A method for high-temperature solid-phase synthesis of lithium manganate positive electrode materials using manganese sulfate
Through high-temperature solid-phase synthesis of manganese sulfate and nitrogen-doped porous carbon composite materials, the problem of chemical stability and cycle stability of lithium manganate cathode materials has been solved, and the cycle stability and electrochemical performance of lithium-ion batteries have been significantly improved.
Patent Information
- Application Number
- CN202411095393.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-08-12
AI Technical Summary
Lithium manganate cathode material has poor chemical stability and long-term cycle stability, which limits its application in lithium-ion batteries.
Using a high-temperature solid-phase synthesis method of manganese sulfate, by adding aluminum salt and nitrogen-doped porous carbon, and optimizing pre-sintering and sintering conditions, lithium manganate with high purity and stable structure is prepared, combining aluminum-doped and nitrogen-doped porous carbon. composite materials to improve the cycle stability and electrochemical performance of the battery.
It significantly improves the chemical stability and cycle stability of lithium manganate, reduces the impact of structural changes on battery performance, extends battery life, and improves the battery's charge and discharge rate and efficiency.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion battery positive electrode materials, in particular to a method for synthesizing lithium manganate positive electrode materials in a solid phase at high temperature using manganese sulfate. Background Art
[0002] With the rapid development of the world economy and technology, a series of problems such as energy crisis, environmental pollution, and global warming have seriously threatened human survival and development, forcing humans to develop green renewable energy. The development of renewable green energy such as solar energy, wind energy, and tidal energy can alleviate these problems to a certain extent, but these energy sources cannot provide energy continuously, so efficient storage devices are needed. Recyclable rechargeable batteries are an effective storage device. Lithium-ion batteries have been rapidly developed around the world, especially in the fields of electronic products and electric vehicles. They are green and environmentally friendly, have high energy density, long service life, and are easy to use.
[0003] The electrical performance of lithium-ion batteries mainly depends on the microstructure and chemical composition of their electrode materials. Among the electrode materials, the positive electrode material is the core component of the lithium-ion battery system. The physical and chemical properties of the material play a vital role in the electrical performance of lithium-ion batteries. 2 O 4 ) has the characteristics of good rate performance, abundant resources, low cost, high safety, and environmental friendliness. It is suitable for electric vehicles, hybrid vehicles, power tools and other fields, and has become a hot topic of research in the industry and an important direction for the development of power batteries. The preparation methods of lithium manganese oxide mainly include high-temperature solid-phase synthesis, co-precipitation, hydrothermal, sol-gel, etc. Among them, the high-temperature solid-phase synthesis method is widely used because of its simple process and easy large-scale production. However, lithium manganese oxide prepared by traditional high-temperature solid-phase sintering methods has poor chemical stability and long-term cycle stability, long reaction time, high impurity content, uneven product particle size distribution, and general activity. In addition, single lithium manganese oxide as a positive electrode material for lithium-ion batteries has poor high-temperature cycle performance and high-rate performance, which limits the application of lithium manganese oxide in lithium-ion batteries. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] In view of the shortcomings of the prior art, the present invention provides a method for high-temperature solid-phase synthesis of lithium manganate positive electrode materials using manganese sulfate, which solves the problems of poor chemical stability and long-term cycle stability of lithium manganate positive electrode materials.
[0006] (II) Technical solution
[0007] In order to achieve the above object, the invention provides a method for high temperature solid phase synthesis of lithium manganate positive electrode material from manganese sulfate, comprising the following steps:
[0008] Step 1: evenly mix manganese sulfate, aluminum sulfate and deionized water, add sodium hydroxide solution and ammonia water, adjust the pH to 9-10, heat, stir, react to obtain a precipitate, wash with deionized water, filter, and dry at 80° C. for 12 hours to obtain a precursor mixture;
[0009] Step 2: After mixing the precursor mixture and lithium hydroxide, use a ball mill to perform ball milling, sintering, and cooling to obtain lithium manganate;
[0010] Step 3: Evenly mix the nitrogen-doped porous carbon and deionized water, add lithium manganate, disperse by ultrasonic, dry, transfer to a tube furnace, and calcine to obtain a positive electrode material;
[0011] The preparation method of nitrogen-doped porous carbon in step 3 comprises the following steps:
[0012] S1, deionized water, sodium hydroxide, and alkali lignin are stirred and mixed uniformly, heated, epichlorohydrin is added, heated, and then 4-aminopyridine is added, stirred and mixed, and reacted. After the reaction is completed, washing, suction filtering, and drying are performed to obtain pyridyl lignin;
[0013] S2. Pyridyl lignin, potassium hydroxide and deionized water are mixed evenly, dried, and then transferred to a tube furnace for carbonization in an argon atmosphere to obtain nitrogen-doped porous carbon.
