Preparation method of high-strength antibacterial thermoplastic polyurethane elastomer
By using hyperbranched polyurethane-amic acid modified nano-zinc oxide in polyurethane elastomer, the problems of poor dispersion of nano-zinc oxide and low strength of polyurethane elastomer are solved, and the mechanical and antibacterial properties of the material are significantly improved.
Patent Information
- Application Number
- CN202411103086.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-08-13
Smart Images

Figure QLYQS_1 
Figure SMS_5 
Figure SMS_6
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyurethane elastomers, in particular to a method for preparing a high-strength antibacterial thermoplastic polyurethane elastomer. Background Art
[0002] Polyurethane is a type of polymer containing carbamate structural units, which has good toughness, heat resistance, shock resistance and other properties. It can be made into elastomers, plastics and other products, and is widely used in the fields of shoemaking, sports goods, cushioning and shock-resistant materials, etc. Improving the mechanical properties and antibacterial properties of polyurethane elastomers will help expand its practical application in high-performance composite materials, medical supplies, etc.
[0003] Nano zinc oxide has a large specific surface area, high mechanical strength, and good antibacterial properties. However, nano zinc oxide is prone to agglomeration, poor compatibility with materials such as polyurethane, and poor dispersibility. Substances such as stearic acid, benzoic acid, and polyacrylic acid contain carboxyl groups, which can interact with the hydroxyl groups on the surface of zinc oxide through esterification reactions to achieve surface modification of nano zinc oxide. This can improve the dispersibility of nano zinc oxide.
[0004] Improving the dispersibility of nano zinc oxide in materials such as polyurethane can effectively enhance the mechanical, UV resistance, and antibacterial properties of the materials. The patent with the authorization announcement number CN104448208B discloses the preparation and application of organic silicon / nano ZnO composite modified polyurethane elastomer, in which isocyanate silane coupling agent, polyether polyol, and organic metal catalyst are reacted to obtain polymer A, which is then reacted with nano zinc oxide to obtain polyether polyol / nano zinc oxide hybrid material, and finally the polyurethane is modified with organic silicon to obtain a polyurethane elastomer material with excellent mechanical properties and UV resistance. However, the tensile strength and elongation at break of the polyurethane elastomer material are low, and it does not show good tear resistance. Summary of the invention
[0005] The technical problem solved by the present invention is: providing a preparation method of a high-strength antibacterial thermoplastic polyurethane elastomer, solving the problem that the dispersion of nano zinc oxide in the polyurethane elastomer is poor, and solving the problem that the polyurethane elastomer has low strength and no antibacterial performance.
[0006] The technical solution adopted by the present invention is: a method for preparing a high-strength antibacterial thermoplastic polyurethane elastomer:
[0007] Step S1: Add N,N-dimethylformamide, carbamate dianhydride monomer and tri(4-aminophenyl)methane into a reaction bottle, react in a nitrogen atmosphere, distill the solution under reduced pressure, wash with acetone, and dry to obtain a hyperbranched polyurethane-amide acid.
[0008] The structural formula of the carbamate dianhydride monomer is as follows:
[0009] ;
[0010] Step S2: adding ethanol, nano zinc oxide, and hyperbranched polyurethane-amic acid into a reaction bottle provided with a condenser reflux tube, performing surface modification after ultrasonic dispersion, centrifugal separation, washing with N,N-dimethylformamide and ethanol in sequence, and drying to obtain hyperbranched polyurethane-amic acid modified zinc oxide;
[0011] Step S3: Add dry polyol and 4,4'-methylenebis(phenyl isocyanate) into the reaction bottle, react at 75-85°C for 1.5-2.5h, then add chain extender and polyurethane-amide acid modified zinc oxide, stir and mix, add to a mold at a temperature of 100-110°C, place for 1-1.5h, demold and place in a heating box, and mature at 110-120°C for 18-30h to obtain a high-strength antibacterial thermoplastic polyurethane elastomer.
[0012] Preferably, in step S1, the mass ratio of the carbamate dianhydride monomer to tris(4-aminophenyl)methane is (290-310):100.
[0013] Preferably, in step S1, the reaction temperature is 20-30°C and the reaction time is 3-6h.
[0014] Preferably, in step S2, the mass ratio of nano zinc oxide to hyperbranched polyurethane-amic acid is 100:(80-300).
[0015] Preferably, in step S2, the surface modification temperature is 65-80° C. and the time is 1-4 h.
