A polymer microsphere material and its preparation method and application
By introducing a functional transition layer into the polymer microsphere material to form a micron-level three-layer core-shell structure, the problems of high swelling rate and insufficient structural stability of polymer microsphere materials in the prior art are solved, and the battery cell is improved stiffness and mechanical and safety performance of the battery.
Patent Information
- Application Number
- CN202411110981.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-14
AI Technical Summary
The existing polymer microsphere materials used in secondary battery separators have problems such as high swelling rate, insufficient structural stability and uneven particle size distribution, resulting in serious defects such as bond failure, diaphragm folds or cell deformation.
Polymer microsphere materials with a micron-scale three-layer core-shell structure include core layer, transition layer and shell layer. By introducing a functional transition layer, the connectivity is enhanced and the particle size uniformity and adhesion of polymer microspheres are improved. Solve the problems of swelling and insufficient structural stability.
It realizes that the cell stiffness is improved, the diaphragm wrinkles and deformation are prevented, and the mechanical and safety performance of the battery is enhanced while ensuring the bonding performance of the electrode.
Smart Images

Figure CN118638326B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of core-shell polymer materials, and in particular to a polymer microsphere material and a preparation method and application thereof. Background Art
[0002] In recent years, polymer microspheres have attracted increasing attention as separator coating materials in the field of battery separators. For example, polymer microspheres are coated on the surface of the separator to achieve the bonding function between the separator and the electrode, or to adjust the mechanical properties of the separator itself; for example, polymer microspheres are used as separator modification materials to improve the thermal response performance, ionic conductivity, stability performance, etc. of the separator, thereby improving the safety performance or electrical performance of the battery.
[0003] CN202110675299.0 discloses a battery separator, including a base film and a coating, wherein the coating includes a core-shell sphere, an inorganic substance, a thickener, and an aqueous adhesive; the core-shell sphere includes a core and a shell coated outside the core, the glass transition temperature of the core is 10°C, the glass transition temperature of the shell is 60°C, and the materials of the core and the shell are both polymethyl methacrylate. This prior art can effectively enhance the bonding ability of the separator through an inorganic-organic composite separator coating, and at the same time realize the transformation of the shell and the core into a highly elastic state during hot pressing, thereby avoiding the separation of the coating from the base film. However, the prior art still includes a high content of ceramic or ceramic-like inorganic components, which has the defect of insufficient thermal stability, and still causes cracks in the coating itself during hot pressing or drying and winding; in addition, the core-shell sphere is a two-layer polymethyl methacrylate, and no other structures or functional groups are introduced. Therefore, the functionality of the core-shell sphere is relatively simple, and its performance in other aspects except the bonding ability with the base film is average. There is still much room for improvement in mechanical strength, electrolyte resistance or electrolyte affinity.
[0004] CN202211325940.9 discloses a large-size core-shell polymer particle and its preparation method and application; the designed core-shell polymer particle has a particle size D50 of 1~50μm, and its structure includes a water-insoluble soft material layer and a hard material layer, the weight ratio of the soft material layer to the hard material layer is 1:0.1~10, and the hard material layer is located on the outer layer of the soft material layer. The polymer particles of the prior art can improve the hardness of the battery core and inhibit the deformation of the battery core without affecting the air permeability; at the same time, compared with the general micron-level homogeneous polymer particles, the soft core and hard shell structure it has is also conducive to improving the performance of the diaphragm. The hard material layer located on the outer layer of the particle ensures that the diaphragm coating is not sticky after drying, so the diaphragm will not stick to each other after rolling up; and the soft material layer located in the inner layer of the particle can provide a strong adhesive force, so that the diaphragm and the pole piece have a higher peel strength. However, after in-depth research, it was found that although the existing technology can meet the bonding requirements of the secondary battery diaphragm and the pole piece and can improve the problem of battery cell rigidity, further test results show that the polymer microspheres provided by it have a high swelling rate in the electrolyte; when used for a long time, the excessive swelling of the polymer microspheres may lead to serious technical defects such as bonding failure, blocking ion transmission channels, causing diaphragm wrinkles or battery cell deformation. In addition, after the emulsion containing polymer microspheres is applied to the diaphragm and dried and rolled up, during the storage process, the microspheres may be squeezed and ruptured due to the long-term rolling tension, causing the diaphragm to stick and the product to fail.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The first purpose of the present invention is to provide a polymer microsphere material, specifically a polymer microsphere material with a micron-level three-layer core-shell structure; it is mainly used to solve the technical defects of existing polymer coating materials used for secondary battery separators, such as high swelling rate, insufficient structural stability, and uneven particle size distribution.
[0007] The second purpose of the present invention is to provide a method for preparing the polymer microsphere material, which is simple and easy to implement and can meet the needs of mass production.
[0008] The third object of the present invention is to provide a separator for a secondary battery, which can improve the rigidity of the battery cell while ensuring the adhesion performance with the electrode, so that it is not easy to wrinkle, open or deform.
[0009] A fourth object of the present invention is to provide a secondary battery, which effectively enhances the mechanical properties and safety performance of the battery as a whole by coating a modified separator with polymer microspheres.
[0010] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0011] A polymer microsphere material comprises a core layer, a transition layer and a shell layer from inside to outside;
[0012] The core layer comprises a first modified acrylate copolymer, and the glass transition temperature of the first modified acrylate copolymer is ≤35°C; the transition layer comprises at least one functional monomer polymerized; the shell layer comprises a second modified acrylate copolymer, and the glass transition temperature of the second modified acrylate copolymer is 60°C to 250°C;
[0013] The raw materials of the transition layer include functional monomers, and the functional monomers include at least one of a front-end cross-linking monomer, a strong polar monomer or a long side chain monomer; wherein the front-end cross-linking monomer contains at least two polymerizable alkenyl functional groups; the functional groups of the strong polar monomer include at least one of a hydroxyl group, a carbonyl group, an acyloxy group, an ether bond, an epoxy group, an amine group, a sulfonic acid group, and an aromatic ring containing a substituent; the side group of the long side chain monomer includes at least one carbon chain or carbon-oxygen chain with a carbon number ≥4.
[0014] Preferably, the mass of the transition layer is 5wt.%~85wt.% of the core layer, and the mass of the shell layer is 5wt.%~200wt.% of the sum of the core layer and the transition layer.
[0015] Preferably, the first modified acrylate copolymer is prepared by including the following components in parts by weight: 45-85 parts of water-insoluble soft monomers, 15-35 parts of water-insoluble hard monomers, 5-20 parts of water-soluble organic acid monomers, 0.001-5 parts of non-ionic surfactants, 0.065-5 parts of water-soluble initiators and some deionized water.
[0016] Preferably, the second modified acrylate copolymer is prepared by including the following components in parts by weight: 50-95 parts of water-insoluble hard monomer, 0.1-15 parts of front-end crosslinking monomer, 0.056-3.9 parts of water-soluble initiator and some deionized water.
[0017] Preferably, the diameter of the polymer microsphere material is 1 μm to 50 μm.