[0014] Preferably, in step 1, the mass ratio of manganese sulfate, aluminum sulfate and deionized water is 100:0.5-2:1500-2100.
[0015] Preferably, the reaction temperature in step 1 is 45-55° C., and the reaction time is 8-10 h.
[0016] Preferably, the sodium hydroxide solution in step 1 is a sodium hydroxide solution with a mass fraction of 10%.
[0017] Preferably, the ammonia water in step 1 is a 4% by mass ammonia water solution.
[0018] Preferably, in step 1, the volume ratio of the sodium hydroxide solution to the ammonia water is 3:1.
[0019] Preferably, in step 2, the mass ratio of the precursor mixture to lithium hydroxide is 320-375:100.
[0020] Preferably, the ball milling time in step 2 is 24-30 minutes.
[0021] Preferably, in the sintering process of step 2, pre-sintering is first performed at a temperature of 400-500°C for 2 hours. After pre-sintering, the temperature is raised to 650-750°C for 2 hours, and then raised to 850-950°C for 2 hours. After sintering, the temperature is cooled to obtain lithium manganate.
[0022] Preferably, in step three, the mass ratio of nitrogen-doped porous carbon, deionized water, and lithium manganate is 5-8:5000-7500:100.
[0023] Preferably, the calcination conditions in step three are: in an argon atmosphere, the calcination temperature is 500° C., and the calcination time is 1 hour.
[0024] Preferably, the specific steps of S1 are as follows: deionized water, sodium hydroxide and alkali lignin are stirred and mixed evenly, heated to 80-95°C, heated to reflux, reacted, and the reaction time is 4-6h, and then 4-aminopyridine is added, wherein the mass ratio of deionized water, sodium hydroxide, alkali lignin, epichlorohydrin and 4-aminopyridine is 1800-2500:4-7:100:18-25:105-118, heated to 105-115°C, stirred and mixed, reacted, and the reaction time is 9-12h. After the reaction, wash with deionized water and anhydrous ethanol, filter, and dry at 80°C for 12h to obtain pyridyl lignin.
[0025] Preferably, the mass ratio of pyridyl lignin, potassium hydroxide and deionized water in S2 is 100:180-250:600-900.
[0026] Preferably, the heating rate of carbonization in S2 is 2-4°C / min, the carbonization temperature is 700-750°C, and the carbonization time is 2-3h.
[0027] 3. Beneficial technical effects
[0028] Compared with the prior art, the present invention has the following chemical mechanisms and beneficial technical effects:
[0029] (1) In the present invention, manganese sulfate is used as a manganese source and aluminum sulfate is used as an aluminum source. Lithium manganate is prepared by high-temperature solid phase synthesis, which has the advantages of low cost and easy acquisition. By optimizing the pre-sintering and sintering conditions, the reaction temperature and time are reduced, the energy consumption is reduced, and the prepared lithium manganate has high purity. At the same time, this method has the advantages of simple process, low energy consumption, and excellent product performance. In the process of high-temperature solid phase synthesis of lithium manganate, aluminum salt is added, and aluminum is introduced into lithium manganate. Aluminum doping can effectively inhibit the Jahn-Taylor effect and manganese dissolution in lithium manganate, and reduce the capacity loss caused by manganese dissolution, because Al ions enter the lattice of lithium manganate, which helps to form a more stable spinel structure and improve the chemical stability of lithium manganate, thereby significantly improving its cycle stability, reducing the impact of structural changes on battery performance, and better maintaining its structural integrity during the charge and discharge process, reducing capacity decay.