[0016] Preferably, in step S3, the mass ratio of the polyol, 4,4'-methylenebis(phenyl isocyanate), chain extender, and polyurethane-amic acid modified zinc oxide is 100:(30-33):(9-12):(2-12).
[0017] Preferably, the polyol is polytetramethylene glycol, polybutylene adipate glycol or polycaprolactone glycol.
[0018] Preferably, the chain extender is 1,4-butanediol or 1,6-hexanediol.
[0019] Preferably, the preparation method of the carbamate dianhydride monomer is as follows: toluene, 4,4'-methylenebis(phenyl isocyanate) in a mass ratio of 100:(130-140):(1.3-1.6), 4-hydroxyphthalic anhydride, and dibutyltin dilaurate are added into a reaction bottle, reacted at 50-60° C. for 2-3 hours, the solution is distilled under reduced pressure, separated by silica gel column chromatography, and eluted with a solution of ethyl acetate and petroleum ether to obtain a carbamate dianhydride monomer.
[0020] Technical effect: The present invention uses a novel carbamate dianhydride monomer to react with tri(4-aminophenyl)methane to obtain a hyperbranched polyurethane-amic acid, which contains a large number of carboxyl groups and can interact with the hydroxyl groups on the surface of nano zinc oxide by esterification reaction, thereby achieving surface modification of nano zinc oxide.
[0021] The invention uses polybutylene adipate glycol diol as diol, 1,4-butanediol or 1,6-hexanediol as chain extender, and 4,4'-methylenebis(phenyl isocyanate) for polymerization reaction, and adds hyperbranched polyurethane-amic acid modified zinc oxide to obtain a high-strength antibacterial thermoplastic polyurethane elastomer. The hyperbranched polyurethane-amic acid molecular chain modified with nano zinc oxide contains a large number of carbamate groups ( ), which has the same carbamate structural unit as the polyurethane elastomer molecular chain, significantly improves the compatibility between nano zinc oxide and polyurethane elastomer, and has better dispersibility in the elastomer matrix. Nano zinc oxide has the characteristics of high specific surface area and high strength, and is evenly dispersed in the polyurethane elastomer matrix, which significantly improves the mechanical properties of the elastomer. The polyurethane-amic acid modified with zinc oxide has a three-dimensional hyperbranched molecular chain, and its carbamate group forms a hydrogen bond interpenetrating cross-linking network with the carbamate group of polyurethane, so that the polyurethane elastomer has better tensile strength, elongation at break and tear strength. At the same time, nano zinc oxide has good antibacterial and bactericidal properties, is evenly dispersed in the polyurethane elastomer, is not easy to agglomerate, has more antibacterial sites, and shows higher inhibition zone diameter and antibacterial properties against bacteria such as Escherichia coli. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] The average particle size of the nano zinc oxide of the present invention is 15nm. The molecular weight of the polytetrahydrofuran ether diol is 2000. The molecular weight of the polybutylene adipate diol is 2000. The molecular weight of the polycaprolactone diol is 2000.
[0024] Example 1: Preparation method of high-strength antibacterial thermoplastic polyurethane elastomer:
[0025] (1) Add 35 mL of toluene, 2 g of 4,4'-methylenebis(phenyl isocyanate), 2.8 g of 4-hydroxyphthalic anhydride, and 26 mg of dibutyltin dilaurate to a reaction flask, react at 55°C for 2 h, distill the solution under reduced pressure, separate by silica gel column chromatography, and elute with a solution of ethyl acetate and petroleum ether to obtain a carbamate dianhydride monomer. The reaction formula is as follows:
[0026] ;
[0027] (2) Add 90 mL of N,N-dimethylformamide, 6 g of carbamate dianhydride monomer, and 3 g of tris(4-aminophenyl)methane to a reaction flask, react at 25°C for 6 h in a nitrogen atmosphere, distill the solution under reduced pressure, wash with acetone, and dry to obtain a hyperbranched polyurethane-amic acid. The reaction formula is as follows:
[0028] ;
[0029] (3) Add 30 mL of ethanol, 2 g of nano zinc oxide, and 1.6 g of hyperbranched polyurethane-amic acid to a reaction bottle equipped with a condenser reflux tube, and after ultrasonic dispersion, stir at 70° C. for surface modification for 1 hour, centrifuge, wash with N,N-dimethylformamide and ethanol in turn, and dry to obtain hyperbranched polyurethane-amic acid modified zinc oxide;
[0030] (4) Add 50 g of dried polybutylene adipate diol 2000 and 16.5 g of 4,4'-methylenebis(phenyl isocyanate) into the reaction bottle, react at 85°C for 1.5 h, then add 4.5 g of chain extender 1,4-butanediol and 1 g of polyurethane-amide acid modified zinc oxide, stir and mix, add to a mold at a temperature of 110°C, leave for 1 h, demold and place in a heating box, and mature at 120°C for 18 h to obtain a high-strength antibacterial thermoplastic polyurethane elastomer.