[0018] A method for preparing the polymer microsphere material comprises the following steps:
[0019] (1) The raw material components of the core layer are fully mixed and polymerized to obtain a core layer emulsion;
[0020] (2) adding the raw material components of the transition layer to the core layer emulsion, and performing a second polymerization reaction to obtain a core emulsion coated with the transition layer;
[0021] (3) Adding the raw material components of the shell layer to the core emulsion of the coating transition layer, performing a third polymerization reaction, and obtaining an emulsion containing the polymer microsphere material.
[0022] Preferably, the polymerization reaction temperature is 55° C. to 75° C., and the polymerization reaction insulation time is 12 h to 15 h.
[0023] Preferably, the temperature of the second polymerization reaction is 70° C. to 90° C., and the insulation time of the second polymerization reaction is 0.5 h to 3 h.
[0024] Preferably, the temperature of the third polymerization reaction is 70° C. to 90° C., and the insulation time of the third polymerization reaction is 1 h to 3 h.
[0025] A separator for a secondary battery comprises the polymer microsphere material.
[0026] A secondary battery comprises the separator for a secondary battery as described above.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] The present invention provides a polymer microsphere material with a micron-scale, three-layer core-shell structure for use in the field of secondary battery separator coatings, including an innermost core layer, an outermost shell layer, and a functional transition layer between the two. The polymer microsphere material of the present invention has good particle size uniformity, good adhesion to the separator, and good rolling and anti-sticking properties. By introducing a functional transition layer, the present invention can effectively enhance the connectivity between the soft core layer and the hard shell layer, making the core-shell structure more compact and strong as a whole; at the same time, it can also effectively solve the structural defects of excessive swelling of the polymer microspheres and easy rupture under long-term pressure.
[0029] The present invention provides a diaphragm and a secondary battery comprising the polymer microsphere material; specifically, the diaphragm with the polymer microsphere material coated on the surface is assembled with the positive and negative electrodes of the battery to obtain a battery cell, and after the battery cell is subjected to a certain temperature and pressure treatment, the diaphragm and the electrode are fixedly connected through the bonding effect of the polymer microsphere material, while the rigidity of the battery cell is improved, and the swelling rate is low in a long-term electrolyte immersion environment; thereby, a secondary battery with good mechanical properties and safety performance is obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0031] Figure 1 Provides a particle size distribution diagram of Example 5 of the present invention;
[0032] Figure 2 The SEM image of Example 5 of the present invention is provided. DETAILED DESCRIPTION
[0033] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but those skilled in the art will appreciate that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. Those who do not specify specific conditions in the embodiments are carried out according to conventional conditions or conditions recommended by the manufacturer. Those who do not specify the manufacturer of the reagents or instruments used are all conventional products that can be purchased commercially. In addition, the terms "one", "two", "1", "2" are only used for descriptive purposes and cannot be interpreted as indicating or implying relative importance.
[0034] The first aspect of the present invention is to provide a polymer microsphere material, comprising a core layer, a transition layer and a shell layer from inside to outside; wherein the core layer comprises a first modified acrylate copolymer, and the glass transition temperature of the first modified acrylate copolymer is ≤35°C; the transition layer comprises at least one functional monomer obtained by polymerization; the shell layer comprises a second modified acrylate copolymer, and the glass transition temperature of the second modified acrylate copolymer is 60°C~250°C.
[0035] As a preferred embodiment, in the polymer microsphere material, the diameter of the microspheres is 1 μm to 50 μm, in some more preferred embodiments the diameter is 1.5 μm to 25 μm, and in a further preferred embodiment the diameter is 2 μm to 10 μm.
[0036] As a preferred embodiment, the mass of the transition layer is 5wt.%~85wt.% of the core layer; in some more preferred embodiments, the ratio is taken from 10wt.%~20wt.% or 55wt.%~70wt.%; in some optional embodiments, the mass ratio of the transition layer to the core layer includes but is not limited to 5%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 75%, 80%, 85%, any one of them or a numerical range composed of any two of them.
[0037] As a preferred embodiment, the mass of the shell layer is 5wt.%~200wt.% of the sum of the core layer and the transition layer; in some more preferred embodiments, the ratio is taken from 10wt.%~20wt.% or 100wt.%~120wt.%; in some optional embodiments, the ratio of the mass of the shell layer to the sum of the mass of the core layer and the transition layer includes but is not limited to 5%, 10%, 20%, 40%, 50%, 60%, 80%, 100%, 120%, 140%, 150%, 160%, 180%, 200%, any one of them or the numerical range composed of any two of them.
[0038] As a preferred embodiment, the glass transition temperature of the first modified acrylate copolymer includes but is not limited to any one of 35, 30, 25, 20, 15, 10, 5, 1, 0 (°C) or a numerical range consisting of any two thereof; in some more preferred embodiments, the glass transition temperature of the first modified acrylate copolymer is calculated by the following formula:
[0039] ;
[0040] Among them, T g is the glass transition temperature of the first modified acrylate copolymer, i is the monomer number (i.e. the i-th monomer), w i is the mass fraction of the ith monomer in the total monomers, T gi is the glass transition temperature of the ith monomer.
[0041] In the present invention, the core layer mainly plays a bonding role; as a preferred embodiment, the first modified acrylate copolymer is prepared by comprising the following components: a water-insoluble soft monomer, a water-insoluble hard monomer, a water-soluble organic acid monomer, a non-ionic surfactant, a water-soluble initiator and deionized water; in some more preferred embodiments, the first modified acrylate copolymer is prepared by comprising the following components in parts by weight: 45 to 85 parts of a water-insoluble soft monomer, 15 to 35 parts of a water-insoluble hard monomer, 5 to 20 parts of a water-soluble organic acid monomer, 0.001 to 2.8 parts of a non-ionic surfactant, 0.065 to 2.8 parts of a water-soluble initiator and some deionized water.
[0042] In some more preferred embodiments, the function of the water-insoluble soft monomer is to provide initial adhesion for the core layer, and the water-insoluble soft monomer includes an acrylate compound containing an olefinic functional group; the solubility of the water-insoluble soft monomer (25°C, water environment) is ≤30g / L, the solubility of the homopolymer of the water-insoluble soft monomer (25°C, water environment) is ≤1g / L, and the glass transition temperature of the homopolymer of the water-insoluble soft monomer is ≤0°C; in a further preferred embodiment, the water-insoluble soft monomer includes but is not limited to at least one of n-butyl acrylate, n-octadecyl acrylate, isooctyl acrylate, lauryl acrylate or vinyl neodecanoate.
