource utilization efficiency.

Method used

The vanadium-containing leaching solution is prepared in situ by using the in-situ preparation method. Through the steps of roasting, leaching, reduction and solvent heat, the vanadium-containing minerals are converted into vanadium-fluorophosphate, eliminating the preparation process of vanadium oxide and vanadate, and directly synthesized in situ. Sodium vanadium fluorophosphate.

Benefits of technology

The process flow has been greatly shortened, production costs and energy consumption have been reduced, efficient utilization of vanadium resources and value-added utilization of vanadium, and extended the vanadium chemical industry chain.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118637588B_ABST
    Figure CN118637588B_ABST
Patent Text Reader

Abstract

The invention relates to a method for in-situ preparing sodium vanadium fluorophosphate by using vanadium-containing leaching solution, the steps of which are: mixing a vanadium-containing mineral with a roasting additive to obtain a mixed material, and then roasting to obtain a roasted clinker, wherein the mass ratio of the vanadium-containing mineral to the roasting additive is 3 to 8:1; crushing the roasted clinker, grinding it, leaching it, and then separating the solid and the liquid to obtain a vanadium-containing leaching solution; adding a reducing agent and an organic solvent to the vanadium-containing leaching solution to obtain a vanadium-containing sodium vanadium fluorophosphate; 4+ The obtained V-containing 4+ After the leachate is air-cooled, a phosphorus source and a fluorine source are added at a V:P:F ratio of 2:2:0.5-5, the pH is adjusted to 5-8, and then the leachate is transferred into a reactor, and the reaction is cooled after completion; the obtained product is subjected to solid-liquid separation, and the precipitation is repeatedly washed and dried to obtain sodium vanadium fluorophosphate. The present invention realizes the short-process, low-energy-consumption and high-efficiency synthesis of sodium vanadium fluorophosphate materials, and the synthesized sodium vanadium fluorophosphate material can be used as a positive electrode material for sodium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of vanadium chemical technology and resource recycling, and specifically relates to a method for in-situ preparation of sodium vanadium fluorophosphate by utilizing vanadium-containing leaching solution. Background Art

[0002] As the global energy crisis and environmental pollution problems intensify, the development of new renewable energy has become a trend, and high-efficiency energy storage devices are the key to the development of clean energy storage, electric vehicles, electronic devices and micro-nano energy. Sodium-ion batteries have become the fastest-growing energy storage batteries due to their excellent performance and abundant sodium resources. Sodium vanadium fluorophosphate is a sodium superionic conductor (NASICON), which has excellent sodium ion conductivity and a high charge and discharge platform, and is one of the excellent positive electrode materials for sodium-ion batteries.

[0003] The traditional process for preparing sodium vanadium fluorophosphate is to use vanadium products such as vanadium pentoxide, sodium metavanadate, and ammonium metavanadate. For example, the preparation method of sodium vanadium fluorophosphate, a positive electrode material for sodium ion batteries, disclosed in Chinese patent CN112919442, uses a vanadium source selected from ammonium metavanadate, vanadium pentoxide, and sodium vanadate.

[0004] However, these vanadium products are prepared from vanadium-containing leachates obtained through roasting, leaching and extraction of vanadium-containing minerals. For example, Chinese patent CN114231758 discloses a vanadium pentoxide, an ammonium-free preparation method and use thereof, which comprises the following steps: sodium roasting, leaching filtration, acid reduction, extraction-strip extraction of vanadium, crystallization to obtain vanadium sulfate crystals, and calcination and decomposition of vanadium sulfate crystals to obtain vanadium pentoxide.

[0005] In summary, in the existing methods, sodium vanadium fluorophosphate, a positive electrode material for batteries, is finally obtained from vanadium minerals, which has many steps, high energy consumption and low efficiency. Summary of the invention

[0006] 1. Technical issues to be resolved

[0007] In order to solve the above problems in the prior art, the present invention provides a method for in-situ preparation of sodium vanadium fluorophosphate using vanadium-containing leaching solution, which realizes the synthesis of sodium vanadium fluorophosphate from vanadium-containing leaching solution in a short process and with high vanadium conversion rate, and the synthesized sodium vanadium fluorophosphate can be used as a positive electrode material for sodium ion batteries.