[0030] (2) In the present invention, alkali lignin is used as a carbon source, and alkali lignin and epichlorohydrin undergo a substitution reaction to introduce epoxy groups, which then undergo a ring-opening reaction with the amino group on 4-aminopyridine to obtain pyridyl lignin, and potassium hydroxide is used as a porogen, and pyridyl is used as a nitrogen source, and carbonization is performed to obtain nitrogen-doped porous carbon. Porous carbon materials have a large specific surface area and rich pore structure, which can greatly improve the conductivity of positive electrode materials, alleviate the volume change caused by the insertion and extraction of lithium ions during the charging and discharging process of the battery, and extend the battery life. At the same time, the incorporation of heteroatom nitrogen introduces additional electrons or holes, changes the electronic structure of the carbon material, and enhances the chemical adsorption and wettability of the porous carbon surface, providing an effective pathway for the transmission of electrons and ions, improving the charging and discharging rate and efficiency of the battery, and improving the electrochemical performance of the positive electrode.
[0031] (3) In the present invention, lithium manganese oxide and nitrogen-doped porous carbon are used as the positive electrode material of lithium-ion batteries. The aluminum-doped lithium manganese oxide can provide a stable crystal structure and a high energy density, which can optimize the lithium ion deintercalation process. The nitrogen-doped porous carbon can provide excellent conductivity and the ability to alleviate volume expansion, providing a channel for the rapid transmission of lithium ions. The two work together to improve battery performance and effectively improve the cycle stability of lithium-ion batteries. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0033] Example 1
[0034] A method for high-temperature solid-phase synthesis of lithium manganate positive electrode materials using manganese sulfate comprises the following steps:
[0035] (1) Mix manganese sulfate, aluminum sulfate and deionized water in a mass ratio of 100:0.5:1500, add sodium hydroxide solution and ammonia water, adjust the pH to 9, heat, stir, react at 45°C for 10 hours, obtain a precipitate, wash with deionized water, filter, and dry at 80°C for 12 hours to obtain a precursor mixture;
[0036] (2) After mixing the precursor mixture and lithium hydroxide in a mass ratio of 320:100, the mixture was ball milled in a ball mill for 24 minutes, and pre-sintered at a temperature of 400°C for 2 hours. After pre-sintering, the temperature was raised to 650°C for 2 hours, and then raised to 850°C for 2 hours. The mixture was cooled to obtain lithium manganate.
[0037] (3) Deionized water, sodium hydroxide and alkali lignin are stirred and mixed uniformly, the temperature is raised to 80°C, heated under reflux, reacted for 6 hours, and then 4-aminopyridine is added, wherein the mass ratio of deionized water, sodium hydroxide, alkali lignin, epichlorohydrin and 4-aminopyridine is 1800:4:100:18:105, the temperature is raised to 105°C, stirred and mixed, reacted for 12 hours, and after the reaction is completed, washed with deionized water and anhydrous ethanol, filtered, and dried at 80°C for 12 hours to obtain pyridyl lignin;
[0038] (4) Pyridyl lignin, potassium hydroxide and deionized water in a mass ratio of 100:180:600 were mixed evenly, dried, and then transferred to a tube furnace for carbonization in an argon atmosphere at a carbonization heating rate of 2°C / min, a carbonization temperature of 700°C, and a carbonization time of 3h to obtain nitrogen-doped porous carbon;
[0039] (5) The nitrogen-doped porous carbon and deionized water are mixed evenly, and lithium manganese oxide is added, wherein the mass ratio of the nitrogen-doped porous carbon, deionized water, and lithium manganese oxide is 5:5000:100. The mixture is ultrasonically dispersed, dried, transferred to a tubular furnace, and calcined in an argon atmosphere at a temperature of 500°C for 1 hour to obtain a positive electrode material.