[0043] In some more preferred embodiments, the function of the water-insoluble hard monomer is to provide the core layer with a holding force; the glass transition temperature of the homopolymer of the water-insoluble hard monomer is ≥60°C, and in further preferred embodiments, the glass transition temperature of the homopolymer of the water-insoluble hard monomer is 70°C~200°C; the solubility of the homopolymer of the water-insoluble hard monomer is ≤1g / L; the solubility of the water-insoluble hard monomer is 10g / L~90g / L or 0~5g / L, and it is divided into a first water-insoluble hard monomer and a second water-insoluble hard monomer according to the above two solubility ranges; in further preferred embodiments, ...≥60°C; the glass transition temperature of the homopolymer of the water-insoluble hard monomer is 70°C~200°C; the solubility of the homopolymer of the water-insoluble hard monomer is ≤1g / L; the solubility of the water-insoluble hard monomer is 10g / L~90g / L or 0~5g / L, and it is divided into a first water-insoluble hard monomer and a second water-insoluble hard monomer according to the above two solubility ranges; In an embodiment, the first water-insoluble hard monomer includes at least one of methyl methacrylate or acrylonitrile, and the second water-insoluble hard monomer includes at least one of styrene or tert-butyl methacrylate; in an optional embodiment, the mass ratio of the first water-insoluble hard monomer to the second water-insoluble hard monomer is 9:1~1:9. It can be understood that core layer polymers with different particle sizes and distributions can be obtained by the mass ratio of the two water-insoluble hard monomers. When the amount of the first water-insoluble hard monomer is higher, the particle size of the core layer polymer is higher and the distribution is wider, and vice versa.
[0044] In some more preferred embodiments, the water-soluble organic acid monomer mainly serves to improve the adhesion of the core layer and the electrolyte resistance; the solubility (25°C, water environment) of the water-soluble organic acid monomer and its homopolymer (the degree of polymerization of the homopolymer is <1000) is ≥50g / L; the water-soluble organic acid monomer used in the present invention is ionized in water to obtain at least one hydrogen ion, and is divided into a first water-soluble organic acid monomer (pKa ≥ 3.0) and a second water-soluble organic acid monomer (pKa <3.0) according to the ionization ability; in a further preferred embodiment, the first water-soluble organic acid monomer includes but is not limited to propylene At least one of olefinic acid, maleic acid, itaconic acid or p-vinylphenol; the second water-soluble organic acid monomer includes but is not limited to at least one of p-styrene sulfonic acid, 2-acrylamide-2-methylpropane sulfonic acid or allyl sulfonic acid; in an optional embodiment, the mass ratio of the first water-soluble organic acid monomer to the second water-soluble organic acid monomer is 1:1~10:1. It can be understood that core layer polymers with different particle sizes and distributions can be obtained by the mass ratio of the two water-soluble organic acid monomers. When the amount of the first non-water-soluble hard monomer is higher, the particle size of the core layer polymer is higher and the distribution is wider, and vice versa.
[0045] In some more preferred embodiments, the function of the non-ionic surfactant is to prevent the core layer product particles from agglomerating and precipitating, maintain the stability of the emulsion, and assist in regulating the particle size; the non-ionic surfactant selected for the present invention is a water-soluble polymer that does not ionize after being dissolved in water; in a further preferred embodiment, the non-ionic surfactant includes but is not limited to at least one of polyvinyl alcohol, polyoxyethylene ether, polyvinyl pyrrolidone or hydroxyethyl cellulose; it can be understood that the higher the mass proportion of the non-ionic surfactant in the core layer raw material, the smaller the particle size of the core layer polymer, and the higher the stability of the obtained core layer.
[0046] In some more preferred embodiments, the water-soluble initiator functions to promote the polymerization reaction of the core layer raw materials; the water-soluble initiator is selected from persulfate compounds, including but not limited to at least one of ammonium persulfate, potassium persulfate or sodium persulfate.
[0047] In some more preferred embodiments, by adjusting the amount of the deionized water, the solid content of the core layer is 10% to 35%, and more preferably 15% to 25%.
[0048] In some more preferred embodiments, the raw material components of the first modified acrylate copolymer also include: a water-soluble neutralizing agent, including but not limited to at least one of alkali metal hydroxides (such as lithium hydroxide, sodium hydroxide, etc.), ammonia water or a monobasic saturated organic amine; in a further preferred embodiment, the amount of the water-soluble neutralizing agent is 70% to 120% of the molar amount of hydrogen ions generated by the ionization of the water-soluble organic acid monomer.
[0049] In some more preferred embodiments, the raw material components of the first modified acrylate copolymer also include: 1 to 10 parts of water-soluble non-electrolyte monomers. Based on its name, it can be seen that this type of monomer is water-soluble and does not ionize after dissolution. Its function is to assist in regulating the particle size of the core layer polymer. By adding water-soluble non-electrolyte monomers, a core layer product with a narrower particle size distribution is obtained; the water-soluble non-electrolyte monomer and its homopolymer (homopolymer polymer ≤ 1000) ≥ 50g / L; in a further preferred embodiment, the water-soluble non-electrolyte monomer includes but is not limited to at least one of acrylamide or hydroxyethyl acrylate.
[0050] In some more preferred embodiments, the raw material components of the first modified acrylate copolymer also include: 0.01 to 10 parts of a front-end cross-linking monomer, whose water solubility is not limited, but should contain at least two polymerizable alkenyl functional groups and complete cross-linking in the polymerization reaction of the core layer, and its function is to improve the bonding strength and electrolyte resistance of the core layer; in a further preferred embodiment, the first modified acrylate copolymer includes but is not limited to at least one of ethylene glycol dimethacrylate, trimethylolpropane trimethacrylate or pentaerythritol tetramethacrylate.
[0051] In some more preferred embodiments, the raw material components of the first modified acrylate copolymer also include: anionic surfactants, which function to assist in improving the stability of the core layer, including but not limited to at least one of sodium dodecyl sulfate or sodium octyl sulfosuccinate; in a further preferred embodiment, the mass ratio of the anionic surfactant to the non-ionic surfactant is 20% to 80%.
[0052] In the present invention, the transition layer is a homopolymer or copolymer synthesized based on several functional monomers, which may be water-soluble or water-insoluble, and generally has no effect on the particle size of the polymer microsphere material, but can significantly improve the key properties of the microsphere material such as adhesion and resistance to electrolyte swelling. Furthermore, when its dosage is limited within certain preferred ranges, specific related properties can be achieved; as a preferred embodiment, the raw materials (functional monomers) of the transition layer include at least one of a front-end cross-linking monomer, a strong polar monomer or a long side chain monomer.
[0053] In some more preferred embodiments, the front-end cross-linking monomer contains at least two polymerizable alkenyl-containing (meth) acrylate compounds to complete cross-linking during the polymerization process and form a dense cross-linking layer on the surface of the core layer to improve the electrolyte resistance of the polymer microsphere material; in a further preferred embodiment, the front-end cross-linking monomer includes but is not limited to at least one of ethylene glycol dimethacrylate, polyethylene glycol diacrylate, trimethylolpropane triacrylate, 1,6-hexanediol diacrylate or 1,4-butanediol diacrylate.
