A ceramic PTC thermistor material and its preparation process
By combining barium titanate doped with niobium and ruthenium and modified silicon boronide, combined with laser treatment and high-temperature sintering technology, the problem of insufficient performance of existing PTC thermistor materials at high temperatures is solved, and ceramic PTC thermal sensitivity is achieved The high Curie temperature, high voltage withstand voltage and high lift-resistance ratio of the resistive material improves the overall performance of the material.
Patent Information
- Application Number
- CN202411103851.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-13
AI Technical Summary
The existing PTC thermistor materials have a large negative temperature coefficient characteristics at high temperatures, and doping technology is difficult to improve the Curie temperature and voltage resistance of the material, resulting in insufficient performance and difficult to promote.
Using barium titanate doped with niobium and ruthenium as the main raw material, the density and resistance characteristics of the material are improved by combining sintering aids, modified silicon boron, binder and dispersant. , form high-performance ceramic PTC thermistor material.
The high Curie temperature, high voltage withstand voltage and high lift-resistance ratio of ceramic PTC thermistor material is realized, which improves the performance of the material and enhances its stability and response speed at high temperatures.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic PTC thermistor materials and relates to a PTC thermistor material and a preparation process thereof. Background Art
[0002] The most notable characteristic of a positive temperature coefficient thermistor (PTC) is that its resistance increases dramatically as the temperature rises. This characteristic makes PTC thermistors ideal for temperature control elements. In a heating element, when the temperature reaches the set value, the PTC resistance increases rapidly, limiting the current flow and reducing the heating power, thereby maintaining the temperature at a stable level. This self-limiting temperature characteristic avoids overheating and damage, and improves the safety of the equipment.
[0003] Positive temperature coefficient thermistors generally include ceramic-based composite PTC materials, organic polymer-based PTC materials, V2O3-based PTC materials and barium titanate-based PTC materials. The matrix of polymer-based PTC materials is a semi-crystalline or amorphous polymer, and the conductive particles are mainly carbon, boron or silicon compounds. These conductive particles are evenly dispersed in the matrix to form a good conductive network, so that the material is semi-conductive at room temperature. The PTC effect is mainly formed because when the temperature rises, the matrix material will expand, causing the conductive network to break, resulting in increased resistance. The disadvantage of polymer-based PTC materials is that they will have a large negative temperature coefficient feature at high temperatures. Ceramic-based PTC materials mainly use ceramics (SiO2, etc.) as the matrix material, and conductive particles (C, etc.) are evenly dispersed in the matrix. The principle of the PTC effect is similar to that of polymer-based PTC materials. As the temperature rises, the matrix material undergoes a phase change, which will cause a volume change, thereby separating the conductive particles and increasing the resistance.
[0004] In the prior art, the PCT strength of thermistor materials and the voltage resistance capability of thermistor materials can be easily reduced by doping technology, so it is difficult to be promoted. Summary of the invention
[0005] The object of the present invention is to provide a PTC thermistor material and a preparation process thereof. The ceramic thermistor material prepared by the present invention has a high Curie temperature, a high withstand voltage, and a high lift-to-resistance ratio, and the obtained ceramic thermistor material has better performance.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] A ceramic PTC thermistor material comprises the following components in parts by weight: 50-70 parts of barium titanate doped with niobium and ruthenium, 5-10 parts of a sintering aid, 10-20 parts of modified borosilicate, 1-3 parts of a dispersant and 4-6 parts of a binder;
[0008] The preparation process of the barium titanate doped with niobium and ruthenium is as follows:
[0009] First, 50-70 parts of barium titanate, 0.1-0.15 parts of niobium oxide powder, and 0.1-0.15 parts of ruthenium oxide powder are dried in an oven, and then ball-milled in a ball mill using anhydrous ethanol as a ball-milling medium to fully mix the powders. The mixed powders are solid-phase sintered at 1100-1200°C for 2-4 hours. After the reaction is completed, the powders are ball-milled and mixed to obtain niobium- and ruthenium-doped barium titanate.