[0040] Example 2
[0041] A method for high-temperature solid-phase synthesis of lithium manganate positive electrode materials using manganese sulfate comprises the following steps:
[0042] (1) Mix manganese sulfate, aluminum sulfate and deionized water in a mass ratio of 100:1:1800, add sodium hydroxide solution and ammonia water, adjust the pH to 9.5, heat, stir, react at 50°C for 9 hours, obtain a precipitate, wash with deionized water, filter, and dry at 80°C for 12 hours to obtain a precursor mixture;
[0043] (2) After mixing the precursor mixture and lithium hydroxide in a mass ratio of 340:100, a ball mill is used for ball milling for 26 minutes, and pre-sintering is first performed at a pre-sintering temperature of 450°C for 2 hours. After pre-sintering, the temperature is raised to 700°C for 2 hours, and then the temperature is raised to 900°C for 2 hours, and then cooled to obtain lithium manganate;
[0044] (3) Stir and mix deionized water, sodium hydroxide and alkali lignin, raise the temperature to 90°C, heat under reflux, react for 5 hours, add 4-aminopyridine, wherein the mass ratio of deionized water, sodium hydroxide, alkali lignin, epichlorohydrin and 4-aminopyridine is 2100:5:100:20:110, heat to 110°C, stir and mix, react for 10 hours, and after the reaction, wash with deionized water and anhydrous ethanol, filter, and dry at 80°C for 12 hours to obtain pyridyl lignin;
[0045] (4) Pyridyl lignin, potassium hydroxide and deionized water in a mass ratio of 100:210:750 were mixed evenly, dried, and then transferred to a tube furnace for carbonization in an argon atmosphere at a carbonization heating rate of 3 °C / min, a carbonization temperature of 720 °C, and a carbonization time of 2.5 h to obtain nitrogen-doped porous carbon;
[0046] (5) The nitrogen-doped porous carbon and deionized water are mixed evenly, and lithium manganese oxide is added, wherein the mass ratio of the nitrogen-doped porous carbon, deionized water, and lithium manganese oxide is 7:7000:100. The mixture is ultrasonically dispersed, dried, transferred to a tubular furnace, and calcined in an argon atmosphere at a temperature of 500°C for 1 hour to obtain a positive electrode material.
[0047] Example 3
[0048] A method for high-temperature solid-phase synthesis of lithium manganate positive electrode materials using manganese sulfate comprises the following steps:
[0049] (1) Mix manganese sulfate, aluminum sulfate and deionized water in a mass ratio of 100:1.5:2000, add sodium hydroxide solution and ammonia water, adjust the pH to 9.5, heat, stir, react at 50°C for 9 hours, obtain a precipitate, wash with deionized water, filter, and dry at 80°C for 12 hours to obtain a precursor mixture;
[0050] (2) After mixing the precursor mixture and lithium hydroxide in a mass ratio of 360:100, the mixture was ball milled in a ball mill for 26 minutes, and pre-sintered at a temperature of 480°C for 2 hours. After pre-sintering, the mixture was heated to 720°C for 2 hours, and then heated to 920°C for 2 hours. The mixture was cooled to obtain lithium manganate.
[0051] (3) Stir and mix deionized water, sodium hydroxide and alkali lignin, raise the temperature to 90°C, heat under reflux, react for 5 hours, add 4-aminopyridine, wherein the mass ratio of deionized water, sodium hydroxide, alkali lignin, epichlorohydrin and 4-aminopyridine is 2100:5:100:20:110, heat to 110°C, stir and mix, react for 10 hours, and after the reaction, wash with deionized water and anhydrous ethanol, filter, and dry at 80°C for 12 hours to obtain pyridyl lignin;
[0052] (4) Pyridyl lignin, potassium hydroxide and deionized water in a mass ratio of 100:210:750 were mixed evenly, dried, and then transferred to a tube furnace for carbonization in an argon atmosphere at a carbonization heating rate of 3 °C / min, a carbonization temperature of 720 °C, and a carbonization time of 2.5 h to obtain nitrogen-doped porous carbon;
[0053] (5) The nitrogen-doped porous carbon and deionized water are mixed evenly, and lithium manganese oxide is added, wherein the mass ratio of the nitrogen-doped porous carbon, deionized water, and lithium manganese oxide is 7:7000:100. The mixture is ultrasonically dispersed, dried, transferred to a tubular furnace, and calcined in an argon atmosphere at a temperature of 500°C for 1 hour to obtain a positive electrode material.
[0054] Example 4
[0055] A method for high-temperature solid-phase synthesis of lithium manganate positive electrode materials using manganese sulfate comprises the following steps:
[0056] (1) Mix manganese sulfate, aluminum sulfate and deionized water in a mass ratio of 100:1.5:2000, add sodium hydroxide solution and ammonia water, adjust the pH to 9.5, heat, stir, react at 50°C for 9 hours, obtain a precipitate, wash with deionized water, filter, and dry at 80°C for 12 hours to obtain a precursor mixture;
[0057] (2) After mixing the precursor mixture and lithium hydroxide in a mass ratio of 360:100, the mixture was ball milled in a ball mill for 26 minutes, and pre-sintered at a temperature of 480°C for 2 hours. After pre-sintering, the mixture was heated to 720°C for 2 hours, and then heated to 920°C for 2 hours. The mixture was cooled to obtain lithium manganate.