[0054] In some more preferred embodiments, the side group of the strongly polar monomer includes at least one strongly polar functional group, and the strongly polar functional group includes but is not limited to hydroxyl, carbonyl, acyloxy, ether bond, epoxy, amine, sulfonic acid, aromatic ring containing substituents, etc. The side group refers to a group on a non-main chain structure, and its function is to promote the interaction between the molecular chain and the positive and negative electrode active materials, thereby improving the adhesion ability to the electrode; in a further preferred embodiment, the strongly polar monomer includes but is not limited to at least one of tetrahydrofuran acrylate, carboxyethyl acrylate, hydroxyethyl acrylate, dimethylaminoethyl acrylate, 2-phenoxyethyl acrylate, ethoxyethoxyethyl acrylate, diacetone acrylamide or cyclotrimethylolpropane formal acrylate.
[0055] In some more preferred embodiments, the side group of the long side chain monomer includes at least one carbon chain or carbon-oxygen chain with a carbon number ≥ 4, which serves to improve the flexibility of the polymer microsphere material, change its mechanical properties after compression and better fit the electrode; in a further preferred embodiment, the long side chain monomer includes but is not limited to at least one of hydroxybutyl methacrylate, lauryl acrylate, PEG350MA or APEG2400.
[0056] In some more preferred embodiments, in addition to the functional monomers, the raw materials of the transition layer also include a transition layer initiator, which functions to promote the polymerization reaction of the functional monomers of the transition layer; the transition layer initiator is a persulfate compound, including but not limited to at least one of ammonium persulfate, potassium persulfate or sodium persulfate; in a further preferred embodiment, the amount of the transition layer initiator used is 0.1% to 2% of the total amount of the functional monomers by mass.
[0057] In some optional embodiments, in addition to the functional monomers, the raw materials of the transition layer also include water-soluble surfactants, including non-ionic surfactants and anionic surfactants. The specific ingredient selection is the same as the ingredient selection range of the corresponding surfactant in the core layer mentioned above, but it is not necessary to select the same surfactant as the core layer; in a further preferred embodiment, the amount of the water-soluble surfactant is 0.002%~2% of the total amount of the functional monomers by mass.
[0058] In some more preferred embodiments, in addition to the functional monomers, the raw materials of the transition layer also include a solvent of deionized water, and the amount of deionized water used is 1 to 5 times the mass of the total raw materials of the transition layer.
[0059] In the present invention, the shell layer mainly plays a supporting and shielding role. When the shell layer is compressed, it softens or breaks, thereby releasing the adhesive components of the core layer (and the transition layer); as a preferred embodiment, the second modified acrylate copolymer is prepared by comprising the following components: a water-insoluble hard monomer, a front-end cross-linking monomer, a water-soluble initiator and deionized water; in some more preferred embodiments, the second modified acrylate copolymer is prepared by comprising the following components in parts by weight: 50 to 95 parts of a water-insoluble hard monomer, 0.1 to 15 parts of a front-end cross-linking monomer, 0.056 to 3.9 parts of a water-soluble initiator and some deionized water.
[0060] As a more preferred embodiment, the role of the water-insoluble hard monomer in the shell layer is mainly to form the shell layer skeleton; the properties or component selection of the water-insoluble hard monomer are consistent with the water-insoluble hard monomer in the core layer, and will not be repeated here; but it can be understood that the property parameters of the water-insoluble hard monomer in the core layer and the shell layer are not necessarily the same, and the specific components selected are not necessarily the same. Those skilled in the art can make the same or different selections within the preferred range of the specification.
[0061] As a more preferred embodiment, the role of the front-end cross-linking monomer in the shell layer is mainly to cross-link during the polymerization of the shell layer and obtain a dense shell structure, thereby improving the supporting effect of the shell layer and improving the electrolyte resistance of the polymer microsphere material; the properties or component selection of the front-end cross-linking monomer are consistent with the front-end cross-linking monomer in the transition layer, and will not be repeated here; but it can be understood that the property parameters of the front-end cross-linking monomer in the core layer and the transition layer are not necessarily the same, and the specific components selected are not necessarily the same. Those skilled in the art can make the same or different selections within the preferred range of the specification.
[0062] As a more preferred embodiment, the water-soluble initiator functions to promote the polymerization reaction of the shell raw material; the water-soluble initiator is selected from persulfate compounds, including but not limited to at least one of ammonium persulfate, potassium persulfate or sodium persulfate.
[0063] As an optional embodiment, the raw material components of the second modified acrylate copolymer also include: 0.1 to 25 parts of a rear-end crosslinking monomer; the rear-end crosslinking monomer includes 1 polymerizable alkenyl functional group and at least 1 rear-end crosslinking group, wherein the rear-end crosslinking group refers to a group that does not react during the polymerization process, but reacts and forms a crosslink during the storage or use of the polymer microsphere material; the role of the rear-end crosslinking monomer is: on the one hand, it can make the shell layer denser, improve the supporting effect of the shell layer, and at the same time enhance the electrolyte resistance of the polymer microsphere; on the other hand, it can promote the formation of chemical bonds between the polymer microsphere and the adherend through the rear-end crosslinking effect, thereby enhancing the bonding ability of the polymer microsphere; in a further preferred embodiment, the rear-end crosslinking group includes but It is not limited to epoxy groups, siloxane groups, hydroxymethyl groups, hydroxyethyl groups or activated hydrogen atoms, etc. (wherein, the case of activated hydrogen atoms is illustrated by way of example: when a methylene group is connected to a carbon-carbon double bond or a carbon-oxygen double bond on both sides by a single bond, such as O=C-CH2-C=O, the hydrogen atoms on the methylene group are activated under the conjugation of the two double bonds and are easily formed into free radicals under the action of oxidative delocalization; those skilled in the art can judge whether the hydrogen atoms are activated based on the actual conditions of the hydrogen atoms); in a further optional embodiment, the rear-end cross-linking monomer includes but is not limited to at least one of N-hydroxymethyl acrylamide, γ-methacryloxypropyltrimethoxysilane, carboxybutyl acrylate, acetoacetoxyethyl methacrylate or glycidyl methacrylate.
[0064] As a further optional embodiment, when the raw material components of the second modified acrylate copolymer include the back-end cross-linking monomer, the second modified acrylate copolymer also includes a water-soluble external cross-linking agent for promoting the cross-linking reaction during storage or use of the polymer microspheres, and the water-soluble external cross-linking agent needs to be added to the product after the preparation polymerization reaction is completed and stirred evenly; in some optional embodiments, the back-end cross-linking monomer includes but is not limited to at least one of a polyamine, a polyacid anhydride or a protonic acid, and the molar ratio of the back-end cross-linking monomer to the back-end cross-linking monomer is 25%~100%.
[0065] As an optional embodiment, the raw material components of the second modified acrylate copolymer also include: 1 to 15 parts of a strong polar monomer, which serves to impart a stronger polarity to the shell layer and promote the interaction between the molecular chains of the polymer microspheres and the positive and negative electrode active materials, thereby enhancing the bonding ability of the polymer microsphere material; the properties or component selection of the strong polar monomer are consistent with the strong polar monomer in the transition layer, and will not be repeated here; but it can be understood that the property parameters of the strong polar monomer in the shell layer and the transition layer are not necessarily the same, and the specific components selected are not necessarily the same. Those skilled in the art can make the same or different selections within the preferred range of the specification.
