A method for preparing negative ion clay air purification particles
The characteristic factors of the calcined image are analyzed by infrared thermal imaging technology, and the sintering time is adjusted adaptively, which solves the problem of sintering time control in the preparation of negative ion clay air purification particles and improves the air flux performance of the particles.
Patent Information
- Application Number
- CN202411104060.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-13
AI Technical Summary
During the preparation of negative ion clay air purification particles, improper control of sintering time will lead to deformation, crushing or insufficient binding force of clay particles, affecting their purification capacity and air flux performance.
Images during the calcination process are collected through infrared thermal imaging technology, edge and corner features of pixel points are analyzed, different temperature points, thermal boundary and neighborhood feature factors are calculated, and the sintering time is adaptively adjusted using the calcination sufficient coefficient of the response cluster cluster. Ensure full calcination.
The negative ion clay air purification particles with sufficient calcination and excellent performance are achieved, which improves its air flux performance and avoids performance degradation caused by excessive or short sintering time.
Smart Images

Figure CN118637897B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of negative ion particle preparation, and in particular to a method for preparing negative ion clay air purification particles. Background Art
[0002] Negative ions refer to ions with negative charges, also known as negatively charged ions. Negative ions have the function of absorbing and decomposing smoke, pollen and harmful gases in the air, and can also kill bacteria, viruses and other microorganisms in the air. Negative ion clay particles refer to a granular material made by mixing clay with negative ion powder. It has good air purification, deodorization and sterilization functions, and can improve human health and environmental quality.
[0003] In the preparation process of negative ion clay air purification particles, the dehydrated product needs to be dried and then calcined at a constant temperature to obtain negative ion clay particles. In the process preparation process, the sintering time needs to be strictly controlled. If the sintering time is too long, it may cause the clay particles to deform and break, and even cause the material to decompose and inactivate to a certain extent, reducing the activity and purification ability of the negative ion clay particles; if the sintering time is too short, the bonding force between the prepared clay particles is weak, and a dense particle structure and a good pore structure cannot be fully formed, which affects the air flux performance of the negative ion clay particles. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a method for preparing negative ion clay air purification particles to solve the existing problems.
[0005] The preparation method of negative ion clay air purification particles of the present invention adopts the following technical scheme:
[0006] The present invention provides a method for preparing negative ion clay air purification particles, the method comprising the following steps:
[0007] (1) Preparing a mixed powder: weighing raw materials active catalyst, boron nitride, titanium oxide, silicon dioxide, graphene, medical stone natural ore, aluminum oxide, zirconium oxide, and magnesium oxide according to the mass ratio, making each raw material into ultrafine powder and mixing them evenly to obtain a mixed powder;
[0008] (2) Preparing a mixture 1: adding the mixed powder obtained in step (1) into an aqueous solution of polyvinyl alcohol to obtain a mixture 1;
[0009] (3) Preparing mixture 2: adding sticky kaolin to the mixture 1 obtained in step (2), and mixing well to obtain mixture 2;
[0010] (4) Preparing negative ion clay air purification particles: dehydrating the mixture 2 obtained in step (3) to obtain a dehydrated product, and then drying the dehydrated product and calcining it at a constant temperature;
[0011] Collect infrared thermal imaging images during the constant temperature calcination process; set the neighborhood window of each pixel point in the infrared thermal imaging image; obtain the different temperature point characteristic factor, thermal boundary characteristic factor and neighborhood characteristic factor of each neighborhood window according to the edge characteristics and corner point characteristics of the pixel points in the infrared thermal imaging image; obtain each response cluster in the infrared thermal imaging image by combining the different temperature point characteristic factor, thermal boundary characteristic factor and neighborhood characteristic factor; obtain the calcination sufficiency coefficient of each response cluster according to the distribution characteristics of the pixel points in each response cluster; use the calcination sufficiency coefficient to complete the constant temperature calcination of the dehydrated product to obtain negative ion clay air purification particles.
[0012] Preferably, in step (1), 1 to 5 parts of raw material active catalyst, 3 to 5 parts of boron nitride, 1 to 5 parts of titanium oxide, 30 to 35 parts of silicon dioxide, 1 to 2 parts of graphene, 1 to 4 parts of medical stone natural ore, 20 to 25 parts of aluminum oxide, 5 to 10 parts of zirconium oxide, and 10 to 15 parts of magnesium oxide are weighed according to the mass ratio.
[0013] Preferably, the active catalyst in step (1) is one of lanthanum oxide, praseodymium oxide and rubidium oxide.
[0014] Preferably, in step (2), the mass ratio of polyvinyl alcohol to mixed powder is 1-5:15.
[0015] Preferably, the mass ratio of the sticky kaolin in step (3) to the mixture 1 is 4-10:30.
[0016] Preferably, the sintering temperature of the constant temperature calcination in step (4) is 1000-1100°C.