[0010] As a preferred technical solution of the present invention, the preparation process of the modified borosilicate is as follows:
[0011] S21, laser treating silicon boride in a nitrogen atmosphere to obtain pretreated silicon boride;
[0012] S22, at 50-60°C, add glycine and pretreated borosilicate in a ratio of 1:1 by mass to deionized water, ultrasonically treat for 0.5-1h to obtain a uniformly dispersed mixed solution, continue heating to 100-110°C, evaporate the water under stirring, collect the obtained solid and dry it;
[0013] S23, moving the dried solid into a tubular furnace for calcination in high-purity nitrogen at 900-1000° C. for 2-3 hours, cooling to room temperature, and then crushing to obtain the modified borosilicate.
[0014] As a preferred technical solution of the present invention, the sintering aid is one or more of alumina, silica and calcium carbonate.
[0015] As a preferred technical solution of the present invention, the binder is polyvinyl alcohol.
[0016] As a preferred technical solution of the present invention, the dispersant is ammonium polyacrylate.
[0017] As a preferred technical solution of the present invention, in step S21, during the laser processing, the pulse width of the laser is 5-20 ps, the power of the laser is 25-50 W, and the frequency of the laser is 2-4 MHz.
[0018] A preparation process of a ceramic PTC thermistor material, comprising the following preparation processes:
[0019] S71. Fully and uniformly mix barium titanate doped with niobium and ruthenium, a sintering aid, and modified silicon boride according to their mass fractions to obtain a mixture;
[0020] S72, ball milling the mixture with deionized water in equal parts by mass at a speed of 500-700 r / min for 8-10 h to obtain a mixture slurry;
[0021] S73, after the mixture slurry is allowed to stand for 4-8 hours, the slurry is impurity-removed, and then a binder and a dispersant are added and stirred for 12 hours to obtain an atomized liquid, and the atomized liquid is heated and rotated by an atomizer and sprayed into a spray tower for granulation. After the granulation is completed, it is pressurized and formed in a punching machine with a tonnage of 5-10 tons to obtain a green body material;
[0022] S74, placing the green body material into a muffle furnace, and keeping the temperature at 600-800°C for 2-4 hours for pre-sintering treatment;
[0023] S75, heating the temperature to 1400-1500° C. at a heating rate of 3-5° C. / min, maintaining the temperature for 2-6 hours, and annealing at 800-900° C. for 5-6 hours, and cooling to room temperature to obtain the ceramic PTC thermistor material.
[0024] As a preferred technical solution of the present invention, in step S73, the particle size of the particles after the granulation is completed is 100-200 meshes.
[0025] As a preferred technical solution of the present invention, in step S73, the process of removing impurities from the slurry is to first remove the supernatant from the mixture slurry after standing, and then filter it through an 80-mesh sieve.
[0026] Beneficial effects of the present invention:
[0027] (1) In the present invention, the main raw material of the PTC thermistor material is prepared by doping barium titanate with niobium and ruthenium. Niobium oxide and ruthenium oxide are first sintered with barium titanate and then sintered together with other sintering aids. This can improve the doping efficiency of metallic niobium and ruthenium in barium titanate, help ruthenium and niobium to be more evenly distributed in the barium titanate matrix material, and thus improve the performance of the PTC thermistor material.
[0028] As donor doping elements, niobium and ruthenium can generate additional free electrons in barium titanate. These free electrons can affect the resistivity of the material. As the doping amount of the two increases, the resistivity of the material will decrease, which can make the PTC thermistor material have a higher lift-to-resistance ratio and a steeper resistance-temperature characteristic curve within a specific temperature range. Through high-temperature sintering, barium titanate doped with niobium and ruthenium can affect the Curie temperature by changing the crystal structure and phase change behavior of the material, refine the grains of barium titanate, and reduce the defects and pores inside the material, thereby improving the density and uniformity of barium titanate. Simultaneous doping of these two elements will produce a synergistic effect. In barium titanate, simultaneous doping of ruthenium and niobium may promote the formation of more donor-acceptor pairs. These donor-acceptor pairs will affect the concentration and mobility of carriers when the temperature changes, thereby affecting the resistivity of the material and further enhancing the PTC effect.