[0008] (II) Technical solution

[0009] In order to achieve the above object, the main technical solutions adopted by the present invention include:

[0010] The present invention provides a method for in-situ preparation of sodium vanadium fluorophosphate using a vanadium-containing leaching solution, which comprises the following steps:

[0011] S1. Mixing a vanadium-containing mineral with a roasting additive to obtain a mixed material, and then roasting the mixed material to obtain a roasted clinker, wherein the mass ratio of the vanadium-containing mineral to the roasting additive is 3 to 8:1; and converting the vanadium spinel phase in the vanadium-containing mineral into a soluble vanadate by roasting;

[0012] S2, crushing and grinding the roasted clinker obtained in step S1, leaching, and then separating the solid and liquid to obtain a vanadium-containing leaching solution and tailings;

[0013] S3, adding a reducing agent and an organic solvent to the vanadium-containing leaching solution obtained in step S2, reducing it at 60-100° C. for 20-120 min, until the solution changes from light yellow to blue, and V 5+ Restore to V 4+ , we get V 4+ Vanadium-containing leaching solution. Adding a reducing agent before solvent heating can reduce the V in the vanadium-containing leaching solution. 5+ Restore to V 4+ , avoiding the solvothermal process V 5+ The reduction and sodium vanadium fluorophosphate synthesis are carried out simultaneously, which improves the vanadium conversion rate;

[0014] S4, air-cooling the low-valent vanadium-containing leaching solution obtained in step S3, adding a phosphorus source and a fluorine source at a V:P:F molar ratio of 2:2:0.5-5, adjusting the pH to 5-8, and then transferring it into a reactor, and cooling it to room temperature after the reaction is completed;

[0015] S5, separating the product obtained in step S4 into solid and liquid, and repeatedly washing and precipitating, and then drying to obtain sodium vanadium fluorophosphate.

[0016] Preferably, in step S1, the vanadium-containing mineral is one or more of vanadium-titanium magnetite, vanadium slag, vanadium extraction tailings, vanadium-containing stone coal or vanadium-containing waste catalyst; the roasting additive is at least one of sodium carbonate, sodium bicarbonate, sodium chloride, sodium sulfate, sodium thiosulfate, sodium nitrate, sodium fluoride and sodium nitrate.

[0017] Preferably, in step S1, the calcination temperature is 750-1000°C, and the calcination time is 30-180 minutes.

[0018] Preferably, in step S2, the calcined clinker is ground to a particle size of less than 74 μm.

[0019] Preferably, in step S2, the leaching medium is water, preferably deionized water, the medium and the roasted clinker are added at a liquid-solid ratio of 3-20 mL:1g, the temperature of the leaching process is 60-95°C; the time of the leaching process is 30-150 min; the solid-liquid separation is achieved by filtration or centrifugation.

[0020] Preferably, in step S3, the molar ratio of the reducing agent to the vanadium in the vanadium-containing leachate is 1:1-5, and the reducing agent is one or more of oxalic acid, citric acid, ascorbic acid, tartaric acid, malic acid, acetic acid, propionic acid, sulfonic acid, sulfinic acid, and sodium nitrite mixed in any proportion; the volume ratio of the organic solvent to the vanadium-containing leachate is 1:1-5, and the organic solvent is one or more of methanol, ethanol, glycerol, ethylene glycol, ethylenediamine, dimethylformamide (DMF), dimethyl sulfoxide (DMSO), and acetone.

[0021] Preferably, in step S3, the reduction temperature is 60-100° C., and the reduction time is 20-120 min.

[0022] Preferably, in step S4, the phosphorus source is one or more of phosphoric acid, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium phosphate, sodium pyrophosphate, and sodium dihydrogen pyrophosphate; the fluorine source is sodium fluoride, aluminum fluoride, calcium fluoride, magnesium fluoride, cryolite (Na 3 AlF 6 ) one or more of them.

[0023] Preferably, in step S4, the reactor is a polytetrafluoroethylene liner hydrothermal synthesis reactor; a solvent thermal reaction is carried out in the reactor, the solvent is a mixed solvent of the organic solvent added in step S3 and the vanadium-containing leaching solution, the pH range is 5 to 8, the solvent thermal temperature is at least 150° C., and the solvent thermal time is 2 to 36 h; the cooling method is natural room temperature cooling or water cooling.