[0017] Preferably, the step of obtaining the different-temperature point characteristic factor, the thermal boundary characteristic factor and the neighborhood characteristic factor of each neighborhood window according to the edge characteristics and corner point characteristics of the pixel points in the infrared thermal imaging image includes:
[0018] For the neighborhood window of each pixel point in the infrared thermal imaging image, the temperature values of all pixels in the neighborhood window are arranged in ascending order as the neighborhood temperature sequence of the neighborhood window, the first quartile and the third quartile of the neighborhood temperature sequence are obtained, and the metric distance between the corner point j in the neighborhood window and the remaining corner points is calculated, and the corner point corresponding to the maximum value of the metric distance is obtained. , and the corner point j is connected to the corner point The two-tuple composed of the temperature values of is taken as the long-range two-tuple of the corner point j, and each boundary in the neighborhood window is extracted and recorded as each thermal boundary. The temperature values of all pixels on each thermal boundary are arranged in ascending order as the boundary temperature sequence of each thermal boundary;
[0019] Calculate the absolute value of the difference between the temperature value of each corner point in the neighborhood window and the average temperature value of all pixels in the neighborhood window, calculate the sum of the absolute values of the difference of all corner points, record it as the first sum, calculate the cosine similarity of the long-distance binary of each corner point in the neighborhood window and the remaining other corner points, calculate the sum of all the cosine similarities of all corner points, record it as the second sum, calculate the sum of the second sum and the preset first adjustment parameter, record it as the third sum, calculate the ratio of the first sum to the third sum, and use the product of the number of corner points in the neighborhood window and the ratio as the characteristic factor of the different temperature points of each neighborhood window;
[0020] Thermal boundary characteristic factor of the i-th neighborhood window The expression is:
[0021]
[0022] In the formula, is the total number of hot boundary pixels in the i-th neighborhood window, is the total number of thermal boundaries in the i-th neighborhood window; , are the boundary temperature sequences corresponding to the pth and qth thermal boundaries in the i-th neighborhood window, respectively. is the DTW distance, is to preset a second adjustment parameter;
[0023] The information entropy of the neighborhood temperature sequence of each neighborhood window is calculated, the absolute value of the difference between the first quartile and the third quartile of each neighborhood window is calculated, recorded as the first difference absolute value, and the product of the information entropy and the first difference absolute value is used as the neighborhood characteristic factor of each neighborhood window.
[0024] Preferably, the step of combining the different temperature point characteristic factors, the thermal boundary characteristic factors and the neighborhood characteristic factors to obtain the response clusters in the infrared thermal imaging image includes:
[0025] The different-temperature point characteristic factors, thermal boundary characteristic factors and neighborhood characteristic factors of each neighborhood window are used as the different-temperature point characteristic factors, thermal boundary characteristic factors and neighborhood characteristic factors of the central pixel points of each neighborhood window. The RSM response surface analysis method is used to obtain the response values corresponding to the different-temperature point characteristic factors, thermal boundary characteristic factors and neighborhood characteristic factors of each pixel point. All pixel points with response values greater than the preset segmentation threshold are used as the input of the clustering algorithm, and the output is each response cluster.
[0026] Preferably, the calcination sufficiency coefficient of each response cluster is obtained according to the distribution characteristics of the pixels in each response cluster, including:
[0027] The local outlier factor of each pixel in each response cluster is calculated, the response values of all pixels in each response cluster are arranged in ascending order as the response sequence of each response cluster, and the infrared thermal imaging image is recorded as the calcination image;
[0028] Calcination deficiency factor of the xth response cluster in the calcination image at the tth acquisition time The expression is:
[0029]
[0030] In the formula, is the total number of pixels in the xth response cluster in the calcination image at the tth acquisition time, , are the local outlier factor of the response value corresponding to the mth pixel in the xth response cluster in the calcination image at the tth acquisition time, and the mean of the local outlier factors corresponding to all the response values in the xth response cluster, respectively. is the total number of response clusters in the calcination image at the tth acquisition time, , are the mean response values of all pixels in the xth and yth response clusters in the calcination image at the tth acquisition time, is to preset a third adjustment parameter;
[0031] The expression of the calcination sufficiency coefficient of each response cluster in the calcination image at each acquisition time is:
[0032]
[0033] In the formula, is the calcination sufficiency coefficient of the xth response cluster in the calcination image at the tth acquisition time, , are the response sequences of the xth and yth response clusters in the calcination image at the tth acquisition time, is the Hausdorff distance, It is the preset fourth adjustment parameter.
[0034] Preferably, the method of using the calcination sufficiency coefficient to complete the constant temperature calcination of the dehydrated product comprises:
[0035] The pixel point with the largest response value in each response cluster is used as the response center point of each response cluster, the response center point with the largest response value in the calcination image is used as the calcination center point of the calcination image, the Euclidean distance between each response center point and the calcination center point is calculated, the sum of the Euclidean distance and a preset fifth adjustment parameter is calculated, the ratio of the calcination sufficiency coefficient of each response cluster to the sum is calculated, and the normalized value of the sum of the ratios of all response clusters is used as the calcination sufficiency of the calcination image at each acquisition time;
[0036] If the calcination degree of the calcination image at the time of acquisition is less than the preset calcination degree threshold, the sintering time of the dehydrated product is extended by the preset time. Otherwise, the constant temperature calcination of the dehydrated product is stopped. If the sintering time reaches the preset calcination stop time, the constant temperature calcination is stopped.