[0029] (2) Silicon boride has good thermal stability and can maintain stable thermal insulation at high temperatures. It can also reduce the resistivity of PTC thermistor materials at room temperature and improve the electrical conductivity of the material. By laser processing silicon boride, the pulse width can be set to control the heat affected zone while achieving phase change of the material through precise energy control. For silicon boride, laser processing will induce rapid melting, recrystallization or phase change in local areas, thereby changing its microstructure, reducing the impact of defects and stress, and improving the long-term stability of the material. At the same time, laser processing can achieve effective diffusion of boron elements in silicon boride, which can improve the electrical properties of silicon boride, such as reducing resistivity and increasing carrier mobility.
[0030] After laser treatment improves the structural stability of silicon boride, glycine is used to treat silicon boride at high temperature. Glycine, as a nitrogen source compound, can help obtain nitrogen-doped silicon boride. After the silicon boride is treated with glycine, the glycine molecules are attached to the surface of the silicon boride by physical or chemical adsorption, thereby changing the charge distribution on the surface of the silicon boride, and the glycine molecules can enter the surface pores of the silicon boride. After high-temperature treatment, glycine decomposes, thereby optimizing the grain structure of the material and improving the surface performance; and through nitrogen doping, the grain boundary resistance of the material is changed to achieve a reduction in resistivity. In the process of preparing PTC thermistor materials together with other materials, the nitrogen element will enter the grain boundary region of the material, affecting the electron transport characteristics at the grain boundary, thereby reducing the grain boundary resistance and improving the sensitivity and response speed of the PTC thermistor.
[0031] (3) In the present invention, the density of the material is improved by high-temperature sintering, and the oxygen vacancies caused by the preparation process of niobium and ruthenium-doped barium titanate ceramics when preparing the main raw materials are eliminated by annealing treatment after high-temperature sintering. The internal stress and residual stress generated in the high-temperature sintering process can also be eliminated, which helps to improve the stability of the material. DETAILED DESCRIPTION
[0032] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.
[0033] In the following examples and comparative examples:
[0034] Barium titanate: purchased from Hubei Baidu Chemical Co., Ltd.;
[0035] Niobium oxide: purchased from Wuhan Lianhekang Biotechnology Co., Ltd., catalog number: A00548;
[0036] Ruthenium oxide: purchased from Hubei Guangao Biotechnology Co., Ltd.;
[0037] Silicon boride: purchased from Hubei Jusheng Technology Co., Ltd.;
[0038] Glycine: purchased from Jinan Jiao Chemical Co., Ltd., product number: 56-40-6;
[0039] Polyvinyl alcohol: purchased from Shanghai MacLean Biochemical Technology Co., Ltd., product number: P875285;
[0040] Ammonium polyacrylate:
[0041] Alumina: purchased from Kangdisi Chemical (Hubei) Co., Ltd.;
[0042] Silica: purchased from Wuhan Jixinyibang Biotechnology Co., Ltd.
[0043] Example 1
[0044] Preparation of the barium titanate doped with niobium and ruthenium:
[0045] First, 50 parts of barium titanate, 0.1 parts of niobium oxide powder, and 0.1 parts of ruthenium oxide powder are dried in an oven, and then ball-milled in a ball mill using anhydrous ethanol as a ball-milling medium to fully mix them. The mixed powder is kept at 1100°C for 2 hours for solid-phase sintering. After the reaction is completed, the powder is ball-milled and mixed to obtain niobium- and ruthenium-doped barium titanate.
[0046] Preparation of modified borosilicate:
[0047] S21. In a nitrogen atmosphere, laser treatment is performed on silicon boride to obtain pretreated silicon boride, wherein the laser pulse width is 5 ps, the laser power is 25 W, and the laser frequency is 2 MHz;
[0048] S22. At 50°C, add glycine and pretreated borosilicate in a ratio of 1:1 by mass to deionized water, perform ultrasonic treatment for 0.5 h to obtain a uniformly dispersed mixed solution, continue heating to 100°C, evaporate the water under stirring, collect the obtained solid and dry it;
[0049] S23, the dried solid is transferred into a tubular furnace for calcination in high-purity nitrogen at 900° C. for 2 h, and then pulverized after cooling to room temperature to obtain the modified borosilicate.
