A corrosion inhibitor and its preparation method, metal etching liquid and application

By using compounds such as epoxy succinic acid to interact with the surface of the copper-titanium composite layer, a protective film is formed, which solves the problem of side etching and low stability of the copper-titanium etching liquid, and achieves a more uniform etching effect and more High product yield.

CN118638252BActive Publication Date: 2024-11-15HEFEI SINOPISE MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411110786.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-15
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The existing copper-titanium etching liquid is prone to side etching during the etching process, and the high metal ion content leads to low stability of the etching liquid, affecting the etching effect, and resulting in low product yield.

Method used

The corrosion inhibitor obtained by reacting epoxysuccinic acid, mono(6-ethylenediamine-6-deoxy)-β-cyclodextrin and 2-acrylamide-2-methylpropanesulfonic acid is used to form a stable The complex interacts with the surface of the copper-titanium composite layer to form a double-layer protective film, reducing the contact between the side walls and the etching liquid, and controlling the etching speed and surface quality by optimizing the proportion of the etching liquid components.

Benefits of technology

It significantly reduces side corrosion, improves the stability and service life of the etching liquid, forms a uniform and smooth etching surface, enhances the etching effect of the copper-titanium composite layer, and improves product yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118638252B_ABST
    Figure CN118638252B_ABST
Patent Text Reader

Abstract

The invention discloses a corrosion inhibitor and a preparation method thereof, a metal etching solution and an application thereof, and belongs to the field of etching technology. The corrosion inhibitor of the invention is obtained by epoxysuccinic acid, mono(6-ethylenediamine-6-deoxy)-β-cyclodextrin and 2-acrylamide-2-methylpropanesulfonic acid, and the corrosion inhibitor is attached to the side wall of the copper-titanium composite layer to form a double-layer protective film, reduce the contact between the side wall and the etching solution, and then adjust the etching speed of the copper-titanium composite layer by the etching solution, which is conducive to forming a suitable CD-Bias and etching angle, thereby reducing side etching. The etching solution of the invention is composed of hydrogen peroxide, a fluoride ion supply source, an organic acid, an organic base, a hydrogen peroxide stabilizer, an inorganic salt, a corrosion inhibitor, etc., and the mass fraction of each component is controlled within a specific range to promote interaction, so that the etching speed of the etching solution to the copper and titanium layers is moderate, and it is helpful to form a uniform and smooth etching surface; and the etching solution has high stability and a long service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of etching, and in particular relates to a corrosion inhibitor and a preparation method thereof, a metal etching solution and applications thereof. Background Art

[0002] In recent years, with the popularity of large-screen and high-definition flat panel displays (FPD), higher requirements have been put forward for wiring materials in thin-film transistors (TFTs), especially materials with lower resistance are needed to improve performance. Traditional aluminum materials have gradually failed to meet the demand due to their relatively high resistance. Copper has been widely adopted as a new generation of wiring materials due to its lower resistance characteristics. However, the introduction of copper as a wiring material also brought new problems, mainly the lack of adhesion between the substrate and the diffusion of copper to the semiconductor substrate. At present, a multi-layer wiring scheme is adopted, that is, a layer of molybdenum film is first deposited on the semiconductor substrate, and then a copper film is deposited on it. The high melting point and good adhesion of the molybdenum film are used to enhance the adhesion between the copper film and the substrate, and may to some extent block the diffusion of copper to the silicon substrate; in order to further ensure the insulation and adhesion with the substrate, the more common practice is to first deposit a layer of titanium film between the copper film and the semiconductor substrate as a base layer.

[0003] The patent application with publication number CN115852372A discloses a copper-titanium etching solution for liquid crystal panels, comprising a main agent; in terms of mass percentage, the main components of the main agent are: 1%-15% hydrogen peroxide, 0.5%-9% inorganic acid, 0.01%-5% organic acid, 0.3%-25% organic base, 0.001%-3% hydrogen peroxide stabilizer, 0.001%-3% metal corrosion inhibitor, fluoride ion source and residual water, and the mass concentration of fluoride ions in the copper-titanium etching solution for liquid crystal panels is 0-150ppm; although the copper-titanium etching solution of the invention reduces substrate damage and overcomes the black spot problem after the panel is covered with silicon nitride, the etching effect of the etching solution on different metal materials such as copper and titanium will still be different, the etching rates of the copper layer and the titanium layer are different, and side etching will occur, and the metal ion content in the etching solution is relatively high, which reduces the stability of the etching solution, thereby affecting the etching effect and resulting in low product yield. Summary of the invention