[0037] The present invention has at least the following beneficial effects:
[0038] The invention obtains the characteristic factor of the different temperature point, the characteristic factor of the thermal boundary and the characteristic factor of the neighborhood according to the temperature difference characteristics in the neighborhood window of each pixel point in the calcination image, comprehensively considers the temperature abnormal point characteristics, the thermal boundary characteristics and the neighborhood temperature difference characteristics caused by insufficient calcination of the dehydrated product, and obtains the response value of each pixel point based on the above characteristics, which more accurately reflects the temperature abnormality caused by insufficient calcination at the position of the pixel point; clusters the calcination image according to the response value, obtains the calcination sufficiency of the calcination image at each acquisition time through the response value characteristics of the response clustering cluster, comprehensively considers the differences between different response clustering clusters in the calcination image on the basis of analyzing the response value characteristics in all response clustering clusters in the calcination image, can more accurately reflect the sintering sufficiency of the dehydrated product in the calcination image, and then judges the calcination sufficiency of the dehydrated product based on the calcination sufficiency, realizes the adaptive adjustment of the sintering time according to the calcination status of the dehydrated product, obtains the negative ion clay air purification particles with sufficient calcination and good performance, and improves the air flux performance of the negative ion clay particles. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the technical solutions and advantages in the embodiments of the present invention or the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0040] Figure 1 A flowchart of the steps of a method for preparing negative ion clay air purification particles;
[0041] Figure 2 A flow chart for the process of preparing negative ion clay air purification particles;
[0042] Figure 3 Construct a flow chart for the constant temperature calcination indicator. DETAILED DESCRIPTION
[0043] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the following is a detailed description of the preparation method of a negative ion clay air purification particle proposed by the present invention, its specific implementation method, structure, characteristics and effects, in combination with the accompanying drawings and preferred embodiments. In the following description, different "one embodiment" or "another embodiment" does not necessarily refer to the same embodiment. In addition, specific features, structures or characteristics in one or more embodiments may be combined in any suitable form.
[0044] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.
[0045] The specific scheme of the preparation method of the negative ion clay air purification particles provided by the present invention is described in detail below with reference to the accompanying drawings.
[0046] Example 1
[0047] Example 1 provides a method for preparing negative ion clay air purification particles. For a flowchart of the steps, please refer to Figure 1 , the specific preparation process is as follows:
[0048] (1) Preparing a mixed powder: weighing 1 part of lanthanum oxide, 3 parts of boron nitride, 1 part of titanium oxide, 30 parts of silicon dioxide, 1 part of graphene, 1 part of medical stone natural ore, 20 parts of aluminum oxide, 5 parts of zirconium oxide, and 10 parts of magnesium oxide according to the mass ratio, making each raw material into ultrafine powder and then mixing them uniformly to obtain a mixed powder;
[0049] (2) Preparing mixture 1: adding the mixed powder prepared in step (1) into an aqueous solution of polyvinyl alcohol to soak the mixed powder in a mass ratio of polyvinyl alcohol to mixed powder of 1:15 to obtain mixture 1;
[0050] (3) Preparing mixture 2: adding viscous kaolin to mixture 1 in the mass ratio of viscous kaolin to mixture 1 to be 4:30, and mixing evenly to obtain mixture 2;
[0051] (4) Preparation of negative ion clay air purification particles: Dehydrating the mixture 2 obtained in step (3) to obtain a dehydrated product, drying the dehydrated product and calcining it at a constant temperature of 1000° C. for 45 to 120 min;
[0052] Step S001, collecting infrared thermal imaging images of the dehydrated product during the constant temperature calcination process, and performing pre-processing.
[0053] The infrared image of the dehydrated product during the constant temperature calcination process is collected from a top-down angle by an infrared imager. The initial collection time is set to the 45th minute after the dehydrated product is calcined at a constant temperature, and the collection time interval is set to 1 minute. In order to enhance the edge and detail features in the image and facilitate subsequent analysis, the collected constant temperature calcination infrared thermal imaging image needs to be sharpened preprocessed. The preprocessing algorithm used in this embodiment is Gaussian filtering. The implementer can select other algorithms to preprocess the constant temperature calcination infrared thermal imaging image according to actual conditions. Gaussian filtering is an existing well-known technology and will not be described in detail in this embodiment.
[0054] At this point, the time-series infrared thermal imaging images of the dehydrated product during constant temperature calcination can be obtained. For the convenience of subsequent description, the acquired images are recorded as calcination images.
[0055] Step S002, obtaining the temperature difference factor of the different temperature points, the thermal boundary factor and the neighborhood factor according to the temperature difference characteristics in the neighborhood window of each pixel point in the calcination image, and thereby obtaining the response value of each pixel point, clustering the calcination image according to the response value, and obtaining the calcination sufficiency of the calcination image according to the response value characteristics of the response clustering cluster.
[0056] Specifically, this embodiment collects infrared thermal imaging images of the dehydration product during the constant temperature calcination process; sets a neighborhood window for each pixel point in the infrared thermal imaging image; obtains the different temperature point characteristic factor, thermal boundary characteristic factor and neighborhood characteristic factor of each neighborhood window according to the edge characteristics and corner point characteristics of the pixel points in the infrared thermal imaging image; obtains each response cluster in the infrared thermal imaging image by combining the different temperature point characteristic factor, thermal boundary characteristic factor and neighborhood characteristic factor; obtains the calcination sufficiency coefficient of each response cluster according to the distribution characteristics of the pixel points in each response cluster; uses the calcination sufficiency coefficient to complete the constant temperature calcination of the dehydration product to obtain negative ion clay air purification particles. The negative ion clay air purification particle process preparation flow chart is shown in FIG. Figure 2 As shown, the constant temperature calcination index construction flow chart is as follows Figure 3 The specific construction process of the calcination sufficiency of the calcination image at each acquisition time is as follows:
[0057] In the calcination image, if the constant temperature calcination time of the dehydrated product is not properly controlled, more abnormal temperature points will be generated in the calcination image, including high temperature abnormal points and low temperature abnormal points; secondly, in the surrounding area of the temperature abnormal point, a more obvious thermal boundary will be generated due to the temperature difference between the temperature abnormal point and the surrounding environment, and when the temperature difference changes greatly, there will be multiple thermal boundaries in the area centered on the temperature abnormal point. The longer the thermal boundary is, the more uneven the sintering reaction of the dehydrated product is. At this time, the sintering time should be extended to make the sintering reaction of the dehydrated product more sufficient and complete, so as to ensure the performance of the negative ion clay particles.