[0031] Example 2: Preparation method of high-strength antibacterial thermoplastic polyurethane elastomer:
[0032] (1) Add 25 mL of toluene, 2 g of 4,4'-methylenebis(phenyl isocyanate), 2.6 g of 4-hydroxyphthalic anhydride, and 32 mg of dibutyltin dilaurate to a reaction bottle, react at 60°C for 2 h, distill the solution under reduced pressure, separate by silica gel column chromatography, and elute with a solution of ethyl acetate and petroleum ether to obtain a carbamate dianhydride monomer;
[0033] (2) Add 80 mL of N,N-dimethylformamide, 6.3 g of carbamate dianhydride monomer, and 3 g of tri(4-aminophenyl)methane to a reaction bottle, react at 20° C. in a nitrogen atmosphere for 6 h, distill the solution under reduced pressure, wash with acetone, and dry to obtain a hyperbranched polyurethane-amic acid;
[0034] (3) Add 50 mL of ethanol, 2 g of nano zinc oxide, and 4 g of hyperbranched polyurethane-amic acid to a reaction bottle equipped with a condenser reflux tube, and after ultrasonic dispersion, stir at 65° C. for 4 h for surface modification, centrifuge, wash with N,N-dimethylformamide and ethanol in turn, and dry to obtain hyperbranched polyurethane-amic acid modified zinc oxide;
[0035] (4) Add 50 g of dry polytetramethylene ether glycol 2000 and 16.5 g of 4,4'-methylenebis(phenyl isocyanate) into the reaction bottle, react at 80°C for 1.5 h, then add 4.5 g of chain extender 1,6-hexanediol and 3 g of polyurethane-amide acid modified zinc oxide, stir and mix, add to a mold at a temperature of 100°C, leave for 1 h, demold and place in a heating box, and mature at 120°C for 24 h to obtain a high-strength antibacterial thermoplastic polyurethane elastomer.
[0036] Example 3: Preparation method of high-strength antibacterial thermoplastic polyurethane elastomer:
[0037] (1) Add 35 mL of toluene, 2 g of 4,4'-methylenebis(phenyl isocyanate), 2.8 g of 4-hydroxyphthalic anhydride, and 30 mg of dibutyltin dilaurate to a reaction bottle, react at 50°C for 3 h, distill the solution under reduced pressure, separate by silica gel column chromatography, and elute with a solution of ethyl acetate and petroleum ether to obtain a carbamate dianhydride monomer;
[0038] (2) Add 80 mL of N,N-dimethylformamide, 5.7 g of carbamate dianhydride monomer, and 3 g of tri(4-aminophenyl)methane to a reaction bottle, react at 30° C. for 3 h in a nitrogen atmosphere, distill the solution under reduced pressure, wash with acetone, and dry to obtain a hyperbranched polyurethane-amic acid;
[0039] (3) Add 60 mL of ethanol, 2 g of nano zinc oxide, and 6 g of hyperbranched polyurethane-amic acid to a reaction bottle equipped with a condenser reflux tube, and after ultrasonic dispersion, stir at 80° C. for surface modification for 3 h, centrifuge, wash with N,N-dimethylformamide and ethanol in turn, and dry to obtain hyperbranched polyurethane-amic acid modified zinc oxide;
[0040] (4) Add 50 g of dried polycaprolactone diol 2000 and 15 g of 4,4'-methylenebis(phenyl isocyanate) into the reaction bottle, react at 75°C for 2.5 h, then add 6 g of chain extender 1,4-butanediol and 6 g of polyurethane-amide acid modified zinc oxide, stir and mix, add to a mold at a temperature of 110°C, leave for 1 h, demold and place in a heating box, and mature at 110°C for 30 h to obtain a high-strength antibacterial thermoplastic polyurethane elastomer.
[0041] Comparative Example 1:
[0042] The difference between this comparative example and Example 1 is that the polyurethane-amic acid modified zinc oxide is not added to the polyurethane elastomer.