[0058] (3) Deionized water, sodium hydroxide and alkali lignin were stirred and mixed uniformly, the temperature was raised to 90°C, heated under reflux, reacted for 5 hours, and then 4-aminopyridine was added, wherein the mass ratio of deionized water, sodium hydroxide, alkali lignin, epichlorohydrin and 4-aminopyridine was 2400:6:100:22:115, the temperature was raised to 110°C, stirred and mixed, reacted for 10 hours, and after the reaction was completed, the mixture was washed with deionized water and anhydrous ethanol, filtered, and dried at 80°C for 12 hours to obtain pyridyl lignin;
[0059] (4) Pyridyl lignin, potassium hydroxide and deionized water in a mass ratio of 100:210:750 were mixed evenly, dried, and then transferred to a tube furnace for carbonization in an argon atmosphere at a carbonization heating rate of 3°C / min, a carbonization temperature of 740°C, and a carbonization time of 2.5 h to obtain nitrogen-doped porous carbon;
[0060] (5) The nitrogen-doped porous carbon and deionized water are mixed evenly, and lithium manganese oxide is added, wherein the mass ratio of the nitrogen-doped porous carbon, deionized water, and lithium manganese oxide is 7:7000:100. The mixture is ultrasonically dispersed, dried, transferred to a tubular furnace, and calcined in an argon atmosphere at a temperature of 500°C for 1 hour to obtain a positive electrode material.
[0061] Example 5
[0062] A method for high-temperature solid-phase synthesis of lithium manganate positive electrode materials using manganese sulfate comprises the following steps:
[0063] (1) Mix manganese sulfate, aluminum sulfate and deionized water in a mass ratio of 100:2:2100, add sodium hydroxide solution and ammonia water, adjust the pH to 10, heat, stir, react at 55°C for 8 hours, obtain a precipitate, wash with deionized water, filter, and dry at 80°C for 12 hours to obtain a precursor mixture;
[0064] (2) After mixing the precursor mixture and lithium hydroxide in a mass ratio of 375:100, a ball mill is used for ball milling for 30 minutes, and pre-sintering is first performed at a pre-sintering temperature of 500°C for 2 hours. After pre-sintering, the temperature is raised to 750°C for 2 hours, and then the temperature is raised to 950°C for 2 hours, and then cooled to obtain lithium manganate;
[0065] (3) Deionized water, sodium hydroxide and alkali lignin were stirred and mixed uniformly, the temperature was raised to 95°C, heated under reflux, reacted for 4 hours, and then 4-aminopyridine was added, wherein the mass ratio of deionized water, sodium hydroxide, alkali lignin, epichlorohydrin and 4-aminopyridine was 2500:7:100:25:118, the temperature was raised to 115°C, stirred and mixed, reacted for 9 hours, and after the reaction was completed, the mixture was washed with deionized water and anhydrous ethanol, filtered, and dried at 80°C for 12 hours to obtain pyridyl lignin;
[0066] (4) Pyridyl lignin, potassium hydroxide and deionized water in a mass ratio of 100:250:900 were mixed evenly, dried, and then transferred to a tube furnace for carbonization in an argon atmosphere at a carbonization heating rate of 4 °C / min, a carbonization temperature of 750 °C, and a carbonization time of 2 h to obtain nitrogen-doped porous carbon;
[0067] (5) The nitrogen-doped porous carbon and deionized water are mixed evenly, and lithium manganese oxide is added, wherein the mass ratio of the nitrogen-doped porous carbon, deionized water, and lithium manganese oxide is 8:7500:100. The mixture is ultrasonically dispersed, dried, transferred to a tubular furnace, and calcined in an argon atmosphere at a temperature of 500°C for 1 hour to obtain a positive electrode material.
[0068] Comparative Example 1
[0069] A method for preparing a lithium manganese oxide positive electrode material comprises the following steps:
[0070] (1) Mix manganese sulfate, aluminum sulfate and deionized water in a mass ratio of 100:1.5:2000, add sodium hydroxide solution and ammonia water, adjust the pH to 9.5, heat, stir, react at 50°C for 9 hours, obtain a precipitate, wash with deionized water, filter, and dry at 80°C for 12 hours to obtain a precursor mixture;
[0071] (2) After mixing the precursor mixture and lithium hydroxide in a mass ratio of 360:100, a ball mill is used for ball milling for 26 minutes. Pre-sintering is first performed at a pre-sintering temperature of 480°C for 2 hours. After pre-sintering, the temperature is raised to 720°C for 2 hours, and then raised to 920°C for 2 hours. The temperature is cooled to obtain a lithium manganese oxide positive electrode material.