[0058] The calcination image at the tth acquisition time is now taken as an example for subsequent analysis. First, all thermal boundaries and corner points in the calcination image are obtained respectively through the edge detection algorithm based on the Canny operator and the Harris corner detection algorithm. Since the corner points are points that are greatly different from the surrounding environment, they are temperature abnormality points in the calcination image. A neighborhood window is constructed with each pixel point in the calcination image as the center. In this embodiment, the size of the neighborhood window is 7*7. The implementer can set it according to the actual situation. This embodiment does not limit this. The temperature values of all pixels in the neighborhood window are arranged in ascending order as the neighborhood temperature sequence of the neighborhood window, which is recorded as , calculate the neighborhood temperature sequence corresponding to each neighborhood window The first quartile and the third quartile of , ; Calculate the Manhattan distance between all corner points in the neighborhood window, record the corner point farthest from the jth corner point as the distant corner point of the corner point, and take the temperature value of the jth corner point and the temperature value of the distant corner point corresponding to the jth corner point as the distant binary group of the jth corner point ; Arrange the temperature values of all pixels on each thermal boundary in the neighborhood window in ascending order as the boundary temperature sequence of each thermal boundary, recorded as , all pixels on the thermal boundary are recorded as thermal boundary pixels.
[0059] Based on the above analysis, this embodiment constructs the different temperature point characteristic factor, thermal boundary characteristic factor and neighborhood characteristic factor based on the neighborhood window respectively, which are used to characterize the temperature difference condition within the neighborhood window. The expression is:
[0060]
[0061]
[0062]
[0063] In the formula, is the characteristic factor of the different temperature points in the i-th neighborhood window, is the total number of corner points in the i-th neighborhood window, , are the temperature value of the jth corner point in the ith neighborhood window and the mean temperature of all pixels in the ith neighborhood window, respectively. , are the long-distance binary pairs corresponding to the jth and fth corner points in the i-th neighborhood window, respectively. Long-distance binary and The cosine similarity between To preset the first adjustment parameter to prevent the denominator from being 0, in this embodiment The implementer can set it according to the actual situation. This embodiment does not limit it. Denoted as the first sum, Denoted as the second sum, Recorded as the third sum;
[0064] is the thermal boundary characteristic factor of the i-th neighborhood window, is the total number of hot boundary pixels in the i-th neighborhood window, is the total number of thermal boundaries in the i-th neighborhood window; , are the boundary temperature sequences corresponding to the pth and qth thermal boundaries in the i-th neighborhood window, respectively. is the DTW distance, To preset the second adjustment parameter to prevent the denominator from being 0, in this embodiment , the implementer can set it according to the actual situation, and this embodiment does not limit it. The calculation of DTW distance is an existing well-known technology, and this embodiment will not be described in detail here;
[0065] is the neighborhood characteristic factor of the i-th neighborhood window, is the information entropy of the neighborhood temperature sequence corresponding to the i-th neighborhood window, , are the first quartile and the third quartile of the neighborhood temperature series corresponding to the i-th neighborhood window, respectively. Recorded as the absolute value of the first difference.
[0066] When the number of corner points in the i-th neighborhood window is large, that is, The larger the value is, the more temperature points in the ith neighborhood window have large temperature differences with the surrounding environment; at the same time, when the sum of the absolute values of the differences between the temperature values of all corner points in the ith neighborhood window and the mean temperature of all pixels in the neighborhood window is larger, that is, The larger the value, the greater the difference between the temperature of all corner points in the i-th neighborhood window, that is, the temperature anomaly point and the average temperature condition in the neighborhood window; at the same time, when the sum of the cosine similarities between the long-distance binary groups corresponding to all corner points in the i-th neighborhood window is smaller, that is The smaller it is, the greater the difference between the long-distance binary groups of all corner points in the i-th neighborhood window, the more significant the temperature difference between the corner points in the i-th neighborhood window, and the higher the characteristic factor of the heterothermal point. The bigger.
[0067] When the total number of hot boundary pixels in the i-th neighborhood window is larger, that is, The larger the value is, the more significant the temperature difference is at the corresponding position of the calcination image in the i-th neighborhood window. At the same time, when the DTW sum distance between the boundary temperature sequences corresponding to all thermal boundaries in the i-th neighborhood window is larger, that is, The larger the value, the greater the temperature difference between all thermal boundaries in the i-th neighborhood window, the more significant the temperature difference at the corresponding position of the i-th neighborhood window, and the larger the thermal boundary characteristic factor. The bigger.
[0068] When the information entropy of the neighborhood temperature sequence corresponding to the i-th neighborhood window is larger, that is, The larger the value, the greater the fluctuation of the temperature values of all pixels in the ith neighborhood window. At the same time, when the difference between the first quartile of the neighborhood temperature sequence corresponding to the ith neighborhood window and the third quartile of the neighborhood temperature sequence is greater, that is, The larger the value is, the larger the interquartile range of the neighborhood temperature sequence corresponding to the i-th neighborhood window is, the more drastic the temperature change at the corresponding position of the i-th neighborhood window is, and the neighborhood characteristic factor of the i-th neighborhood window is The bigger.