[0043] (1) Add 50 g of dried polybutylene adipate diol 2000 and 16.5 g of 4,4'-methylenebis(phenyl isocyanate) into a reaction bottle, react at 85°C for 1.5 h, then add 4.5 g of chain extender 1,4-butanediol, stir and mix, add to a mold at a temperature of 110°C, leave for 1 h, demold and place in a heating box, and mature at 120°C for 18 h to obtain a thermoplastic polyurethane elastomer.
[0044] Comparative Example 2:
[0045] The difference between this comparative example and Example 1 is that unmodified nano zinc oxide is added to the polyurethane elastomer.
[0046] (1) Add 50 g of dried polybutylene adipate diol 2000 and 16.5 g of 4,4'-methylenebis(phenyl isocyanate) into a reaction bottle, react at 85°C for 1.5 h, then add 4.5 g of chain extender 1,4-butanediol and 1 g of nano zinc oxide, stir and mix, add to a mold at a temperature of 110°C, leave for 1 h, demold and place in a heating box, and mature at 120°C for 18 h to obtain a thermoplastic polyurethane elastomer.
[0047] Comparative Example 3:
[0048] The difference between this comparative example and Example 1 is that, in preparing the hyperbranched polyamic acid, 3,3',4,4'-biphenyltetracarboxylic dianhydride monomer is used instead of the carbamate dianhydride monomer.
[0049] (1) Add 90 mL of N,N-dimethylformamide, 6 g of 3,3',4,4'-biphenyltetracarboxylic dianhydride, and 3 g of tris(4-aminophenyl)methane to a reaction bottle, react at 25° C. in a nitrogen atmosphere for 6 h, distill the solution under reduced pressure, wash with acetone, and dry to obtain a hyperbranched polyamic acid;
[0050] (2) Add 30 mL of ethanol, 2 g of nano zinc oxide, and 1.6 g of hyperbranched polyamic acid to a reaction bottle equipped with a condenser reflux tube, and after ultrasonic dispersion, stir at 70° C. for surface modification for 1 hour, centrifuge, wash with N,N-dimethylformamide and ethanol in turn, and dry to obtain hyperbranched polyamic acid-modified zinc oxide;
[0051] (3) Add 50 g of dried polybutylene adipate diol 2000 and 16.5 g of 4,4'-methylenebis(phenyl isocyanate) into a reaction bottle, react at 85°C for 1.5 h, then add 4.5 g of chain extender 1,4-butanediol and 1 g of hyperbranched polyamic acid modified zinc oxide, stir and mix, add to a mold at a temperature of 110°C, leave for 1 h, demold and place in a heating box, and mature at 120°C for 18 h to obtain a thermoplastic polyurethane elastomer.
[0052] Comparative Example 4:
[0053] The difference between this comparative example and Example 1 is that, in preparing the polyurethane-amic acid, 4,4'-diaminodiphenylmethane is used instead of tris(4-aminophenyl)methane.
[0054] (1) Add 90 mL of N,N-dimethylformamide, 6 g of carbamate dianhydride monomer, and 3 g of 4,4'-diaminodiphenylmethane into a reaction bottle, react at 25°C for 6 h in a nitrogen atmosphere, distill the solution under reduced pressure, wash with acetone, and dry to obtain polyurethane-amic acid;
[0055] (2) Add 30 mL of ethanol, 2 g of nano zinc oxide, and 1.6 g of polyurethane-amic acid to a reaction bottle equipped with a condenser reflux tube, and after ultrasonic dispersion, stir at 70°C for surface modification for 1 hour, centrifuge, wash with N,N-dimethylformamide and ethanol in turn, and dry to obtain polyurethane-amic acid modified zinc oxide;
[0056] (3) Add 50 g of dried polybutylene adipate diol 2000 and 16.5 g of 4,4'-methylenebis(phenyl isocyanate) into a reaction bottle, react at 85°C for 1.5 h, then add 4.5 g of chain extender 1,4-butanediol and 1 g of polyurethane-amic acid modified zinc oxide, stir and mix, add to a mold at a temperature of 110°C, leave for 1 h, demold and place in a heating box, and mature at 120°C for 18 h to obtain a thermoplastic polyurethane elastomer.
[0057] Comparative Example 5:
[0058] The difference between this comparative example and Example 1 is that the polyurethane-amic acid modified zinc oxide is not added to the polyurethane elastomer, but hyperbranched polyurethane-amic acid is added.