[0072] Comparative Example 2
[0073] A method for high-temperature solid-phase synthesis of lithium manganate positive electrode materials using manganese sulfate comprises the following steps:
[0074] (1) Mix manganese sulfate and deionized water in a mass ratio of 101.5:2000, add sodium hydroxide solution and ammonia water, adjust the pH to 9.5, heat, stir, react at 50°C for 9 hours, obtain a precipitate, wash with deionized water, filter, and dry at 80°C for 12 hours to obtain a manganese hydroxide precursor;
[0075] (2) After mixing a manganese hydroxide precursor and lithium hydroxide in a mass ratio of 360:100, a ball mill is used for ball milling for 26 minutes, and a pre-sintering temperature is firstly performed at 480°C for 2 hours. After the pre-sintering, the temperature is raised to 720°C for 2 hours, and then the temperature is raised to 920°C for 2 hours, and then cooled to obtain lithium manganate;
[0076] (3) Deionized water, sodium hydroxide and alkali lignin were stirred and mixed uniformly, the temperature was raised to 90°C, heated under reflux, reacted for 5 hours, and then 4-aminopyridine was added, wherein the mass ratio of deionized water, sodium hydroxide, alkali lignin, epichlorohydrin and 4-aminopyridine was 2400:6:100:22:115, the temperature was raised to 110°C, stirred and mixed, reacted for 10 hours, and after the reaction was completed, the mixture was washed with deionized water and anhydrous ethanol, filtered, and dried at 80°C for 12 hours to obtain pyridyl lignin;
[0077] (4) Pyridyl lignin, potassium hydroxide and deionized water in a mass ratio of 100:210:750 were mixed evenly, dried, and then transferred to a tube furnace for carbonization in an argon atmosphere at a carbonization heating rate of 3°C / min, a carbonization temperature of 740°C, and a carbonization time of 2.5 h to obtain nitrogen-doped porous carbon;
[0078] (5) The nitrogen-doped porous carbon and deionized water are mixed evenly, and lithium manganese oxide is added, wherein the mass ratio of the nitrogen-doped porous carbon, deionized water, and lithium manganese oxide is 7:7000:100. The mixture is ultrasonically dispersed, dried, transferred to a tubular furnace, and calcined in an argon atmosphere at a temperature of 500°C for 1 hour to obtain a positive electrode material.
[0079] Performance Test:
[0080] The materials synthesized in Examples 1-5 and Comparative Examples 1-2 were dissolved in 0.02 g / mL N-methylpyrrolidone with acetylene black and polyvinylidene fluoride at a mass ratio of 8:1:1, and mixed evenly to obtain a mixed slurry. The mixed slurry was evenly coated on an aluminum foil and dried to obtain a positive electrode of a battery, which was pressed into a circular electrode sheet with a diameter of 12 mm. A lithium sheet was used as a negative electrode, a polypropylene film was used as a diaphragm, ethylene carbonate, dimethyl carbonate, and diethyl carbonate were mixed at a mass ratio of 1:1:1 and 1 mol / L LiPF 6After mixing, it was used as the electrolyte. The test battery was a LIR2016 button battery. The battery was assembled in a glove box with an argon atmosphere. Nickel foam was used as a filler to ensure full contact between the battery shell, the positive and negative electrodes, and the diaphragm. The battery was pressed and sealed on a button battery sealing machine. The battery was assembled and tested on a CS120 electrochemical workstation. The test temperature was 25°C, the test voltage was 3-5V, the scan rate was 0.5mV / s, the charge and discharge current density was 100mA / g, and the cycle was 200 times. The test results are shown in Table 1:
[0081] Table 1
[0082]
[0083] According to the test data in Table 1, it can be seen that the positive electrode materials prepared in Examples 1-5 are applied to lithium-ion batteries, and the lithium-ion batteries show excellent cycle stability. The battery corresponding to Example 5 can still maintain a capacity retention rate of 91.9% after 200 cycles. In Comparative Example 1, nitrogen-doped porous carbon was not added to the positive electrode material, and the specific capacity of the lithium-ion battery was improved, but the cycle stability was poor. After 200 cycles, the capacity retention rate was less than 78.3%. In Comparative Example 2, aluminum was not added to the lithium manganese oxide, and the specific capacity was reduced, and the capacity retention rate decreased.