[0069] At this point, the different temperature point characteristic factors, thermal boundary characteristic factors and neighborhood characteristic factors of all neighborhood windows in the calcination image at the t-th acquisition time can be obtained, and the different temperature point characteristic factors, thermal boundary characteristic factors and neighborhood characteristic factors are assigned to the central pixel of the corresponding neighborhood window. The different temperature point characteristic factors, thermal boundary characteristic factors and neighborhood characteristic factors of the pixel points are used as independent variables, and the RSM response surface method (Response Surface Methodology) is used to obtain the response value of each pixel point in the calcination image. The functional relationship in the RSM response surface method is: the larger the different temperature point characteristic factors, thermal boundary characteristic factors and neighborhood characteristic factors, the larger the response value; and when the response value is larger, it means that the temperature abnormality caused by insufficient calcination in the neighborhood range at the corresponding position of the pixel point is more significant. The RSM response surface method is an existing well-known technology, and this embodiment will not be described in detail here.
[0070] The response values of all pixels in the calcined image are arranged in ascending order as the temperature response sequence of the calcined image, and the segmentation threshold of the temperature response sequence is obtained by the OTSU method. The pixel points in the calcined image whose response values are greater than the segmentation threshold are recorded as temperature response points in the calcined image. All temperature response points are used as inputs of the Chameleon clustering algorithm. The Chameleon clustering algorithm is used to obtain each clustering cluster in the calcined image, and the absolute value of the difference in response values between the temperature response points is used as the metric distance. Since the OTSU method and the Chameleon clustering algorithm are both existing well-known technologies, they are not described in detail in this embodiment.
[0071] At this point, each response cluster in the calcined image at each acquisition time can be obtained according to the above method. The calcined image at the tth acquisition time is still taken as an example for subsequent analysis. The response values of all pixels in each response cluster in the calcined image are used as input, and the LOF outlier detection algorithm (Local Outlier Factor) is used to obtain the local outlier factor of each pixel in each response cluster, which is recorded as Lof, wherein the neighborhood distance is determined by the cross-validation method (Cross-Validation). Since the LOF outlier detection algorithm and the cross-validation method are both existing well-known technologies, this embodiment will not be described in detail here.
[0072] The pixel with the largest response value in each response cluster in the calcination image is taken as the response center point of the response cluster, denoted as , the response center point with the largest response value in the calcination image is recorded as the calcination center point of the calcination image, recorded as ; Arrange the response values of all pixels in each response cluster in the calcination image in ascending order as the response sequence of each response cluster, denoted as M.
[0073] Based on the above analysis, this example constructs the calcination sufficiency to characterize the sintering sufficiency of the dehydrated product, and the expression is:
[0074]
[0075]
[0076]
[0077] In the formula, is the calcination deficiency factor of the xth response cluster in the calcination image at the tth acquisition time, is the total number of pixels in the xth response cluster in the calcination image at the tth acquisition time, , are the local outlier factor of the response value corresponding to the mth pixel in the xth response cluster in the calcination image at the tth acquisition time, and the mean of the local outlier factors corresponding to all the response values in the xth response cluster, respectively. is the total number of response clusters in the calcination image at the tth acquisition time, , are the mean response values of all pixels in the xth and yth response clusters in the calcination image at the tth acquisition time, To preset the third adjustment parameter to prevent the denominator from being 0, in this embodiment , the implementer can set it according to the actual situation, and this embodiment does not limit it;
[0078] is the calcination sufficiency coefficient of the xth response cluster in the calcination image at the tth acquisition time, , are the response sequences of the xth and yth response clusters in the calcination image at the tth acquisition time, is the Hausdorff distance, To preset the fourth adjustment parameter to prevent the denominator from being 0, in this embodiment , the implementer can set it according to the actual situation, and this embodiment does not limit it. The calculation of Hausdorff distance is a well-known technology, and this embodiment will not be described in detail here;
[0079] is the calcination sufficiency of the calcination image at the tth acquisition time, , are respectively the response center point of the xth response cluster in the calcination image at the tth acquisition time and the calcination center point of the calcination image at the tth acquisition time, Respond to the center point Calcination center The Euclidean distance between To preset the fifth adjustment parameter to prevent the denominator from being 0, in this embodiment , the implementer can set it according to the actual situation, and this embodiment does not limit it. is a normalization function, so that The value range of is in the range of [0,1].
[0080] When the sum of the absolute values of the differences between the local outlier factors of the response values of each pixel in the xth response cluster in the calcination image at the tth acquisition time and the mean of the local outlier factors of all response values in the response cluster is smaller, that is, The smaller it is, the milder the temperature anomaly at the corresponding position of the response cluster is; at the same time, when the sum of the absolute values of the difference between the mean response values of all pixels in the xth response cluster in the calcination image at the tth acquisition time and the mean response values corresponding to all other response clusters in the calcination image is larger, that is, The larger the value, the greater the difference between the response cluster and the other response clusters. The more obvious the temperature anomaly caused by insufficient calcination in the calcination image at the tth acquisition time is, and the calcination deficiency factor is The bigger.
[0081] When the Hausdorff distance between the response sequences corresponding to the xth response cluster in the calcined image at the tth acquisition time and all other response clusters in the calcined image is smaller, that is, The smaller it is, the smaller the difference between all the response clusters in the calcination image at the tth acquisition time is; at the same time, when the calcination deficiency factor of the xth response cluster in the calcination image at the tth acquisition time is smaller, that is, The smaller it is, the less abnormal temperature is caused by insufficient calcination at the corresponding position of the xth response cluster in the calcination image at the tth acquisition time, and the calcination sufficiency coefficient of the response cluster is The bigger.