[0066] As an optional embodiment, the raw material components of the second modified acrylate copolymer also include: 5 to 45 parts of a water-insoluble soft monomer, whose main function is to reduce the rigidity of the shell layer so that it is easier to soften or break when under pressure; the solubility of the water-insoluble soft monomer (25°C, water environment) is ≤30g / L, the solubility of the homopolymer of the water-insoluble soft monomer (25°C, water environment) is ≤1g / L, and the glass transition temperature of the homopolymer of the water-insoluble soft monomer is ≤35°C; the component selection of the water-insoluble soft monomer is consistent with the water-insoluble soft monomer in the core layer, and will not be repeated here; but it can be understood that the specific selected components of the water-insoluble soft monomer in the shell layer and the core layer are not necessarily the same, and those skilled in the art can make the same or different selections within the preferred range of the specification.
[0067] As an optional embodiment, the raw material components of the second modified acrylate copolymer also include: 0.001 to 3.9 parts of a water-soluble surfactant, which serves to improve the stability of the outer shell layer of the polymer microspheres; the properties or component selection of the water-soluble surfactant are consistent with those of the water-soluble surfactant in the transition layer, and will not be repeated here; but it can be understood that the property parameters of the water-soluble surfactant in the shell layer and the transition layer are not necessarily the same, and the specific components selected are not necessarily the same. Those skilled in the art can make the same or different selections within the preferred range of the specification.
[0068] As a further preferred embodiment, the mass of the deionized water is 1 to 5 times the total mass of the raw material components of the second modified acrylate copolymer (excluding the deionized water itself).
[0069] The second aspect of the present invention is to provide a method for preparing the polymer microsphere material as described in the first aspect, comprising the following steps (1) to (3):
[0070] (1) Preparation of the core layer: The raw material components of the core layer are fully mixed and subjected to polymerization reaction to obtain a core layer emulsion.
[0071] As a preferred embodiment, the polymerization reaction temperature is 55° C. to 75° C., and the polymerization reaction insulation time is 12 h to 15 h.
[0072] As a preferred embodiment, the polymerization reaction is carried out in an intermittent process. The intermittent process is a conventional preparation process in the art, specifically, the raw material components of the core layer except the initiator are fully mixed, the temperature is raised to the polymerization reaction temperature, the initiator is added, and the monomers are initiated at one time to carry out the polymerization reaction, so as to obtain the core layer emulsion.
[0073] (2) Preparation of core layer-transition layer: adding the raw material components of the transition layer to the core layer emulsion, performing a second polymerization reaction, and obtaining a core emulsion coated with the transition layer.
[0074] As a preferred embodiment, the temperature of the second polymerization reaction is 70° C. to 90° C., and the insulation time of the second polymerization reaction is 0.5 h to 3 h.
[0075] As a preferred embodiment, the second polymerization reaction is carried out by an intermittent process or a semi-continuous process; wherein the semi-continuous process is also a conventional preparation process in the art, specifically referring to: after the raw material components are fully mixed, they are gradually added to the core layer emulsion at a slow rate to achieve continuous initiation and conduction of the second polymerization reaction, and obtain the core emulsion of the coating transition layer.
[0076] (3) Preparation of core layer-transition layer-shell layer: adding the raw material components of the shell layer to the core emulsion of the coating transition layer, performing a third polymerization reaction, and obtaining an emulsion containing polymer microsphere material.
[0077] As a preferred implementation manner, the temperature of the third polymerization reaction is 70° C. to 90° C., and the insulation time of the third polymerization reaction is 1 h to 3 h.
[0078] As a preferred embodiment, the entire preparation method is carried out under a protective gas atmosphere.
[0079] The third aspect of the present invention is to provide a separator for a secondary battery, comprising the polymer microsphere material as described in the first aspect.
[0080] A fourth aspect of the present invention provides a secondary battery, comprising the separator for a secondary battery according to the third aspect.
[0081] As a preferred embodiment, the preparation method of the secondary battery comprises: coating an emulsion containing the polymer microsphere material on at least one side of a base film, and then assembling it with a positive electrode and a negative electrode, performing a pressurization treatment and obtaining a battery cell.
[0082] As a more preferred embodiment, the pressure of the pressurization treatment is 4±0.5 MPa, and the temperature of the pressurization treatment is 23±2°C.
[0083] Embodiment 1~6
[0084] S1: Preparation of core layer: The raw material components of the core layer are fully stirred and mixed, and after stirring for 30 minutes, a polymerization reaction is carried out at 60°C in a nitrogen atmosphere for 14 hours to obtain a core layer emulsion. The core layer raw materials of each embodiment are provided in Tables 1 and 2 below, wherein the numbers after the ingredients refer to the weight percentage of each raw material; the neutralization degree 100% in Table 1 means that the amount of M1-3-a is equivalent to the molar amount of hydrogen ions generated by the ionization of M1-3. It is also worth noting that the materials used in Tables 1 and 2 are all conventional commercial products.
[0085] S2: Preparation of core layer-transition layer: 100 parts of the core layer emulsion of each embodiment S1 (since the designed solid content is 21%±1%, the total non-volatile matter is calculated as 21 parts) are respectively put into a reaction container with nitrogen atmosphere, and then the raw material components of each transition layer are respectively put into the reaction container, and after fully stirring for 30 minutes, the temperature in the reaction container is raised to 80°C, and then the temperature is continued to be kept for 2 hours to obtain an intermediate emulsion (transition layer-core layer emulsion). The raw material components of the transition layer of each embodiment are provided as shown in Table 3 below, wherein the numbers after the ingredients refer to the weight parts of each raw material.
[0086] S3: Preparation of core layer-transition layer-shell layer: Take 400 parts of the emulsion prepared in S2 (since the designed solid content is 21%±1%, the total non-volatile matter is calculated as 84 parts), maintain 80°C and keep it in a stirring state; add the raw material components of the shell layer except the external cross-linking agent (M3-3-a) to each embodiment respectively, and complete the addition evenly within 4 hours; then continue to keep the reaction for 2 hours, cool to room temperature, add the external cross-linking agent (M3-3-a), stir evenly and collect the material to obtain the microsphere material of each embodiment. The raw material components of the shell layer of each embodiment are provided as shown in Table 4 below, where the numbers after the ingredients refer to the weight percentage of each raw material. In addition, the mass concentration of ammonia water in Table 4 is 25%.
[0087] Table 1
[0088]
[0089] Table 2
[0090]
[0091] Table 3
[0092]
[0093] Table 4
[0094]
[0095] Comparative Example 1
[0096] An aqueous suspension with a solid content of 21%±1%, a particle size (D50) of 3.1μm and a microsphere glass transition temperature of 40±2℃ was prepared by microsuspension polymerization method with 10 parts of methyl methacrylate, 10 parts of styrene, 8 parts of butyl acrylate and 0.14 parts of ethylene glycol dimethacrylate as monomers, deionized water as the dispersion system, azobisisobutyronitrile as the initiator, sodium dodecyl sulfate and polyvinyl alcohol as surfactants.