[0004] The purpose of the present invention is to provide a corrosion inhibitor to solve the problem that etching solution is prone to side corrosion; to provide a metal etching solution to solve the problem that the etching effect of the etching solution is poor.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A corrosion inhibitor is obtained by reacting epoxysuccinic acid, mono(6-ethylenediamino-6-deoxy)-β-cyclodextrin and 2-acrylamide-2-methylpropanesulfonic acid. The structure of the corrosion inhibitor is shown below:

[0007] .

[0008] A method for preparing a corrosion inhibitor comprises the following steps:

[0009] S1. Add epoxysuccinic acid and mono(6-ethylenediamino-6-deoxy)-β-cyclodextrin to N,N-dimethylformamide, stir and react at 55-65° C. for 4-5 hours, cool to room temperature, filter, wash, and rotary evaporate to obtain epoxysuccinic acid-cyclodextrin;

[0010] S2. Add epoxysuccinic acid-cyclodextrin and 2-acrylamide-2-methylpropanesulfonic acid into water, raise the temperature to 75-95°C, adjust the pH value to 12-13 with 50wt% NaOH solution, add initiator ammonium persulfate, react for 3-4h, cool to room temperature, adjust the pH value to 1-3 with 30wt% dilute sulfuric acid, add ethanol and let stand for 2-4h, filter, wash the filter cake with acetone, and dry to obtain a corrosion inhibitor.

[0011] Preferably, the ratio of epoxysuccinic acid, mono(6-ethylenediamino-6-deoxy)-β-cyclodextrin and N,N-dimethylformamide in S1 is 1 g:17-23 g:100 mL.

[0012] Preferably, the ratio of epoxysuccinic acid-cyclodextrin, 2-acrylamide-2-methylpropanesulfonic acid, ammonium persulfate, water and ethanol in S2 is 21-25g:2g:0.01-0.5g:100mL:400-500mL.

[0013] The preparation principle of corrosion inhibitor is as follows:

[0014]

[0015] A metal etching solution is composed of the following components in mass fractions: 12-25wt% hydrogen peroxide, 4-9wt% fluoride ion supply source, 0.1-0.5wt% organic acid, 0.05-0.5wt% organic base, 0.1-3wt% hydrogen peroxide stabilizer, 0.1-4wt% inorganic salt, 0.1-5wt% above-mentioned corrosion inhibitor, and the balance is deionized water.

[0016] Preferably, the fluoride ion supply source is one or more of hydrofluoric acid, ammonium fluoride, potassium fluoride, ammonium fluoroborate, potassium bifluoride, potassium fluoroborate, sodium fluoride and sodium bifluoride.

[0017] Preferably, the organic acid is one or more of citric acid, caffeic acid, ferulic acid, tannic acid and humic acid.

[0018] Preferably, the organic acid is obtained by mixing citric acid, caffeic acid and humic acid in a mass ratio of 4:2-7:5.

[0019] Preferably, the organic base is tetramethylguanidine and / or diglycolamine.

[0020] Preferably, the inorganic salt is one or more of diammonium hydrogen phosphate, ammonium phosphate, ammonium dihydrogen phosphate, ammonium nitrate, ammonium sulfate and ammonium chloride.

[0021] Preferably, the hydrogen peroxide stabilizer is one or more of phytic acid, phenylurea and cyclohexylamine.

[0022] The invention discloses an application of a metal etching liquid in etching a copper-titanium composite layer.