[0082] When the sum of the calcination sufficiency coefficients of all the response clusters in the calcination image at the tth acquisition time is larger, that is, The larger the value is, the more complete the calcination reaction of the dehydration product is at the tth acquisition time. At the same time, when the sum of the Euclidean distances between the response center points of all response clusters in the calcination image at the tth acquisition time and the calcination center point corresponding to the calcination image is smaller, that is, When the value is larger, it means that the spatial distribution of each response cluster in the calcination image at the tth acquisition time is more concentrated, the temperature abnormality change range of the dehydrated product caused by insufficient calcination at the tth acquisition time is smaller, the calcination reaction degree of the dehydrated product is greater, and the calcination degree is greater. The bigger.
[0083] At this point, the calcination sufficiency of the calcination image at each acquisition moment can be obtained according to the above method, which is used for subsequent adaptive adjustment of the sintering time to obtain negative ion clay particles that are fully calcined and have good performance.
[0084] Step S003, adaptively controlling the sintering time in the calcination process according to the calcination sufficiency, and completing the preparation of negative ion clay air purification particles.
[0085] Set the calcination sufficient threshold Z, in this embodiment , the implementer can set it according to the actual situation, and this embodiment does not limit it. When the calcination degree of the calcination image is less than the calcination sufficient threshold, the sintering time of the dehydrated product is extended by 1 minute until the calcination degree of the calcination image is greater than or equal to the calcination sufficient threshold Z or the sintering time reaches 120 minutes, and then the constant temperature calcination is stopped.
[0086] Example 2
[0087] Example 2 provides a method for preparing negative ion clay air purification particles. For a flowchart of the steps, please refer to Figure 1 , the specific preparation process is as follows:
[0088] (1) Preparing a mixed powder: weighing 5 parts of raw materials of praseodymium oxide, 5 parts of boron nitride, 5 parts of titanium oxide, 35 parts of silicon dioxide, 2 parts of graphene, 4 parts of medical stone natural ore, 25 parts of aluminum oxide, 10 parts of zirconium oxide, and 15 parts of magnesium oxide according to the mass ratio, making each raw material into ultrafine powder and then mixing them uniformly to obtain a mixed powder;
[0089] (2) Preparing mixture 1: adding the mixed powder prepared in step (1) into an aqueous solution of polyvinyl alcohol in a mass ratio of polyvinyl alcohol to mixed powder of 5:15 to obtain mixture 1;
[0090] (3) Preparing mixture 2: adding viscous kaolin to mixture 1 in a mass ratio of viscous kaolin to mixture 1 of 10:30, and mixing evenly to obtain mixture 2;
[0091] (4) Preparation of negative ion clay air purification particles: Dehydrating the mixture 2 obtained in step (3) to obtain a dehydrated product, drying the dehydrated product and calcining it at a constant temperature of 1100° C. for 45 to 120 min;
[0092] The infrared thermal imaging image acquisition process during the constant temperature calcination process is the same as in Example 1, and negative ion clay air purification particles are obtained.
[0093] Example 3
[0094] Example 3 provides a method for preparing negative ion clay air purification particles. For a flowchart of the steps, please refer to Figure 1 , the specific process is as follows:
[0095] (1) Preparing a mixed powder: weighing raw materials of rubidium oxide 3 parts, boron nitride 4 parts, titanium oxide 3 parts, silicon dioxide 32 parts, graphene 1 part, medical stone natural ore 2 parts, aluminum oxide 22 parts, zirconium oxide 8 parts, and magnesium oxide 12 parts according to the mass ratio, making each raw material into ultrafine powder and mixing them uniformly to obtain a mixed powder;
[0096] (2) Preparing mixture 1: adding the mixed powder prepared in step (1) into an aqueous solution of polyvinyl alcohol in a mass ratio of polyvinyl alcohol to mixed powder of 2:15 to obtain mixture 1;
[0097] (3) Preparing mixture 2: adding viscous kaolin to mixture 1 in the mass ratio of viscous kaolin to mixture 1 to be 6:30, and mixing evenly to obtain mixture 2;
[0098] (4) Preparation of negative ion clay air purification particles: Dehydrate the mixture 2 obtained in step (3) to obtain a dehydrated product, dry the dehydrated product and calcine it at 1020° C. for 45 to 120 min; the infrared thermal imaging image acquisition process during the constant temperature calcination process is the same as that in Example 1, to obtain negative ion clay air purification particles.
[0099] Comparative Example 1
[0100] (1) Preparing a mixed powder: weighing 1 part of lanthanum oxide, 3 parts of boron nitride, 1 part of titanium oxide, 30 parts of silicon dioxide, 1 part of graphene, 1 part of medical stone natural ore, 20 parts of aluminum oxide, 5 parts of zirconium oxide, and 10 parts of magnesium oxide according to the mass ratio, making each raw material into ultrafine powder and then mixing them uniformly to obtain a mixed powder;
[0101] (2) Preparing mixture 1: adding the mixed powder prepared in step (1) into an aqueous solution of polyvinyl alcohol to soak the mixed powder in a mass ratio of polyvinyl alcohol to mixed powder of 1:15 to obtain mixture 1;
[0102] (3) Preparing mixture 2: adding viscous kaolin to mixture 1 in the mass ratio of viscous kaolin to mixture 1 to be 4:30, and mixing evenly to obtain mixture 2;
[0103] (4) Preparation of negative ion clay air purification particles: Dehydrate the mixture 2 obtained in step (3) to obtain a dehydrated product, dry the dehydrated product and calcine it at 1000° C. for 90 min to obtain negative ion clay air purification particles.