[0059] (1) Add 50 g of dried polybutylene adipate diol 2000 and 16.5 g of 4,4'-methylenebis(phenyl isocyanate) into a reaction bottle, react at 85°C for 1.5 h, then add 4.5 g of chain extender 1,4-butanediol and 1 g of hyperbranched polyurethane-amide acid, stir and mix, add to a mold at a temperature of 110°C, leave for 1 h, demold and place in a heating box, and mature at 120°C for 18 h to obtain a thermoplastic polyurethane elastomer.
[0060] The cured polyurethane elastomer was placed at room temperature for 7 days. The tensile stress-strain properties were tested according to GB / T 528-2009. The tear strength was tested according to GB / T 529-2008. The test results are shown in the following table. Table 1: Mechanical properties test results of various embodiments and comparative examples
[0061]
[0062] As shown in Table 1, polyurethane-amic acid modified zinc oxide is not added to the polyurethane elastomer of Comparative Example 1. Its tensile strength is 22.3 MPa, elongation at break is 620.7%, and tear strength is 87.3 kN / m.
[0063] Hyperbranched polyurethane-amic acid modified zinc oxide is added to the polyurethane elastomers in Examples 1 to 3. After the zinc oxide is surface-modified with the hyperbranched polyurethane-amic acid, it has better compatibility with the polyurethane elastomer and good dispersibility in the elastomer matrix, which significantly improves the mechanical properties of the elastomer. In addition, the polyurethane-amic acid modified with zinc oxide has a three-dimensional hyperbranched molecular chain, which forms a hydrogen bond interpenetrating cross-linking network with the polyurethane, so that the polyurethane elastomer has better tensile strength, elongation at break and tear strength.
[0064] The nano zinc oxide added in Comparative Example 2 has not been surface modified, has poor compatibility with the polyurethane elastomer, poor dispersibility, and does not significantly improve the mechanical properties of the elastomer.
[0065] Comparative Example 3 prepares a hyperbranched polyurethane-amic acid, and uses 3,3',4,4'-biphenyltetracarboxylic dianhydride monomer instead of the carbamate dianhydride monomer. The obtained hyperbranched polyamic acid does not contain a carbamate group, and its compatibility with the polyurethane elastomer is lower than that of the hyperbranched polyurethane-polyamic acid. After surface modification of nano-zinc oxide, the compatibility and dispersibility of the obtained hyperbranched polyamic acid-modified zinc oxide in the polyurethane elastomer are lower than those of the hyperbranched polyurethane-amic acid-modified zinc oxide in Example 1. Therefore, the tensile strength, elongation at break and tear strength of the polyurethane elastomer are lower than those in Example 1.
[0066] Comparative Example 4 prepares polyurethane-amic acid, using 4,4'-diaminodiphenylmethane instead of tris(4-aminophenyl)methane. The obtained polyurethane-amic acid does not contain a three-dimensional hyperbranched molecular structure, and has a low reinforcing effect on the polyurethane elastomer, resulting in lower tensile strength, elongation at break and tear strength than Example 1.
[0067] The polyurethane elastomer of Comparative Example 5 is added with hyperbranched polyurethane-amic acid, but without polyurethane-amic acid modified zinc oxide. Its tensile strength and other properties are higher than those of Comparative Example 1, but without zinc oxide, its tensile strength and other properties are lower than those of Example 1.
[0068] The polyurethane elastomer was cut into sheets and pressed into a polyurethane film with a thickness of 1 mm; sterilized under ultraviolet light. Escherichia coli, Staphylococcus aureus and Candida albicans were activated at 37°C for 24 h and gradiently diluted to a concentration of 10 7 cfu / mL bacterial suspension. Then, 0.1 mL of the bacterial suspension was transferred to the surface of the beef extract peptone agar medium, and then the polyurethane film was attached to the surface of the medium, placed in a constant temperature incubator, and cultured at 37 for 24 hours, and the diameter of the inhibition zone was measured. Each group of film samples was tested 5 times and the average value was taken. The test results are shown in the following table. Table 2: Antibacterial performance test results of each embodiment and comparative example
[0069]
[0070] As can be seen from Table 2, the nano zinc oxide in Examples 1 to 3 and Comparative Example 4 is surface modified with polyurethane-polyamic acid, which significantly improves the dispersibility of nano zinc oxide in the polyurethane elastomer. The better the dispersibility, the more antibacterial sites there are, the better the antibacterial performance of the elastomer against bacteria such as Escherichia coli, and the higher the inhibition zone diameter.