[0024] Preferably, in step S5, the solid-liquid separation is achieved by filtering or centrifuging, and the rinsing is repeated several times with water and ethanol in sequence. The drying temperature is 60-120°C, and the vacuum drying is 6-48 hours.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] The invention provides a method for in-situ preparing sodium vanadium fluorophosphate by using a vanadium-containing leachate, which comprises the following steps: using a vanadium-containing leaching solution obtained by pre-treating a vanadium-containing mineral and a sodium-containing roasting additive through roasting, leaching, reduction, etc. as a vanadium source, adding a phosphorus source and a fluorine source, and in-situ preparing sodium vanadium fluorophosphate; and further ensuring that the final product is pure-phase sodium vanadium fluorophosphate by controlling the dosage ratio of the vanadium-containing mineral and the roasting additive, the amount of F added, and the solvent thermal temperature.

[0027] The present invention uses vanadium-containing leaching solution as mother liquor, and the process eliminates the process of preparing vanadium products such as vanadium oxide and vanadate from vanadium-containing resources. The in-situ preparation of sodium vanadium fluorophosphate can greatly shorten the process flow and reduce production costs and energy consumption. The prepared sodium vanadium fluorophosphate can be used in the positive electrode of sodium ion batteries, which makes efficient use of vanadium-containing resources, realizes process innovation and value-added utilization of vanadium, and extends the vanadium chemical industry chain. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is the XRD pattern of sodium vanadium fluorophosphate prepared in Example 1 of the present invention;

[0029] Figure 2 This is a SEM image of sodium vanadium fluorophosphate prepared in Example 1 of the present invention;

[0030] Figure 3 This is the full XPS spectrum of sodium vanadium fluorophosphate prepared in Example 1 of the present invention;

[0031] Figure 4 This is a high-resolution V 2p XPS spectrum of sodium vanadium fluorophosphate prepared in Example 1 of the present invention;

[0032] Figure 5 The charge and discharge curve of sodium vanadium fluorophosphate prepared in Example 1 of the present invention;

[0033] Figure 6 This is the SEM image of Comparative Example 1 when the V:P:F molar ratio is 2:2:0.1;

[0034] Figure 7 This is the SEM image of Comparative Example 2 when the V:P:F molar ratio is 2:2:5.5;

[0035] Figure 8 This is the SEM image of Comparative Example 4 when the pH is 4.5;

[0036] Fig. 9 This is the SEM image of Comparative Example 5 when the pH is 8.5;

[0037] Fig.10 This is the SEM image of Comparative Example 6 when the solvent thermal temperature is 140°C;

[0038] Fig.11 This is the SEM image of Comparative Example 7 when the solvent thermal temperature is 220°C. DETAILED DESCRIPTION

[0039] In order to better explain the present invention and facilitate understanding, the present invention is described in detail below in conjunction with the accompanying drawings through specific implementation methods. The vanadium-containing resources described in the present invention are mainly recovered vanadium-containing minerals, wherein the vanadium content in vanadium-titanium magnetite is 0.3% to 1.8% in terms of V2O5; the vanadium content in vanadium slag is 5% to 20% in terms of V2O5; the vanadium content in vanadium extraction tailings is 0.3% to 2.8% in terms of V2O5; the vanadium content in vanadium-containing stone coal is 0.1% to 1% in terms of V2O5; the vanadium content in vanadium-containing waste catalyst is 3% to 8% in terms of V2O5. Water is tap water, pure water, etc., which is not specifically limited in this embodiment. Other chemical reagents are all commercially available reagents.

[0040] The principle of the present invention is to transfer vanadium in vanadium-containing minerals into leachate through roasting-leaching and other processes. Specifically, in the roasting process, sodium-containing roasting additives are added to convert the insoluble spinel in the vanadium-containing minerals into vanadates soluble in the leaching medium; then a reducing agent and an organic solvent are added for reduction to obtain a low-valent vanadium-containing leachate, and the vanadium and sodium in the vanadium-containing leachate are used as vanadium source and sodium source respectively, and then a phosphorus source and a fluorine source are added, and sodium vanadium fluorophosphate is prepared in situ by a solvothermal method, and the present invention specifically defines the dosage ratio of vanadium-containing minerals and roasting additives to ensure that more spinel phases in vanadium-containing minerals are converted into soluble vanadates; vanadates are dissolved in the leachate by leaching, and the present invention further defines the amount of F added and the hydrothermal temperature to further ensure that the final product is pure phase sodium vanadium fluorophosphate.