[0097] The microsuspension polymerization method in this comparative example refers to: after dissolving the initiator in the water-insoluble monomer, the dispersion system and the surfactant are added in sequence, and a microsuspension of monomer droplets is obtained by high-speed shear homogenization; then the temperature is raised to initiate polymerization to obtain the polymer microspheres of this comparative example.
[0098] Comparative Example 2
[0099] An aqueous suspension with a solid content of 21%±1%, a particle size (D50) of 5.5μm and a microsphere glass transition temperature of 75±2℃ was prepared by a dispersion polymerization method with 27 parts of styrene, 3 parts of butyl acrylate and 0.15 parts of p-divinylbenzene as monomers, a deionized water-ethanol mixed solution as a dispersion system, potassium persulfate as an initiator and polyvinyl pyrrolidone as a surfactant.
[0100] The dispersion polymerization method in this comparative example refers to: dissolving the monomer, initiator and surfactant in a dispersion system, and then heating to initiate polymerization; the generated polymer is continuously precipitated due to its insolubility, and is uniformly dispersed into spheres under the action of the surfactant to obtain the polymer microspheres of this comparative example.
[0101] Comparative Example 3
[0102] With 15 parts of methyl methacrylate, 15 parts of isobornyl methacrylate and 0.15 parts of ethylene glycol dimethacrylate as monomers, azobisisobutyronitrile as initiator, sodium dodecyl sulfate and polyvinyl alcohol as surfactants, a microsuspension polymerization method was used to prepare an aqueous suspension with a solid content of 21%±1%, a particle size (D50) of 4.5μm, and a microsphere glass transition temperature of ≥130°C. The implementation method of the microsuspension polymerization method is the same as that of Comparative Example 1.
[0103] Then, 10 parts of sodium acrylate, 40 parts of butyl acrylate, 10 parts of methyl methacrylate and 0.3 parts of 1,6-hexanediol diacrylate were used as monomers, sodium dodecyl sulfate was used as an emulsifier, and potassium persulfate was used as an initiator. A soft shell layer with a glass transition temperature of about -10°C was coated on the surface of the aforementioned microspheres through a semi-continuous method, and finally a core-shell structure microsphere aqueous suspension with a solid content of 21%±1% and a particle size (D50) of 4.8μm was obtained. Among them, the semi-continuous method in this comparative example means: after all the raw material components are fully mixed, they are gradually added to the aforementioned aqueous suspension at a slow speed to achieve continuous initiation and polymerization reaction, and the core-shell structure microsphere material of this comparative example is obtained.
[0104] Comparative Example 4
[0105] The particle size (D50) of a certain brand of commercially available water-based PVDF microspheres is nominally 7±1μm, but the actual measured value is 7.2μm.
[0106] Comparative Example 5
[0107] It is basically the same as Example 1, except that step S2 is cancelled.
[0108] Comparative Example 6
[0109] It is basically the same as Example 1, except that step S3 is cancelled.
[0110] Comparative Example 7
[0111] The method is basically the same as the first embodiment, except that steps S2 and S3 are eliminated.
[0112] Test Example 1
[0113] The materials of Examples 1 to 6 and the comparative example were tested for their key properties as follows.
[0114] (1) Particle size: D50 is measured using a laser particle size analyzer.
[0115] (2) Adhesion I: Each microsphere material was evenly coated on the surface of a 9 μm thick polyethylene-polypropylene three-layer composite wet-process porous diaphragm and dried. The coating amount was 0.3 g / m 2 Then, the coated surface of the separator was attached to the graphite negative electrode sheet, and pressure was applied at 25°C and 1 MPa for 10 seconds to form a bond between the separator and the negative electrode sheet; the 180° peel strength (referred to as peel strength I in Table 5) was tested by an electronic tensile testing machine.
[0116] (3) Adhesion II: The microsphere materials, ceramic powders, and other additives are mixed at a dry weight ratio of 10wt.%: 85wt.%: 5wt.% to form an aqueous slurry, which is applied to the surface of the composite wet-process porous diaphragm as in step (2) to obtain a diaphragm with a ceramic-polymer microsphere composite coating on the surface; wherein the other additives include adhesives (water-based polyacrylates, commercially available, 3.75wt.%), dispersants (polyacrylates, commercially available, 0.75wt.%), and wetting agents (Laurel Spring polyoxyethylene ethers, commercially available, 0.5wt.%). The dry weight of the microsphere material in the coating accounts for 10wt.%, and the coating surface density is 3g / m 2 After the separator with the composite coating was attached to the graphite negative electrode sheet, pressure was applied at 25°C and 7 MPa for 120 seconds to allow the separator and the negative electrode sheet to form a bond; the 180° peel strength (referred to as peel strength II in Table 5) was tested using an electronic tensile testing machine.
[0117] (4) Anti-sticking performance during winding: used to test the adhesion degree of the membrane caused by winding tension, storage temperature, etc. after the microsphere material of the present invention is coated on the membrane. Each microsphere material is evenly coated on the surface of a 9μm thick polyethylene-polypropylene three-layer composite wet-process porous membrane and dried. The coating amount is 0.3g / m 2 The coated diaphragm was laminated with another uncoated diaphragm, and pressure was applied at 40°C and 1 MPa for 120 s, and then the 180° peel strength (referred to as peel strength III in Table 5) was tested by an electronic tensile testing machine.
[0118] Combined with the test results, the microsphere material prepared by the present invention will not have the negative defect of membrane rolling and adhesion when performing a single coating operation; wherein, single coating refers to directly coating the microsphere material prepared by the present invention directly on the membrane; if the microsphere material is mixed with ceramic powder (such as alumina, boehmite, etc.) for coating, it is mixed coating.
[0119] (5) Air permeability: The single-coated and mixed-coated diaphragms prepared in steps (2) and (3) were tested for their air permeability using a Gurley air permeability tester, and the air permeability value of the uncoated base film was subtracted to obtain the air permeability increase value I and air permeability increase value II, respectively.
[0120] (6) Resistance to swelling in electrolyte: The microsphere materials prepared in each embodiment and comparative example were dried to obtain a film; the film was immersed in an electrolyte at 70°C for 7 days, and the difference in weight change before and after immersion was measured (equivalent to the swelling rate). The electrolyte composition was: EC:DEC:DMC = 3:5:2 by mass.
[0121] The test results of Experimental Example 1 are provided as shown in Table 5. Additionally, Figure 1 Provides particle size distribution detection information and particle size diagram of Example 5, Figure 2 A SEM image of Example 5 is provided.
[0122] Table 5
[0123]
[0124] Examples 7 to 19: used to investigate the influence of the proportion of the core layer, transition layer and shell layer on the performance of the polymer microsphere material. In Example 1, it is calculated that the weight ratio of the solid content in the three-layer structure is 21:17.1:59.26; that is, the amount of the transition layer in Example 1 is approximately equal to 81wt.% of the core layer, and the amount of the shell layer is approximately equal to 155wt.% of the sum of the core layer and the transition layer. Therefore, in this part of the examples, it is basically the same as Example 1, the only difference is: the total solid content of the transition layer or the shell layer is changed separately.