[0050] Preparation of ceramic PTC thermistor materials:
[0051] S71. Fully mix 50 parts of barium titanate doped with niobium and ruthenium, 5 parts of aluminum oxide, and 10 parts of modified borosilicate silicon according to their mass fractions to obtain a mixture;
[0052] S72, ball milling the mixture with deionized water in equal parts by mass at a speed of 500 r / min for 8 h to obtain a mixture slurry;
[0053] S73, after the mixture slurry is allowed to stand for 4 hours, the upper clear liquid is first removed from the slurry, and then filtered through an 80-mesh sieve, and then 1 part of ammonium polyacrylate and 4 parts of polyvinyl alcohol are added and stirred for 12 hours to obtain an atomized liquid, and the atomized liquid is heated and rotated by an atomizer and sprayed into a spray tower for granulation. After the granulation is completed, the particle size of the particles is 100 mesh, and then the particles are pressurized and formed in a punching machine with a tonnage of 5T to obtain a green body material;
[0054] S74, placing the green body material into a muffle furnace, and keeping the temperature at 600° C. for 2 hours for pre-sintering treatment;
[0055] S75, heating the temperature to 1400° C. at a heating rate of 3° C. / min, maintaining the temperature for 2 hours, and performing annealing treatment at 800° C. for 5 hours, and cooling to room temperature to obtain the ceramic PTC thermistor material.
[0056] Example 2
[0057] Preparation of the barium titanate doped with niobium and ruthenium:
[0058] First, 60 parts of barium titanate, 0.12 parts of niobium oxide powder, and 0.13 parts of ruthenium oxide powder were dried in an oven, and then ball-milled in a ball mill using anhydrous ethanol as a ball-milling medium to fully mix them. The mixed powders were kept at 1150°C for 3 hours for solid-phase sintering. After the reaction was completed, the powders were ball-milled and mixed to obtain niobium- and ruthenium-doped barium titanate.
[0059] Preparation of modified borosilicate:
[0060] S21. In a nitrogen atmosphere, laser treatment is performed on silicon boride to obtain pretreated silicon boride, wherein the laser pulse width is 14 ps, the laser power is 30 W, and the laser frequency is 3 MHz;
[0061] S22. At 55°C, add glycine and pretreated borosilicate in a ratio of 1:1 by mass to deionized water, perform ultrasonic treatment for 0.8h to obtain a uniformly dispersed mixed solution, continue heating to 105°C, evaporate the water under stirring, collect the obtained solid and dry it;
[0062] S23, the dried solid is transferred into a tubular furnace for calcination in high-purity nitrogen at 950° C. for 2.5 h, and then pulverized after cooling to room temperature to obtain the modified borosilicate.
[0063] Preparation of ceramic PTC thermistor materials:
[0064] S71, mixing 60 parts of barium titanate doped with niobium and ruthenium, 8 parts of aluminum oxide, and 15 parts of modified borosilicate silicon in parts by mass to obtain a mixture;
[0065] S72, ball milling the mixture with equal mass parts and deionized water at a speed of 600 r / min for 9 h to obtain a mixture slurry;
[0066] S73, after the mixture slurry is allowed to stand for 6 hours, the supernatant is first removed from the slurry, and then filtered through an 80-mesh sieve, and then 2 parts of ammonium polyacrylate and 5 parts of polyvinyl alcohol are added and stirred for 12 hours to obtain an atomized liquid, and the atomized liquid is heated and rotated by an atomizer and sprayed into a spray tower for granulation. After the granulation is completed, the particle size of the particles is 150 mesh, and then the particles are pressurized and formed in a punching machine with a tonnage of 8T to obtain a green body material;
[0067] S74, placing the green body material into a muffle furnace, and keeping the temperature at 700° C. for 3 hours for pre-sintering treatment;
[0068] S75, heating the temperature to 1450° C. at a heating rate of 4° C. / min, maintaining the temperature for 4 hours, and performing annealing treatment at 850° C. for 5.5 hours, and cooling to room temperature to obtain the ceramic PTC thermistor material.