[0084] Although the embodiments of the present invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that all equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.
Claims
1. A method for high temperature solid phase synthesis of lithium manganate positive electrode materials using manganese sulfate, Features: The steps include: Step 1: evenly mix manganese sulfate, aluminum sulfate and deionized water, add sodium hydroxide solution and ammonia water, adjust the pH to 9-10, heat, stir, react to obtain a precipitate, wash with deionized water, filter, and dry at 80° C. for 12 hours to obtain a precursor mixture; Step 2: After mixing the precursor mixture and lithium hydroxide, use a ball mill to perform ball milling, sintering, and cooling to obtain lithium manganate; Step 3: Evenly mix the nitrogen-doped porous carbon and deionized water, add lithium manganate, ultrasonically disperse, dry, transfer to a tube furnace, and calcine to obtain a positive electrode material; The preparation method of nitrogen-doped porous carbon in step 3 comprises the following steps: S1, deionized water, sodium hydroxide, and alkali lignin are stirred and mixed uniformly, heated, epichlorohydrin is added, heated, and then 4-aminopyridine is added, stirred and mixed, and reacted. After the reaction is completed, washing, suction filtering, and drying are performed to obtain pyridyl lignin; S2. Pyridyl lignin, potassium hydroxide and deionized water are mixed evenly, dried, and then transferred to a tube furnace for carbonization in an argon atmosphere to obtain nitrogen-doped porous carbon.
2. The method for high temperature solid phase synthesis of lithium manganate positive electrode material using manganese sulfate according to claim 1, Features: In the step 1, the mass ratio of manganese sulfate, aluminum sulfate and deionized water is 100:0.5-2:1500-2100.
3. The method for high temperature solid phase synthesis of lithium manganate positive electrode material using manganese sulfate according to claim 1, Features: The reaction temperature in step 1 is 45-55° C., and the reaction time is 8-10 h.
4. The method for high temperature solid phase synthesis of lithium manganate positive electrode material using manganese sulfate according to claim 1, Features: In the step 2, the mass ratio of the precursor mixture to lithium hydroxide is 320-375:
100.
5. The method for high temperature solid phase synthesis of lithium manganate positive electrode material using manganese sulfate according to claim 1, Features: In the sintering process of step 2, pre-sintering is first performed at a temperature of 400-500°C for 2 hours. After pre-sintering, the temperature is raised to 650-750°C for 2 hours, and then raised to 850-950°C for 2 hours. After sintering, the temperature is cooled to obtain lithium manganate.
6. The method for high temperature solid phase synthesis of lithium manganate positive electrode material using manganese sulfate according to claim 1, Features: In the step three, the mass ratio of nitrogen-doped porous carbon, deionized water, and lithium manganate is 5-8:5000-7500:
100.
7. The method for high temperature solid phase synthesis of lithium manganate positive electrode material using manganese sulfate according to claim 1, Features: The calcination conditions in step 3 are: in an argon atmosphere, the calcination temperature is 500° C., and the calcination time is 1 hour.
8. The method for high temperature solid phase synthesis of lithium manganate positive electrode material using manganese sulfate according to claim 1, Features: The specific steps of S1 are as follows: deionized water, sodium hydroxide and alkali lignin are stirred and mixed evenly, heated to 80-95°C, heated to reflux, reacted, and the reaction time is 4-6h, and then 4-aminopyridine is added, wherein the mass ratio of deionized water, sodium hydroxide, alkali lignin, epichlorohydrin and 4-aminopyridine is 1800-2500:4-7:100:18-25:105-118, heated to 105-115°C, stirred and mixed, reacted, and the reaction time is 9-12h. After the reaction, wash with deionized water and anhydrous ethanol, filter, and dry at 80°C for 12h to obtain pyridyl lignin.
9. The method for high temperature solid phase synthesis of lithium manganate positive electrode material using manganese sulfate according to claim 1, Features: The heating rate of carbonization in S2 is 2-4°C / min, the carbonization temperature is 700-750°C, and the carbonization time is 2-3h.