[0125] In Examples 7 to 11, the amounts of the transition layer, calculated on a solid content basis, were respectively equal to 72 wt%, 54 wt%, 36 wt%, 18 wt%, and 5 wt% of the core layer. In addition, in Comparative Example 8, the amounts of the transition layer, calculated on a solid content basis, were respectively equal to 100 wt% of the core layer.
[0126] In Examples 12 to 19, the amount of the shell layer is approximately equal to 200 wt.%, 175 wt.%, 135 wt.%, 100 wt.%, 75 wt.%, 55 wt.%, 25 wt.%, and 5 wt.% of the sum of the core layer and the transition layer, calculated on a solid content basis. In addition, in Comparative Example 9, the amount of the shell layer is respectively equal to 220 wt.% of the sum of the core layer and the transition layer, calculated on a solid content basis.
[0127] Test Example 2: The same test items as those of Test Example 1 were used, with only the test object changed. The test results of Test Example 2 are shown in Tables 6 and 7.
[0128] Table 6
[0129]
[0130] It can be seen from Table 6 above that the amount of transition layer has almost no effect on the particle size, and has little effect on the air permeability and swelling rate. The transition layer mainly affects the adhesion, and has a greater impact on the electrode adhesion (mixed coating) and the mutual adhesion of the diaphragm. When the amount of transition layer is high, the electrode adhesion (mixed coating) of the product is better; when the amount of transition layer is low, the product has a lower mutual adhesion of the diaphragm while maintaining good electrode adhesion (single coating), that is, it has a better anti-adhesion effect of the diaphragm. However, when the amount of transition layer is too much (as shown in Comparative Example 8), although it is beneficial to improve the electrode adhesion, it also leads to a significant increase in the mutual adhesion of the diaphragm, which means that the anti-adhesion effect of the diaphragm is significantly deteriorated.
[0131] Table 7
[0132]
[0133] It can be seen from Table 7 above that, in general, the thinner the shell, the stronger the adhesion, but the indicators such as air permeability and swelling rate have different degrees of deterioration. Among them, when the amount of shell is high, especially in Examples 12 to 15 (the amount of shell exceeds 100wt.%), the electrode adhesion (single coating) increases significantly, and at the same time, the membrane mutual adhesion, air permeability, swelling rate and other indicators do not deteriorate significantly, but when the amount of shell is too high (such as comparative example 9), the electrode adhesion deteriorates significantly; and when the amount of shell is low, especially in Examples 18 to 19 (the amount of shell does not exceed 25wt.%), the electrode adhesion (mixed coating) increases significantly, and at the same time, the air permeability (mixed coating), swelling rate and other indicators do not deteriorate significantly.
[0134] In summary, it can be seen from Tables 6 and 7 that, under the premise of ensuring that various performance indicators are in good condition, the present invention can achieve the enhancement of a certain performance indicator by adjusting the dosage of each layer; those skilled in the art can adjust the layer dosage and thickness according to the emphasis of actual performance requirements.
[0135] Examples 20 to 48: used to investigate the influence of the proportion of each raw material component in the core layer on the performance of the polymer microsphere material. In Example 2, it is calculated that: based on solid content, the mass proportion of M1-1 is 56wt.%, the mass proportion of M1-2 (including M1-2-1 and M1-2-2) is 28wt.%, the mass proportion of M1-3 (including M1-3-1 and M1-3-2) is 9.5wt.%, the mass proportion of M1-4 is 2.8wt.%, the mass proportion of M1-5 is 1.9wt.%, and the mass proportion of M1-6 is 0.05wt.%.
[0136] Therefore, in this part of the embodiments, it is basically the same as Embodiment 2, and the only difference is that the solid content of a certain raw material component or a certain type of raw material component is changed separately. It should be noted that after changing a certain solid content, the other raw material components are increased or decreased according to the proportion of Embodiment 2; when the solid content of a certain type of raw material component is changed, taking M1-2 as an example, M1-2-1 and M1-2-2 are also increased or decreased synchronously according to the proportion of Embodiment 2.
[0137] Examples 20-23: Based on solid content, the amounts of M1-1 used were 45wt.%, 67wt.%, 78wt.%, and 85wt.%, respectively.
[0138] Examples 24-26: Based on solid content, the amounts of M1-2 used were 34 wt.%, 22 wt.%, and 16 wt.%, respectively.
[0139] Examples 27-31: Based on solid content, the amounts of M1-3 used were 7.5wt.%, 5.5wt.%, 11.5wt.%, 15.5wt.%, and 19.5wt.%, respectively.
[0140] Examples 32-36: Based on solid content, the amounts of M1-4 used were 1.4wt.%, 4.2wt.%, 5.6wt.%, 7.7wt.%, and 9.6wt.%, respectively.
[0141] Examples 37-43: In terms of solid content, the amounts of M1-5 used were 0.9wt.%, 0.09wt.%, 0.01wt.%, 3.8wt.%, 5.7wt.%, 7.6wt.%, and 9.5wt.%, respectively.
[0142] Examples 44-48: Based on solid content, the amounts of M1-6 used are 0.01wt.%, 0.001wt.%, 0.1wt.%, 1wt.%, and 2wt.%, respectively.
[0143] Test Example 3: The same test items as those of Test Example 1 were used, with only the test object changed. Table 8 provides the test results of Test Example 3.
[0144] Table 8
[0145]
[0146] Examples 49-60: used to investigate the influence of the proportion of each raw material component in the transition layer on the performance of the polymer microsphere material. In Example 3, it was calculated that, based on solid content, the mass proportion of M2-1 was 24.83wt.%, the mass proportion of M2-2 was 55.86wt.%, and the mass proportion of M2-3 was 18.62wt.%.
[0147] Therefore, in this part of the examples, it is basically the same as Example 3, the only difference is that the solid content of a certain raw material component or a certain type of raw material component is changed separately. It should be noted that after changing a certain solid content, the other raw material components are increased or decreased according to the proportion of Example 3.
[0148] Examples 49 to 53: Based on solid content, the amounts of M2-1 used were 15wt.%, 5wt.%, 35wt.%, 45wt.%, and 55wt.%, respectively.
[0149] Examples 54-57: Based on solid content, the amounts of M2-2 used were 28 wt.%, 14 wt.%, 7 wt.%, and 70 wt.%, respectively.
[0150] Examples 58-60: Based on solid content, the amounts of M2-3 used are 9wt.%, 3wt.%, and 27wt.%, respectively.
[0151] Test Example 4: The same test items as those of Test Example 1 were used, with only the test object changed. Table 9 provides the test results of Test Example 4.
[0152] Table 9
[0153]
[0154] Examples 61 to 79: used to investigate the influence of the proportion of each raw material component in the shell layer on the performance of the polymer microsphere material. In Example 5, it was calculated that, based on solid content, the mass proportion of M3-1 was 67.83wt.%, the mass proportion of M3-2 was 9.69wt.%, the mass proportion of M3-3 (including M3-3 and M3-3-a) was 4.8wt.%, the mass proportion of M3-4 was 7.75wt.%, and the mass proportion of M3-5 was 6.78wt.%.