[0041] Example 1

[0042] A method for in-situ preparation of sodium vanadium fluorophosphate using a vanadium-containing leaching solution comprises the following steps:

[0043] (1) The vanadium slag with a vanadium content (in terms of V2O5) of 13.43% was subjected to sodium roasting, the roasting additive was sodium carbonate, the mass ratio of vanadium slag to sodium carbonate was 4:1, the roasting temperature was 900°C, the heating rate was 10°C / min, the roasting time was 60 min, and the roasted clinker was obtained after roasting;

[0044] (2) crushing the roasted clinker and grinding it to about 200 mesh, i.e., to a particle size of less than 74 μm, adding water at a liquid-solid ratio of water to roasted clinker of 10 mL / g for leaching, the leaching temperature is 90°C, the leaching time is 60 min, and after the leaching is completed, filtering to separate the solid and liquid, and obtaining a vanadium-containing leaching solution;

[0045] (3) Take 40 mL of vanadium-containing leaching solution, add 20 ml of ethanol and oxalic acid, the molar ratio of oxalic acid to vanadium is 1:2, and reduce at 80 °C for 1 h to remove V in the vanadium-containing leaching solution. 5+ Restore to V 4+ , and then air-cooled to room temperature (25°C) to obtain a low-valent vanadium-containing leaching solution;

[0046] (4) adding sodium dihydrogen phosphate and sodium fluoride to the reduced low-valent vanadium-containing leaching solution at a V:P:F ratio of 2:2:2.5, adjusting the pH to 6 with sodium hydroxide, and transferring the solution to a hydrothermal reactor for reaction at 180 °C for 24 h. After the reaction, the solution was naturally cooled to room temperature.

[0047] (5) The reaction product was separated by filtration, and the solid was repeatedly washed with water and ethanol for several times to obtain a light blue-green solid. The solid was then dried in an oven at 80 °C for 24 h to obtain sodium vanadium fluorophosphate. The vanadium recovery rate was 91.86%. X-ray diffraction analysis showed that the XRD pattern was consistent with that of the sodium vanadium fluorophosphate standard card.

[0048] Example 2

[0049] A method for in-situ preparation of sodium vanadium fluorophosphate using a vanadium-containing leaching solution comprises the following steps:

[0050] (1) The vanadium content (in V 2 O 5 The vanadium-titanium magnetite with a mass ratio of 0.5% by weight of vanadium-titanium magnetite is subjected to sodium roasting, the roasting additive is sodium sulfate, the mass ratio of vanadium-titanium magnetite to sodium sulfate is 3:1, the roasting temperature is 750°C, the heating rate is 10°C / min, the roasting time is 180 min, and the roasted clinker is obtained after roasting;

[0051] (2) The roasted clinker was crushed and ground to less than 74 μm, and water was added to the roasted clinker at a liquid-solid ratio of 3 mL / g for leaching. The leaching temperature was 95 °C and the leaching time was 30 min. After the leaching was completed, the solid and liquid were separated by filtration to obtain a vanadium-containing leaching solution;

[0052] (3) Take 40 mL of vanadium-containing leaching solution, add 20 mL of ethylene glycol and citric acid, the molar ratio of citric acid to vanadium is 1:5, reduce at 100 °C for 20 min, and then air cool to obtain a low-valent vanadium-containing leaching solution;

[0053] (4) adding disodium hydrogen phosphate and sodium fluoride to the reduced low-valent vanadium-containing leaching solution at a V:P:F ratio of 2:2:0.5, adjusting the pH to 5 with oxalic acid and transferring the solution to a hydrothermal reactor, reacting at 150°C for 36 h, and cooling the solution naturally to room temperature after the reaction;

[0054] (5) The reaction product was separated by filtration, and the solid was repeatedly washed with water and ethanol for several times to obtain a light blue-green solid, which was then dried in an oven at 80 °C for 24 h to obtain sodium vanadium fluorophosphate. The vanadium recovery rate was 92.33%.