[0069] Example 3
[0070] Preparation of the barium titanate doped with niobium and ruthenium:
[0071] 70 parts of barium titanate, 0.15 parts of niobium oxide powder, and 0.15 parts of ruthenium oxide powder were dried in an oven, and ball-milled in a ball mill using anhydrous ethanol as a ball-milling medium to be fully mixed. The mixed powder was kept at 1200°C for 4 hours for solid-phase sintering. After the reaction was completed, the powder was ball-milled and mixed again to obtain niobium- and ruthenium-doped barium titanate.
[0072] Preparation of modified borosilicate:
[0073] S21. In a nitrogen atmosphere, laser treatment is performed on silicon boride to obtain pretreated silicon boride, wherein the laser pulse width is 20 ps, the laser power is 50 W, and the laser frequency is 4 MHz;
[0074] S22. At 60° C., add glycine and pretreated borosilicate in a ratio of 1:1 by mass to deionized water, perform ultrasonic treatment for 0.5 to 1 h to obtain a uniformly dispersed mixed solution, continue heating to 110° C., evaporate the water under stirring, collect the obtained solid and dry it;
[0075] S23, the dried solid is transferred into a tubular furnace for calcination in high-purity nitrogen at 1000° C. for 3 h, and then pulverized after cooling to room temperature to obtain the modified borosilicate.
[0076] Preparation of ceramic PTC thermistor materials:
[0077] S71, fully and uniformly mixing 70 parts of barium titanate doped with niobium and ruthenium, 10 parts of silicon dioxide, and 20 parts of modified silicon boride according to their mass fractions to obtain a mixture;
[0078] S72, ball milling the mixture with deionized water in equal parts by mass at a speed of 700 r / min for 10 h to obtain a mixture slurry;
[0079] S73, after the mixture slurry is allowed to stand for 8 hours, the supernatant is first removed from the slurry, and then filtered through an 80-mesh sieve, 3 parts of ammonium polyacrylate and 6 parts of polyvinyl alcohol are added and stirred for 12 hours to obtain an atomized liquid, the atomized liquid is heated and rotated by an atomizer and sprayed into a spray tower for granulation. After the granulation is completed, the particle size of the particles is 200 mesh, and then the particles are pressurized and formed in a punching machine with a tonnage of 10T to obtain a green body material;
[0080] S74, placing the green body material into a muffle furnace, and keeping the temperature at 800° C. for 4 hours for pre-sintering treatment;
[0081] S75, heating the temperature to 1500° C. at a heating rate of 5° C. / min, maintaining the temperature for 6 hours, and performing annealing treatment at 900° C. for 6 hours, and cooling to room temperature to obtain the ceramic PTC thermistor material.
[0082] Comparative Example 1
[0083] The difference between Comparative Example 1 and Example 1 is that niobium oxide is not added in Comparative Example 1, and the other operations are the same.
[0084] Comparative Example 2
[0085] The difference between Comparative Example 2 and Example 1 is that ruthenium oxide is not added in Comparative Example 2, and the other operations are the same.
[0086] Comparative Example 3
[0087] The difference between Comparative Example 3 and Example 1 is that in Comparative Example 3, the silicon boride is not treated by laser, and the other operations are the same.
[0088] Comparative Example 4
[0089] The difference between Comparative Example 4 and Example 1 is that in Comparative Example 4, the boron silicon is not treated with glycine, and the other operations are the same.
[0090] Comparative Example 5
[0091] The difference between Comparative Example 5 and Example 1 is that no modification treatment is performed in Comparative Example 5, and the other operations are the same.
[0092] Comparative Example 6
[0093] The difference between Comparative Example 6 and Example 1 is that in step S75 of Comparative Example 6, no annealing treatment is performed, and the other operations are the same.
[0094] Performance Testing:
[0095] 1. Impedance analysis: Use Wenke precision impedance analyzer, model 6510B, with a test frequency of 20Hz~10MHz for impedance testing;
[0096] 2. Room temperature resistance: Use a multimeter to test the resistance at room temperature;
[0097] 3. Curie temperature: Use a multimeter to measure the resistance, and the temperature corresponding to when the resistance reaches the maximum;
[0098] 4. Rise-to-drag ratio: lg (Curie point resistance / room temperature resistance);
[0099] 5. Withstand voltage: Use BYD-GN-02 withstand voltage tester to test the breakdown voltage. The test results are shown in Table 1.