[0104] Comparative Example 2
[0105] (1) Preparing a mixed powder: weighing 5 parts of raw materials of praseodymium oxide, 5 parts of boron nitride, 5 parts of titanium oxide, 35 parts of silicon dioxide, 2 parts of graphene, 4 parts of medical stone natural ore, 25 parts of aluminum oxide, 10 parts of zirconium oxide, and 15 parts of magnesium oxide according to the mass ratio, making each raw material into ultrafine powder and then mixing them uniformly to obtain a mixed powder;
[0106] (2) Preparing mixture 1: adding the mixed powder prepared in step (1) into an aqueous solution of polyvinyl alcohol in a mass ratio of polyvinyl alcohol to mixed powder of 5:15 to obtain mixture 1;
[0107] (3) Preparing mixture 2: adding viscous kaolin to mixture 1 in a mass ratio of viscous kaolin to mixture 1 of 10:30, and mixing evenly to obtain mixture 2;
[0108] (4) Preparation of negative ion clay air purification particles: Dehydrate the mixture 2 obtained in step (3) to obtain a dehydrated product, dry the dehydrated product and calcine it at 1100° C. for 90 min to obtain negative ion clay air purification particles.
[0109] Comparative Example 3
[0110] (1) Preparing a mixed powder: weighing raw materials of rubidium oxide 3 parts, boron nitride 4 parts, titanium oxide 3 parts, silicon dioxide 32 parts, graphene 1 part, medical stone natural ore 2 parts, aluminum oxide 22 parts, zirconium oxide 8 parts, and magnesium oxide 12 parts according to the mass ratio, making each raw material into ultrafine powder and mixing them uniformly to obtain a mixed powder;
[0111] (2) Preparing mixture 1: adding the mixed powder prepared in step (1) into an aqueous solution of polyvinyl alcohol in a mass ratio of polyvinyl alcohol to mixed powder of 2:15 to obtain mixture 1;
[0112] (3) Preparing mixture 2: adding viscous kaolin to mixture 1 in the mass ratio of viscous kaolin to mixture 1 to be 6:30, and mixing evenly to obtain mixture 2;
[0113] (4) Preparation of negative ion clay air purification particles: Dehydrate the mixture 2 obtained in step (3) to obtain a dehydrated product, dry the dehydrated product and calcine it at 1020° C. for 90 min to obtain negative ion clay air purification particles.
[0114] The air flux of the negative ion clay air purification particles prepared in Examples 1 to 3 and Comparative Examples 1 to 3 was tested, wherein the test environment was a pressure of 0.1 MPa and a temperature of 25°C. The test method was to calculate the air flux of the air flowing through 1 m in 1 hour. 2 The amount of negative ion clay air purification particles, the test results are shown in Table 1.
[0115] Table 1 Air flux test results
[0116]
[0117] In summary, the present invention solves the problem of poor performance caused by improper sintering time control in the preparation process of negative ion clay air purification particles. Combined with the edge and corner point features of pixel points in the calcined image, the sintering time is adaptively controlled to improve the air flux performance of the negative ion clay particles.
[0118] It should be noted that the sequence of the above embodiments of the present invention is only for description and does not represent the advantages and disadvantages of the embodiments. The above is a description of a specific embodiment of this specification. In addition, the processes depicted in the accompanying drawings do not necessarily require the specific order or continuous order shown to achieve the desired results. In some embodiments, multitasking and parallel processing are also possible or may be advantageous.
[0119] The various embodiments in this specification are described in a progressive manner, and the same or similar parts between the various embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.
[0120] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing negative ion clay air purification particles, characterized in that: The method comprises the following steps: (1) Preparing a mixed powder: weighing raw materials active catalyst, boron nitride, titanium oxide, silicon dioxide, graphene, medical stone natural ore, aluminum oxide, zirconium oxide, and magnesium oxide according to the mass ratio, making each raw material into ultrafine powder and mixing them evenly to obtain a mixed powder; (2) Preparing a mixture 1: adding the mixed powder obtained in step (1) into an aqueous solution of polyvinyl alcohol to obtain a mixture 1; (3) Preparing mixture 2: adding sticky kaolin to the mixture 1 obtained in step (2), and mixing well to obtain mixture 2; (4) Preparing negative ion clay air purification particles: dehydrating the mixture 2 obtained in step (3) to obtain a dehydrated product, and then drying the dehydrated product and calcining it at a constant temperature; Collect infrared thermal imaging images during the constant temperature calcination process; set the neighborhood window of each pixel point in the infrared thermal imaging image; obtain the different temperature point characteristic factor, thermal boundary characteristic factor and neighborhood characteristic factor of each neighborhood window according to the edge characteristics and corner point characteristics of the pixel points in the infrared thermal imaging image; obtain each response cluster in the infrared thermal imaging image by combining the different temperature point characteristic factor, thermal boundary characteristic factor and neighborhood characteristic factor; obtain the calcination sufficiency coefficient of each response cluster according to the distribution characteristics of the pixel points in each response cluster; use the calcination sufficiency coefficient to complete the constant temperature calcination of the dehydrated product to obtain negative ion clay air purification particles; The method of obtaining the different-temperature point characteristic factor, thermal boundary characteristic factor and neighborhood characteristic factor of each neighborhood window according to the edge characteristics and corner point characteristics of the pixel points in the infrared thermal imaging image includes: For the neighborhood window of each pixel point in the infrared thermal imaging image, the temperature values of all pixels in the neighborhood window are arranged in ascending order as the neighborhood temperature sequence of the neighborhood window, the first quartile and the third quartile of the neighborhood temperature sequence are obtained, and the metric distance between the corner point j in the neighborhood window and the remaining corner points is calculated, and the corner point corresponding to the maximum value of the metric distance is obtained. , and the corner point j is connected to the corner point The two-tuple composed of the temperature values of is taken as the long-range two-tuple of the corner point j, and each boundary in the neighborhood window is extracted and recorded as each thermal boundary. The temperature values of all pixels on each thermal boundary are arranged in ascending