[0023] Beneficial effects of the present invention:

[0024] 1. The corrosion inhibitor of the present invention is obtained from epoxysuccinic acid, mono(6-ethylenediamino-6-deoxy)-β-cyclodextrin and 2-acrylamide-2-methylpropanesulfonic acid. Epoxysuccinic acid is used as a connector to connect mono(6-ethylenediamino-6-deoxy)-β-cyclodextrin and 2-acrylamide-2-methylpropanesulfonic acid in the form of a chemical bond; one end of the corrosion inhibitor is 2-acrylamide-2-methylpropanesulfonic acid, and its sulfonic acid group reacts with metal ions to form a stable complex that can be adsorbed on the surface of the copper-titanium composite layer; the amide group can provide additional adsorption capacity, so that the corrosion inhibitor is more firmly attached to the surface of the copper-titanium composite layer; at the same time, the other end of the corrosion inhibitor is cyclodextrin, and its cavity structure can form a physical barrier on the surface of the copper-titanium composite layer, thereby preventing the etching solution from further corroding the metal. During the etching process, the copper film layer and the titanium film layer will form a certain galvanic effect under the action of copper ions in the system. The corrosion inhibitor of the present invention can adhere to the side wall of the copper-titanium composite layer to form a double-layer protective film, which significantly reduces the contact between the side wall and the etching solution, thereby adjusting the etching speed of the etching solution on the copper-titanium composite layer, which is conducive to forming a suitable CD-Bias and etching angle, thereby reducing side etching.

[0025] 2. The metal etching solution of the present invention is composed of hydrogen peroxide, a fluoride ion supply source, an organic acid, an organic base, a hydrogen peroxide stabilizer, an inorganic salt, a corrosion inhibitor, etc., and the mass fraction of each component is controlled within a specific range. The components interact with each other, so that the etching speed of the etching solution on the copper and titanium layers is moderate, which helps to form a uniform and smooth etching surface; and the etching solution has high stability and a long service life.

[0026] 3. The metal etching solution of the present invention contains an organic base and an organic acid. Since the complexing ability of the corrosion inhibitor is passivated when the concentration of the hydrogen peroxide and fluoride ion supply source is high in the early stage of etching, the organic acid and organic base can complex with the copper ions, reducing the oxidation reaction between the copper ions and the elemental copper, and can also effectively avoid the safety problem of high-concentration copper ions catalyzing hydrogen peroxide. The present invention further preferably uses a mixture of citric acid, caffeic acid and humic acid as an organic acid. The three have different structures and different complexing abilities with copper ions, and synergize to promote the organic acid to effectively adjust the copper ion concentration in the etching solution, thereby maintaining a high safety and stability of the etching solution, while maintaining good etching ability, and ensuring an excellent etching effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The present invention will be further described below in conjunction with the accompanying drawings.

[0028] Figure 1 is a scanning electron microscope image of the etching effect in Example 1 of the present invention;

[0029] Figure 2 is a scanning electron microscope image of the etching effect in Example 8 of the present invention;

[0030] Figure 3 It is a scanning electron microscope image of the etching effect in comparative example 1 of the present invention. DETAILED DESCRIPTION

[0031] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Preparation Example 1

[0033] Corrosion inhibitor, prepared by the following method:

[0034] S1. Add 1 g of epoxysuccinic acid and 17 g of mono(6-ethylenediamino-6-deoxy)-β-cyclodextrin to 100 mL of N,N-dimethylformamide, stir and react at 55° C. for 5 h, cool to room temperature, filter, wash, and rotary evaporate to obtain epoxysuccinic acid-cyclodextrin;

[0035] S2. Add 21g of epoxysuccinic acid-cyclodextrin and 2g of 2-acrylamide-2-methylpropanesulfonic acid to 100mL of water, heat to 75°C, adjust the pH value to 12 with 50wt% NaOH solution, add 0.01g of initiator ammonium persulfate, react for 4h, cool to room temperature, adjust the pH value to 3 with 30wt% dilute sulfuric acid, add 400mL of ethanol, let stand for 2h, filter, wash the filter cake with acetone, and dry to obtain a corrosion inhibitor.

[0036] Preparation Example 2

[0037] Corrosion inhibitor, prepared by the following method:

[0038] S1. Add 1 g of epoxysuccinic acid and 20 g of mono(6-ethylenediamino-6-deoxy)-β-cyclodextrin to 100 mL of N,N-dimethylformamide, stir and react at 60° C. for 4.5 h, cool to room temperature, filter, wash, and rotary evaporate to obtain epoxysuccinic acid-cyclodextrin;

[0039] S2. Add 23 g of epoxysuccinic acid-cyclodextrin and 2 g of 2-acrylamide-2-methylpropanesulfonic acid to 100 mL of water, heat to 85 ° C, adjust the pH value to 12 with 50 wt % NaOH solution, add 0.03 g of initiator ammonium persulfate, react for 3.5 h, cool to room temperature, adjust the pH value to 2 with 30 wt % dilute sulfuric acid, add 450 mL of ethanol and let stand for 3 h, filter, wash the filter cake with acetone, and dry to obtain a corrosion inhibitor.