[0100] Table 1
[0101]
[0102] The ceramic thermistor material prepared by the present invention has high Curie temperature, high withstand voltage, high lift-to-resistance ratio, simple process, low sintering condition requirements and easy control, and the prepared PTC thermistor has better performance.
[0103] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A ceramic PTC thermistor material, characterized in that: The invention comprises the following components in the following amounts by weight: 50-70 parts of barium titanate doped with niobium and ruthenium, 5-10 parts of a sintering aid, 10-20 parts of modified borosilicate, 1-3 parts of a dispersant and 4-6 parts of a binder; The preparation process of the barium titanate doped with niobium and ruthenium is as follows: First, 50-70 parts of barium titanate, 0.1-0.15 parts of niobium oxide powder, and 0.1-0.15 parts of ruthenium oxide powder are dried in an oven, and anhydrous ethanol is used as a ball milling medium to fully mix the powders in a ball mill, and the mixed powders are kept at 1100-1200° C. for 2-4 hours for solid phase sintering. After the reaction is completed, the powders are further ball milled to obtain niobium and ruthenium doped barium titanate; The preparation process of the modified borosilicate is as follows: S21. Under a nitrogen atmosphere, laser-treating silicon boride to obtain pretreated silicon boride, wherein the laser pulse width during the laser treatment is 5 to 20 ps, the laser power is 25 to 50 W, and the laser frequency is 2 to 4 MHz; S22, at 50-60°C, add glycine and pretreated borosilicate in a ratio of 1:1 by mass to deionized water, ultrasonically treat for 0.5-1h to obtain a uniformly dispersed mixed solution, continue heating to 100-110°C, evaporate the water under stirring, collect the obtained solid and dry it; S23, moving the dried solid into a tubular furnace for calcination in high-purity nitrogen at 900-1000° C. for 2-3 hours, cooling to room temperature and then crushing to obtain the modified borosilicate; The preparation process of the ceramic PTC thermistor material includes the following processes: S71. Fully and uniformly mix barium titanate doped with niobium and ruthenium, a sintering aid, and modified silicon boride according to their mass fractions to obtain a mixture; S72, ball milling the mixture with deionized water in equal parts by mass at a speed of 500-700 r / min for 8-10 h to obtain a mixture slurry; S73, after the mixture slurry is allowed to stand for 4-8 hours, the slurry is impurity-removed, and then a binder and a dispersant are added and stirred for 12 hours to obtain an atomized liquid, and the atomized liquid is heated and rotated by an atomizer and sprayed into a spray tower for granulation. After the granulation is completed, it is pressurized and formed in a punching machine with a tonnage of 5-10 tons to obtain a green body material; S74, placing the green body material into a muffle furnace, and keeping it at a high temperature of 600-800°C for 2-4 hours for pre-sintering treatment; S75, heating the temperature to 1400-1500° C. at a heating rate of 3-5° C. / min, maintaining the temperature for 2-6 hours, and annealing at 800-900° C. for 5-6 hours, and cooling to room temperature to obtain the ceramic PTC thermistor material.
2. The ceramic PTC thermistor material according to claim 1, characterized in that: The sintering aid is one or more of alumina, silicon dioxide and calcium carbonate.
3. The ceramic PTC thermistor material according to claim 1, characterized in that: The binder is polyvinyl alcohol.
4. The ceramic PTC thermistor material according to claim 1, characterized in that: The dispersant is ammonium polyacrylate.
5. The ceramic PTC thermistor material according to claim 1, characterized in that: In step S73, after the granulation is completed, the particle size of the particles is 100-200 meshes.
6. The ceramic PTC thermistor material according to claim 1, characterized in that: In step S73, the process of removing impurities from the slurry is to first remove the supernatant from the mixture slurry after standing, and then filter it through an 80-mesh sieve.