order as the boundary temperature sequence of each thermal boundary; Calculate the absolute value of the difference between the temperature value of each corner point in the neighborhood window and the average temperature value of all pixels in the neighborhood window, calculate the sum of the absolute values of the difference of all corner points, record it as the first sum, calculate the cosine similarity of the long-distance binary of each corner point in the neighborhood window and the remaining other corner points, calculate the sum of all the cosine similarities of all corner points, record it as the second sum, calculate the sum of the second sum and the preset first adjustment parameter, record it as the third sum, calculate the ratio of the first sum to the third sum, and use the product of the number of corner points in the neighborhood window and the ratio as the characteristic factor of the different temperature points of each neighborhood window; Thermal boundary characteristic factor of the i-th neighborhood window The expression is: In the formula, is the total number of hot boundary pixels in the i-th neighborhood window, is the total number of thermal boundaries in the i-th neighborhood window; , are the boundary temperature sequences corresponding to the pth and qth thermal boundaries in the i-th neighborhood window, respectively. is the DTW distance, is to preset a second adjustment parameter; Calculate the information entropy of the neighborhood temperature sequence of each neighborhood window, calculate the absolute value of the difference between the first quartile and the third quartile of each neighborhood window, record it as the first absolute value of the difference, and use the product of the information entropy and the first absolute value of the difference as the neighborhood characteristic factor of each neighborhood window; The method of combining the different temperature point characteristic factors, the thermal boundary characteristic factors and the neighborhood characteristic factors to obtain each response cluster in the infrared thermal imaging image includes: The different-temperature point characteristic factor, thermal boundary characteristic factor and neighborhood characteristic factor of each neighborhood window are used as the different-temperature point characteristic factor, thermal boundary characteristic factor and neighborhood characteristic factor of the central pixel of each neighborhood window, and the response value corresponding to the different-temperature point characteristic factor, thermal boundary characteristic factor and neighborhood characteristic factor of each pixel is obtained by RSM response surface analysis method, and all pixel points whose response value is greater than a preset segmentation threshold are used as the input of the clustering algorithm, and the output is each response cluster; The method of obtaining the calcination sufficiency coefficient of each response cluster according to the distribution characteristics of the pixel points in each response cluster comprises: The local outlier factor of each pixel in each response cluster is calculated, the response values of all pixels in each response cluster are arranged in ascending order as the response sequence of each response cluster, and the infrared thermal imaging image is recorded as the calcination image; Calcination deficiency factor of the xth response cluster in the calcination image at the tth acquisition time The expression is: In the formula, is the total number of pixels in the xth response cluster in the calcination image at the tth acquisition time, , are the local outlier factor of the response value corresponding to the mth pixel in the xth response cluster in the calcination image at the tth acquisition time, and the mean of the local outlier factors corresponding to all the response values in the xth response cluster, respectively. is the total number of response clusters in the calcination image at the tth acquisition time, , are the mean response values of all pixels in the xth and yth response clusters in the calcination image at the tth acquisition time, is to preset a third adjustment parameter; The expression of the calcination sufficiency coefficient of each response cluster in the calcination image at each acquisition time is: In the formula, is the calcination sufficiency coefficient of the xth response cluster in the calcination image at the tth acquisition time, , are the response sequences of the xth and yth response clusters in the calcination image at the tth acquisition time, is the Hausdorff distance, is to preset a fourth adjustment parameter; The method of using the calcination sufficiency coefficient to complete the constant temperature calcination of the dehydrated product comprises: The pixel point with the largest response value in each response cluster is used as the response center point of each response cluster, the response center point with the largest response value in the calcination image is used as the calcination center point of the calcination image, the Euclidean distance between each response center point and the calcination center point is calculated, the sum of the Euclidean distance and a preset fifth adjustment parameter is calculated, the ratio of the calcination sufficiency coefficient of each response cluster to the sum is calculated, and the normalized value of the sum of the ratios of all response clusters is used as the calcination sufficiency of the calcination image at each acquisition time; If the calcination degree of the calcination image at the time of acquisition is less than the preset calcination degree threshold, the sintering time of the dehydrated product is extended by the preset time. Otherwise, the constant temperature calcination of the dehydrated product is stopped. If the sintering time reaches the preset calcination stop time, the constant temperature calcination is stopped.
2. The method for preparing negative ion clay air purification particles according to claim 1, characterized in that: In the step (1), 1-5 parts of raw material active catalyst, 3-5 parts of boron nitride, 1-5 parts of titanium oxide, 30-35 parts of silicon dioxide, 1-2 parts of graphene, 1-4 parts of medical stone natural ore, 20-25 parts of aluminum oxide, 5-10 parts of zirconium oxide, and 10-15 parts of magnesium oxide are weighed according to the mass ratio.
3. The method for preparing negative ion clay air purification particles according to claim 1, characterized in that: The active catalyst in step (1) is one of lanthanum oxide, praseodymium oxide and rubidium oxide.
4. The method for preparing negative ion clay air purification particles according to claim 1, characterized in that: In the step (2), the mass ratio of polyvinyl alcohol to mixed powder is 1-5:
15.
5. The method for preparing negative ion clay air purification particles according to claim 1, characterized in that: In the step (3), the mass ratio of the sticky kaolin to the mixture 1 is 4-10:
30.