[0040] Preparation Example 3

[0041] Corrosion inhibitor, prepared by the following method:

[0042] S1. Add 1 g of epoxysuccinic acid and 23 g of mono(6-ethylenediamino-6-deoxy)-β-cyclodextrin to 100 mL of N,N-dimethylformamide, stir and react at 65° C. for 4 h, cool to room temperature, filter, wash, and rotary evaporate to obtain epoxysuccinic acid-cyclodextrin;

[0043] S2. Add 25 g of epoxysuccinic acid-cyclodextrin and 2 g of 2-acrylamide-2-methylpropanesulfonic acid to 100 mL of water, heat to 95 ° C, adjust the pH value to 13 with 50 wt % NaOH solution, add 0.5 g of initiator ammonium persulfate, react for 3 h, cool to room temperature, adjust the pH value to 1 with 30 wt % dilute sulfuric acid, add 500 mL of ethanol and let stand for 4 h, filter, wash the filter cake with acetone, and dry to obtain a corrosion inhibitor.

[0044] Example 1

[0045] A metal etching solution, composed of the following components by mass fraction: 12wt% hydrogen peroxide, 4wt% fluoride ion supply source, 0.1wt% organic acid, 0.05wt% organic base, 0.1wt% hydrogen peroxide stabilizer, 0.1wt% inorganic salt, 0.1wt% corrosion inhibitor, 83.55wt% deionized water;

[0046] The fluoride ion supply source is hydrofluoric acid; the organic acid is tannic acid; the organic base is tetramethylguanidine; the hydrogen peroxide stabilizer is phytic acid; the inorganic salt is diammonium hydrogen phosphate; and the corrosion inhibitor is prepared by Preparation Example 1.

[0047] Example 2

[0048] A metal etching solution, composed of the following components by mass fraction: 18wt% hydrogen peroxide, 7wt% fluoride ion supply source, 0.25wt% organic acid, 0.15wt% organic base, 1wt% hydrogen peroxide stabilizer, 2wt% inorganic salt, 1.5wt% corrosion inhibitor, 70.1wt% deionized water;

[0049] The fluoride ion supply source is ammonium fluoride; the organic acid is obtained by mixing caffeic acid and ferulic acid in a mass ratio of 1:1; the organic base is diglycolamine; the hydrogen peroxide stabilizer is cyclohexylamine; the inorganic salt is ammonium nitrate; and the corrosion inhibitor is prepared by Preparation Example 2.

[0050] Example 3

[0051] A metal etching solution, composed of the following components by mass fraction: 25wt% hydrogen peroxide, 9wt% fluoride ion supply source, 0.5wt% organic acid, 0.5wt% organic base, 3wt% hydrogen peroxide stabilizer, 4wt% inorganic salt, 5wt% corrosion inhibitor, 53wt% deionized water;

[0052] The fluoride ion supply source is potassium bifluoride; the organic acid is humic acid; the organic base is obtained by mixing tetramethylguanidine and diglycolamine in a mass ratio of 1:1; the hydrogen peroxide stabilizer is phenyl urea; the inorganic salt is ammonium chloride; and the corrosion inhibitor is obtained by Preparation Example 3.

[0053] Example 4

[0054] A metal etching solution, composed of the following components by mass fraction: 12wt% hydrogen peroxide, 4wt% fluoride ion supply source, 0.1wt% organic acid, 0.05wt% organic base, 0.1wt% hydrogen peroxide stabilizer, 0.1wt% inorganic salt, 0.1wt% corrosion inhibitor, 83.55wt% deionized water;

[0055] The fluoride ion supply source is hydrofluoric acid; the organic acid is obtained by mixing caffeic acid and humic acid in a mass ratio of 1:1; the organic base is tetramethylguanidine; the hydrogen peroxide stabilizer is phytic acid; the inorganic salt is diammonium hydrogen phosphate; and the corrosion inhibitor is prepared by Preparation Example 1.