[0055] Example 3

[0056] A method for in-situ preparation of sodium vanadium fluorophosphate using a vanadium-containing leaching solution comprises the following steps:

[0057] (1) The vanadium content (in V 2 O 5 The high chrome vanadium slag with a content of 14.12% is subjected to sodium roasting, the roasting additive is sodium bicarbonate, the mass ratio of high chrome vanadium slag to sodium bicarbonate is 8:1, the roasting temperature is 1000°C, the heating rate is 10°C / min, the roasting time is 30 min, and the roasting clinker is obtained after roasting;

[0058] (2) The roasted clinker was crushed and ground to less than 74 μm, and water was added to the roasted clinker at a liquid-to-solid ratio of 20 mL / g for leaching. The leaching temperature was 60°C and the leaching time was 150 min. After the leaching was completed, the solid and liquid were separated by filtration to obtain a vanadium-containing leaching solution;

[0059] (3) Take 40 mL of vanadium-containing leaching solution, add 20 mL of ethylene glycol and tartaric acid, the molar ratio of tartaric acid to vanadium is 1:3, reduce at 60 °C for 120 min, and then air cool to obtain a low-valent vanadium-containing leaching solution;

[0060] (4) Phosphoric acid and sodium fluoride were added to the reduced low-valent vanadium-containing leaching solution at a V:P:F molar ratio of 2:2:5, and the pH was adjusted to 8 with sodium hydroxide. The solution was transferred into a hydrothermal reactor and reacted at 210 °C for 2 h. After the reaction was completed, the solution was naturally cooled to room temperature.

[0061] (5) The reaction product was separated by filtration, and the solid was repeatedly washed with water and ethanol for several times to obtain a light blue-green solid, which was then dried in an oven at 80 °C for 24 h to obtain sodium vanadium fluorophosphate. The vanadium recovery rate was 91.52%.

[0062] The sodium vanadium fluorophosphate prepared in situ in Examples 1-3 was analyzed by scanning electron microscope, and the following results were obtained: Figure 2 The SEM images shown are from Figure 2 It can be seen that the prepared sodium vanadium fluorophosphate is composed of micron particles. Figure 3 The XPS spectrum shows that the elemental composition is Na, V, P, O, F and C. The high-resolution XPS spectrum of V 2p ( Figure 4 ) analyzed the valence state of the V element, and the peaks at 517.28 eV and 524.68 eV correspond to the V 2p 3 / 2 Electron Orbitals and V 2p 1 / 2 The electron orbit was determined to determine the valence state of the vanadium element to be +4, and it was further confirmed that the product prepared in situ by the vanadium-containing leaching solution was sodium vanadium fluorophosphate.

[0063] Figure 5 When sodium vanadium fluorophosphate material is used as the positive electrode of sodium ion battery, the theoretical specific capacity is 130mA g -1) under the cycle performance diagram. After 500 charge and discharge cycles, the reversible specific capacity is stable at 45.78 mA h g -1 The capacity retention rate is excellent, reaching 78.03%, and it has good cycle stability. The electrochemical performance of sodium vanadium fluorophosphate prepared in situ after 500 cycles is comparable to that of sodium vanadium fluorophosphate prepared by current pure chemical reagents, but the preparation process of the present invention is shorter and the process is simpler, which promotes the commercial production of sodium vanadium fluorophosphate.

[0064] Comparative Example 1

[0065] The difference between Comparative Example 1 and Example 1 is that in step (4), V:P:F is 2:2:0.1. Figure 6 As shown, the final material obtained is mainly composed of micron blocks with rough surfaces, which can affect the electrochemical properties of the material. The vanadium recovery rate is only 53.35%, and sodium vanadium fluorophosphate with different fluorine contents is generated.

[0066] Comparative Example 2

[0067] The difference between Comparative Example 2 and Example 1 is that in step (4), V:P:F is 2:2:5.5. Figure 7 As shown, the final material obtained is mainly composed of rough micron blocks and nano powders from the scanning electron microscope, which will affect the stability of the electrode. In addition, the vanadium recovery rate is low, at 75.36%, and sodium vanadium fluorophosphate with different fluorine contents is generated.