[0071] Comparative Examples 1 and 5 did not add nano zinc oxide, and the polyurethane elastomer did not have an inhibition zone diameter against bacteria such as Escherichia coli.
[0072] The nano zinc oxide in Comparative Example 2 has not been surface modified, has poor dispersibility in the polyurethane elastomer, and is easily agglomerated, resulting in a lower diameter of the inhibition zone.
[0073] The compatibility and dispersibility of the hyperbranched polyamic acid-modified zinc oxide in the polyurethane elastomer of Comparative Example 3 are lower than those of the hyperbranched polyurethane-amic acid-modified zinc oxide in Example 1, resulting in a lower inhibition zone diameter than that in Example 1.
Claims
1. A method for preparing a high-strength antibacterial thermoplastic polyurethane elastomer, characterized in that: The preparation method is: Step S1: Add N,N-dimethylformamide, carbamate dianhydride monomer, and tri(4-aminophenyl)methane into a reaction bottle, react in a nitrogen atmosphere, and distill the solution under reduced pressure, wash, and dry to obtain a hyperbranched polyurethane-amic acid; The structural formula of the carbamate dianhydride monomer is as follows: ; Step S2: adding ethanol, nano zinc oxide, and hyperbranched polyurethane-amic acid into a reaction bottle provided with a condenser reflux tube, performing surface modification after ultrasonic dispersion, centrifugal separation, washing, and drying to obtain hyperbranched polyurethane-amic acid modified zinc oxide; Step S3: Add dry polyol and 4,4'-methylenebis(phenyl isocyanate) into the reaction bottle, react at 75-85°C for 1.5-2.5h, then add chain extender and polyurethane-amide acid modified zinc oxide, stir and mix, add to a mold at a temperature of 100-110°C, place for 1-1.5h, demold and place in a heating box, and mature at 110-120°C for 18-30h to obtain a high-strength antibacterial thermoplastic polyurethane elastomer.
2. The method for preparing a high-strength antibacterial thermoplastic polyurethane elastomer according to claim 1, characterized in that: In the step S1, the mass ratio of the carbamate dianhydride monomer to tris(4-aminophenyl)methane is (290-310):
100.
3. The method for preparing a high-strength antibacterial thermoplastic polyurethane elastomer according to claim 1, characterized in that: In the step S1, the reaction temperature is 20-30°C and the reaction time is 3-6 hours.
4. The method for preparing a high-strength antibacterial thermoplastic polyurethane elastomer according to claim 1, characterized in that: In the step S2, the mass ratio of nano zinc oxide to hyperbranched polyurethane-amic acid is 100:(80-300).
5. The method for preparing a high-strength antibacterial thermoplastic polyurethane elastomer according to claim 1, characterized in that: In the step S2, the surface modification temperature is 65-80°C and the time is 1-4 hours.
6. The method for preparing a high-strength antibacterial thermoplastic polyurethane elastomer according to claim 1, characterized in that: In the step S3, the mass ratio of the polyol, 4,4'-methylenebis(phenyl isocyanate), chain extender, and polyurethane-amic acid modified zinc oxide is 100:(30-33):(9-12):(2-12).
7. The method for preparing a high-strength antibacterial thermoplastic polyurethane elastomer according to claim 1, characterized in that: The polyol is polytetramethylene glycol, polybutylene adipate glycol or polycaprolactone glycol.
8. The method for preparing a high-strength antibacterial thermoplastic polyurethane elastomer according to claim 1, characterized in that: The chain extender is 1,4-butanediol or 1,6-hexanediol.
9. The method for preparing a high-strength antibacterial thermoplastic polyurethane elastomer according to claim 1, characterized in that: The preparation method of the carbamate dianhydride monomer comprises the following steps: adding toluene, 4,4'-methylenebis(phenyl isocyanate), 4-hydroxyphthalic anhydride and dibutyltin dilaurate into a reaction bottle, reacting at 50-60° C. for 2-3 hours, distilling the solution under reduced pressure, separating by silica gel column chromatography, and eluting with a solution of ethyl acetate and petroleum ether to obtain the carbamate dianhydride monomer.
10. The method for preparing a high-strength antibacterial thermoplastic polyurethane elastomer according to claim 9, characterized in that: The mass ratio of the 4,4'-methylenebis(phenyl isocyanate), 4-hydroxyphthalic anhydride and dibutyltin dilaurate is 100:(130-140):(1.3-1.6).