[0056] Example 5

[0057] A metal etching solution, composed of the following components by mass fraction: 12wt% hydrogen peroxide, 4wt% fluoride ion supply source, 0.1wt% organic acid, 0.05wt% organic base, 0.1wt% hydrogen peroxide stabilizer, 0.1wt% inorganic salt, 0.1wt% corrosion inhibitor, 83.55wt% deionized water;

[0058] The fluoride ion supply source is hydrofluoric acid; the organic acid is obtained by mixing citric acid and caffeic acid in a mass ratio of 1:1; the organic base is tetramethylguanidine; the hydrogen peroxide stabilizer is phytic acid; the inorganic salt is diammonium hydrogen phosphate; and the corrosion inhibitor is prepared by Preparation Example 1.

[0059] Example 6

[0060] A metal etching solution, composed of the following components by mass fraction: 12wt% hydrogen peroxide, 4wt% fluoride ion supply source, 0.1wt% organic acid, 0.05wt% organic base, 0.1wt% hydrogen peroxide stabilizer, 0.1wt% inorganic salt, 0.1wt% corrosion inhibitor, 83.55wt% deionized water;

[0061] The fluoride ion supply source is hydrofluoric acid; the organic acid is obtained by mixing citric acid and humic acid in a mass ratio of 1:1; the organic base is tetramethylguanidine; the hydrogen peroxide stabilizer is phytic acid; the inorganic salt is diammonium hydrogen phosphate; and the corrosion inhibitor is prepared by Preparation Example 1.

[0062] Example 7

[0063] A metal etching solution, composed of the following components by mass fraction: 12wt% hydrogen peroxide, 4wt% fluoride ion supply source, 0.1wt% organic acid, 0.05wt% organic base, 0.1wt% hydrogen peroxide stabilizer, 0.1wt% inorganic salt, 0.1wt% corrosion inhibitor, 83.55wt% deionized water;

[0064] The fluoride ion supply source is hydrofluoric acid; the organic acid is obtained by mixing citric acid, caffeic acid and humic acid in a mass ratio of 4:2:5; the organic base is tetramethylguanidine; the hydrogen peroxide stabilizer is phytic acid; the inorganic salt is diammonium hydrogen phosphate; and the corrosion inhibitor is prepared by Preparation Example 1.

[0065] Example 8

[0066] A metal etching solution, composed of the following components by mass fraction: 12wt% hydrogen peroxide, 4wt% fluoride ion supply source, 0.1wt% organic acid, 0.05wt% organic base, 0.1wt% hydrogen peroxide stabilizer, 0.1wt% inorganic salt, 0.1wt% corrosion inhibitor, 83.55wt% deionized water;

[0067] The fluoride ion supply source is hydrofluoric acid; the organic acid is obtained by mixing citric acid, caffeic acid and humic acid in a mass ratio of 4:7:5; the organic base is tetramethylguanidine; the hydrogen peroxide stabilizer is phytic acid; the inorganic salt is diammonium hydrogen phosphate; and the corrosion inhibitor is prepared by Preparation Example 1.

[0068] Comparative Example 1

[0069] Comparative Example 1 is different from Example 1 in that 5-aminotetrazolyl is used to replace the corrosion inhibitor prepared in Preparation Example 1.

[0070] Comparative Example 2

[0071] Comparative Example 2 is different from Example 1 in that no organic acid is added and an equal mass of deionized water is used to replace the organic acid.

[0072] Comparative Example 3

[0073] Comparative Example 3 is different from Example 1 in that no organic base is added, and an equal mass of deionized water is used to replace the organic base.

[0074] The etching solutions of Examples 1-8 and Comparative Examples 1-3 were subjected to performance tests. The performance test process is as follows. The test results are shown in Tables 1, Figure 1-3 As shown;

[0075] (1) Etching effect of etching solution: The etching effects of the etching solutions of Examples 1-8 and Comparative Examples 1-3 were tested. The copper-titanium composite layer substrate was etched using an etcher at 30°C, and the CD-Bias and Taper angle were observed by SEM. The SEM image of Example 1 is shown in FIG. Figure 1 As shown; the scanning electron microscope image of Example 8 is as shown Figure 2 As shown; the scanning electron microscope image of comparative example 1 is as shown Figure 3 shown.