[0068] Comparative Example 3

[0069] The difference between Comparative Example 3 and Example 1 is that, in step S3, after adding the reducing agent and the organic solvent, a solvothermal reaction is directly carried out, and the specific steps are:

[0070] (1) The vanadium content (in V 2 O 5 The vanadium slag with a vanadium content of 13.43% is subjected to sodium roasting, the roasting additive is sodium carbonate, the mass ratio of vanadium slag to sodium carbonate is 4:1, the roasting temperature is 900°C, the heating rate is 10°C / min, the roasting time is 60 min, and the roasted clinker is obtained after roasting;

[0071] (2) crushing the roasted clinker and grinding it to about 200 mesh, i.e., to a particle size of less than 74 μm, adding water at a liquid-solid ratio of water to roasted clinker of 10 mL / g for leaching, the leaching temperature is 90°C, the leaching time is 60 min, and after the leaching is completed, filtering to separate the solid and liquid, and obtaining a vanadium-containing leaching solution;

[0072] (3) Take 40 mL of vanadium-containing leaching solution, add 20 ml of ethanol and oxalic acid, and the molar ratio of oxalic acid to vanadium is 1:2 to obtain solution A; add sodium dihydrogen phosphate and sodium fluoride to solution A with a V:P:F ratio of 2:2:2.5, adjust the pH to 6 with sodium hydroxide, and transfer it into a hydrothermal reactor, react at 180°C for 24 h, and naturally cool to room temperature after the reaction is completed;

[0073] (4) The reaction product was separated by filtration, and the solid was repeatedly washed with water and ethanol for several times to obtain a light blue-green solid, which was then dried in an oven at 80 °C for 24 h to obtain sodium vanadium fluorophosphate. The vanadium recovery rate was 67.75%.

[0074] Comparative Example 4

[0075] The difference between Comparative Example 4 and Example 1 is that the pH in step (4) is 4.5. Figure 8 As shown, the final material obtained is mainly composed of micron blocks of uneven size from the scanning electron microscope image, which will affect the diffusion of sodium ions. The vanadium recovery rate is 90.74%, and pure phase sodium vanadium fluorophosphate is generated.

[0076] Comparative Example 5

[0077] The difference between Comparative Example 5 and Example 1 is that the pH in step (4) is 8.5. Fig. 9 As shown, the final material obtained is mainly composed of nanoparticles, and the crystallinity is poor, which affects the cycle stability. The vanadium recovery rate is 91.53%, and pure phase sodium vanadium fluorophosphate and a small amount of sodium vanadium fluorophosphate with different fluorine contents are generated.

[0078] Comparative Example 6

[0079] The difference between Comparative Example 6 and Example 1 is that the solvent thermal temperature in step (4) is 140°C. Fig.10 As shown, the final material obtained is mainly composed of micron particles and nanoparticles from the scanning electron microscope. This irregular morphology will affect the deintercalation of sodium ions. In addition, the vanadium recovery rate is only 62.15%, generating pure phase sodium vanadium fluorophosphate.

[0080] Comparative Example 7

[0081] The difference between Comparative Example 7 and Example 1 is that the solvent thermal temperature in step (4) is 220°C. Fig.11 As shown, the final material obtained is mainly composed of micron particles and nano powders, and the morphology is irregular, resulting in poor electrode stability. The vanadium recovery rate is 90.34%, and pure phase sodium vanadium fluorophosphate is generated.

[0082] In summary, in the present method, the amount of F added determines whether pure sodium vanadium fluorophosphate is generated; although pure sodium vanadium fluorophosphate is generated by the reduction reaction and the solvent thermal reaction, the vanadium recovery rate is very low; the pH value has little effect on the vanadium recovery rate, but the sodium vanadium fluorophosphate generated in an acidic environment is relatively pure; although pure sodium vanadium fluorophosphate is generated when the solvent thermal temperature is lower than 150°C, the vanadium recovery rate is very low; when the solvent thermal temperature is higher than 210°C, pure sodium vanadium fluorophosphate is generated and the vanadium recovery rate is ideal, but from the perspective of the possible low exhaustion of production energy, the temperature is too high, which is not conducive to production, so the solvent thermal temperature is preferably 150-210°C.

[0083] Moreover, the existing sodium vanadium fluorophosphate is usually prepared from vanadium products such as vanadium pentoxide and sodium metavanadate. The vanadium products are made from vanadium-containing minerals as raw materials, and the vanadium-containing leachate is obtained through roasting-leaching and other processes. Various vanadium products are prepared from the vanadium-containing leachate by means of impurity removal, precipitation, crystallization, extraction, stripping, ion exchange and other methods. Therefore, the present invention uses vanadium-containing minerals as raw materials, and prepares sodium vanadium fluorophosphate in situ through the process of sodium roasting-water leaching-reduction-solvothermal, which can shorten the preparation process, simplify the preparation process, and reduce production costs.