[0076] (2) Life of etching solution: Add copper powder to the etching solution and control the initial dissolved copper content in the range of 200 to 500 ppm to complete the pretreatment of the etching solution; raise the temperature to 33°C and use the pretreated etching solution to etch the copper-titanium composite layer substrate until the etching parameters meet the production line design standards; starting from the initial dissolved copper content, gradually increase the dissolved copper content in the etching solution from 3000 to 15000 ppm, and then etch the copper-titanium composite layer substrates separately until the etching parameters meet the production line design standards.

[0077] Table 1

[0078]

[0079] It can be seen from Table 1 that the metal etching solution provided by the present invention can obtain a smaller CD-Bias (0.1-0.2μm) and a better Taper angle (30-40°), which meets the design and production requirements of high-precision large-size display panels, and has no titanium layer tailing and copper-titanium metal stacking fault phenomenon. It is suitable for promotion in the field of etching solutions and has broad development prospects.

[0080] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0081] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a corrosion inhibitor, characterized in that: The steps include: S1. Add epoxysuccinic acid and mono(6-ethylenediamino-6-deoxy)-β-cyclodextrin to N,N-dimethylformamide, stir and react at 55-65° C. for 4-5 hours, cool to room temperature, filter, wash, and rotary evaporate to obtain epoxysuccinic acid-cyclodextrin; S2. Add epoxysuccinic acid-cyclodextrin and 2-acrylamide-2-methylpropanesulfonic acid into water, raise the temperature to 75-95°C, adjust the pH value to 12-13 with 50wt% NaOH solution, add initiator ammonium persulfate, react for 3-4h, cool to room temperature, adjust the pH value to 1-3 with 30wt% dilute sulfuric acid, add ethanol and let stand for 2-4h, filter, wash the filter cake with acetone, and dry to obtain a corrosion inhibitor.

2. The method for preparing a corrosion inhibitor according to claim 1, characterized in that: The ratio of epoxysuccinic acid, mono(6-ethylenediamino-6-deoxy)-β-cyclodextrin and N,N-dimethylformamide in S1 is 1 g:17-23 g:100 mL; The ratio of epoxysuccinic acid-cyclodextrin, 2-acrylamide-2-methylpropanesulfonic acid, ammonium persulfate, water and ethanol in S2 is 21-25g:2g:0.01-0.5g:100mL:400-500mL.

3. A metal etching solution, characterized in that: The invention is composed of the following components in mass fractions: 12-25wt% hydrogen peroxide, 4-9wt% fluoride ion source, 0.1-0.5wt% organic acid, 0.05-0.5wt% organic base, 0.1-3wt% hydrogen peroxide stabilizer, 0.1-4wt% inorganic salt, 0.1-5wt% corrosion inhibitor, and the balance is deionized water, wherein the corrosion inhibitor is prepared by the method according to any one of claims 1 to 2.

4. A metal etching solution according to claim 3, characterized in that: The fluoride ion supply source is one or more of hydrofluoric acid, ammonium fluoride, potassium fluoride, ammonium fluoroborate, potassium bifluoride, potassium fluoroborate, sodium fluoride and sodium bifluoride; The inorganic salt is one or more of diammonium hydrogen phosphate, ammonium phosphate, ammonium dihydrogen phosphate, ammonium nitrate, ammonium sulfate and ammonium chloride.

5. A metal etching solution according to claim 3, characterized in that: The organic acid is one or more of citric acid, caffeic acid, ferulic acid, tannic acid and humic acid.

6. A metal etching solution according to claim 3, characterized in that: The organic acid is obtained by mixing citric acid, caffeic acid and humic acid in a mass ratio of 4:2-7:

5.

7. A metal etching solution according to claim 3, characterized in that: The organic base is tetramethylguanidine and / or diglycolamine.

8. A metal etching solution according to claim 3, characterized in that: The hydrogen peroxide stabilizer is one or more of phytic acid, phenylurea and cyclohexylamine.

9. Use of the metal etching solution as claimed in any one of claims 3 to 8 in etching a copper-titanium composite layer.