Claims

1. A method for in-situ preparation of sodium vanadium fluorophosphate using a vanadium-containing leaching solution, characterized in that: The steps are: S1. Mixing a vanadium-containing mineral with a roasting additive to obtain a mixed material, and then roasting to obtain a roasted clinker, wherein the mass ratio of the vanadium-containing mineral to the roasting additive is 3 to 8:1; the roasting additive is at least one of sodium carbonate, sodium bicarbonate, sodium chloride, sodium sulfate, sodium thiosulfate, sodium nitrate, sodium fluoride, and sodium nitrate; S2, crushing and grinding the roasted clinker obtained in step S1, leaching, and then separating the solid and liquid to obtain a vanadium-containing leaching solution; S3, adding a reducing agent and an organic solvent to the vanadium-containing leaching solution obtained in step S2 to obtain a vanadium-containing 4+ leachate; S4, the V-containing 4+ After the leachate is air-cooled, a phosphorus source and a fluorine source are added at a V:P:F molar ratio of 2:2:0.5-5, wherein the fluorine source is sodium fluoride, and the pH is adjusted to 5-8, and then the leachate is transferred into a reactor, and cooled to room temperature after the reaction is completed; S5, separating the product obtained in step S4 from the solid and liquid, and repeatedly washing and precipitating, and then drying to obtain sodium vanadium fluorophosphate.

2. The method for in-situ preparation of sodium vanadium fluorophosphate using a vanadium-containing leaching solution according to claim 1, characterized in that: In step S1, the vanadium-containing mineral is one or more of vanadium-titanium magnetite, vanadium slag, vanadium extraction tailings, vanadium-containing stone coal or vanadium-containing waste catalyst.

3. The method for in-situ preparation of sodium vanadium fluorophosphate using a vanadium-containing leaching solution according to claim 1, characterized in that: In step S1, the calcination temperature is 750-1000°C, and the calcination time is 30-180 minutes.

4. The method for in-situ preparation of sodium vanadium fluorophosphate using a vanadium-containing leaching solution according to claim 1, characterized in that: In step S2, the calcined clinker is ground to a particle size of less than 74 μm.

5. The method for in-situ preparation of sodium vanadium fluorophosphate using a vanadium-containing leachate according to claim 1, characterized in that: In step S2, the leaching medium is water; the medium and the roasted clinker are added at a liquid-solid ratio of 3-20 mL:1 g, the temperature of the leaching process is 60-95° C.; and the time of the leaching process is 30-150 min.

6. The method for in-situ preparation of sodium vanadium fluorophosphate using a vanadium-containing leaching solution according to claim 1, characterized in that: In step S3, the molar ratio of the reducing agent to the vanadium in the vanadium-containing leachate is 1:1-5, and the reducing agent is one or more of oxalic acid, citric acid, ascorbic acid, tartaric acid, malic acid, acetic acid, propionic acid, sulfonic acid, sulfinic acid, and sodium nitrite mixed in any proportion; the volume ratio of the organic solvent to the vanadium-containing leachate is 1:1-5, and the organic solvent is one or more of methanol, ethanol, glycerol, ethylene glycol, ethylenediamine, dimethylformamide, dimethyl sulfoxide, and acetone.

7. The method for in-situ preparation of sodium vanadium fluorophosphate using a vanadium-containing leaching solution according to claim 1, characterized in that: In step S3, the reduction temperature is 60-100° C., and the reduction time is 20-120 min.

8. The method for in-situ preparation of sodium vanadium fluorophosphate using a vanadium-containing leaching solution according to claim 1, characterized in that: In step S4, the phosphorus source is one or more of phosphoric acid, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium phosphate, sodium pyrophosphate, and sodium dihydrogen pyrophosphate.

9. The method for in-situ preparation of sodium vanadium fluorophosphate using a vanadium-containing leachate according to claim 1, characterized in that: In step S4, the reactor is a polytetrafluoroethylene liner hydrothermal synthesis reactor; a solvent thermal reaction is carried out in the reactor, the pH range is 5 to 8, the solvent thermal temperature is at least 150° C., and the solvent thermal time is 2 to 36 h; the cooling method is natural room temperature cooling or water cooling.

10. The method for in-situ preparation of sodium vanadium fluorophosphate using a vanadium-containing leaching solution according to claim 1, characterized in that: In step S5, the drying temperature is 60-120° C., and the vacuum drying is performed for 6-48 hours.