[0155] Therefore, in this part of the examples, it is basically the same as Example 5, the only difference is that the solid content of a certain raw material component or a certain type of raw material component is changed separately. It should be noted that after changing a certain solid content, the other raw material components are increased or decreased according to the proportion of Example 5.
[0156] Examples 61-64: Based on solid content, the amounts of M3-1 used were 60 wt.%, 50 wt.%, 85 wt.%, and 95 wt.%, respectively.
[0157] Examples 65-68: Based on solid content, the amounts of M3-2 used were 15wt.%, 5wt.%, 1wt.%, and 0.1wt.%, respectively.
[0158] Examples 69-72: Based on solid content, the amounts of M3-3 used are 1 wt.%, 0.1 wt.%, 15 wt.%, and 25 wt.%, respectively.
[0159] Examples 73-76: Based on solid content, the amounts of M3-4 used are 4wt.%, 1wt.%, 12wt.%, and 15wt.%, respectively.
[0160] Examples 77-79: Based on solid content, the amounts of M3-5 used were 14 wt.%, 28 wt.%, and 42 wt.%, respectively.
[0161] Test Example 5: The same test items as those of Test Example 1 were used, with only the test object changed. Table 10 provides the test results of Test Example 5.
[0162] Table 10
[0163]
[0164] Examples 80-83: used to investigate the effect of the polymerization reaction temperature of the core layer on the performance of the polymer microsphere material. Examples 80-83 are substantially the same as Example 4, except that the polymerization reaction temperatures in step S1 are 55°C, 65°C, 70°C, and 75°C, respectively. In addition, Comparative Examples 10-11 are substantially the same as Example 4, except that the polymerization reaction temperatures in step S1 are 45°C and 85°C, respectively.
[0165] The results show that:
[0166] (1) The expected products were obtained in Example 4 and Examples 80-83. The relevant test results are shown in Table 11.
[0167] (2) Comparative Example 10 failed to obtain the expected product because the polymerization reaction temperature in step S1 was too low and the reaction could not be effectively initiated. A large amount of lumps and unreacted residual monomers were observed in the reaction system.
[0168] (3) Comparative Example 11 failed to obtain the expected product because the polymerization reaction temperature in step S1 was too high and the initiator was consumed too quickly, resulting in a large amount of monomers failing to be initiated and remaining in the reaction system.
[0169] Test Example 6: The same test items as those in Test Example 1 were used, with only the test objects changed; the test results of Test Example 6 are provided in Table 11. It is understandable that since Comparative Examples 10 and 11 cannot provide the expected microsphere material products, the relevant data of Comparative Examples 10 and 11 are not provided in Table 11.
[0170] Table 11
[0171]
[0172] As can be seen from Table 11, when the polymerization temperature is within the appropriate range, the temperature only has a significant effect on the particle size of the core layer product, and has almost no effect on other properties. When the core layer polymerization temperature is too low (such as Comparative Example 10), the monomer is difficult to be initiated and the reaction is difficult to proceed; when the core layer polymerization temperature is too high (such as Comparative Example 11), the initiator is consumed too quickly and the product has too much residual monomer. Both too low or too high core layer polymerization temperatures will have an adverse effect on the performance of the microsphere material.
[0173] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.
Claims
1. A polymer microsphere material, characterized in that: The polymer microsphere material comprises a core layer, a transition layer and a shell layer from inside to outside; The core layer comprises a first modified acrylate copolymer, and the glass transition temperature of the first modified acrylate copolymer is ≤35°C; the transition layer comprises at least one functional monomer polymerized; the shell layer comprises a second modified acrylate copolymer, and the glass transition temperature of the second modified acrylate copolymer is 60°C to 250°C; The raw material of the transition layer includes functional monomers, and the functional monomers include at least one of a front cross-linking monomer, a strong polar monomer or a long side chain monomer; wherein the front cross-linking monomer contains at least two polymerizable alkenyl functional groups; the functional group of the strong polar monomer includes at least one of a hydroxyl group, a carbonyl group, an acyloxy group, an ether bond, an epoxy group, an amine group, a sulfonic acid group, and an aromatic ring containing a substituent; the side group of the long side chain monomer includes at least one carbon chain or carbon oxygen chain with a carbon number ≥ 4; In the transition layer: the front cross-linking monomer includes at least one of ethylene glycol dimethacrylate, polyethylene glycol diacrylate, trimethylolpropane triacrylate, 1,6-hexanediol diacrylate or 1,4-butanediol diacrylate, the strong polar monomer includes at least one of tetrahydrofuran acrylate, carboxyethyl acrylate, hydroxyethyl acrylate, dimethylaminoethyl acrylate, 2-phenoxyethyl acrylate, ethoxyethoxyethyl acrylate, diacetone acrylamide or cyclotrimethylolpropane formal acrylate, and the long side chain monomer includes at least one of hydroxybutyl methacrylate, lauryl acrylate, PEG350MA or APEG2400; The first modified acrylic ester copolymer is prepared by including the following components by weight: 45-85 parts of non-water-soluble soft monomer, 15-35 parts of non-water-soluble hard monomer, 5-20 parts of water-soluble organic acid monomer, 0.001-5 parts of non-ionic surfactant, 0.065-5 parts of water-soluble initiator and some deionized water; In the core layer: the water-insoluble soft monomer includes at least one of n-butyl acrylate, n-octadecyl acrylate, isooctyl acrylate, lauryl acrylate or vinyl neodecanoate; the water-insoluble hard monomer includes a first water-insoluble hard monomer and a second water-insoluble hard monomer, the first water-insoluble hard monomer includes at least one of methyl methacrylate or acrylonitrile, and the second water-insoluble hard monomer includes at least one of styrene or tert-butyl methacrylate; the water-soluble organic acid monomer includes a first water-soluble organic acid monomer and a second water-soluble organic acid monomer, the first water-soluble organic acid monomer includes at least one of acrylic acid, maleic acid, itaconic acid or p-vinylphenol; the second water-soluble organic acid monomer includes at least one of p-styrene sulfonic acid, 2-acrylamide-2-methylpropane sulfonic acid or allyl sulfonic acid; The second modified acrylate copolymer is prepared by including the following components by weight: 50-95 parts of water-insoluble hard monomer, 0.1-15 parts of front-end crosslinking monomer, 0.056-3.9 parts of water-soluble initiator and some deionized water; In the shell layer: the components of the water-insoluble hard monomer are the same as those of the water-insoluble hard monomer in the core layer; the components of the front-end cross-linking monomer are the same as those of the front-end cross-linking monomer in the transition layer; The mass of the transition layer is 5wt.%~85wt.% of the core layer, and the mass of the shell layer is 5wt.%~200wt.% of the sum of the core layer and the transition layer.
2. The polymer microsphere material according to claim 1, characterized in that: The diameter of the polymer microsphere material is 1 μm to 50 μm.
3. The method for preparing the polymer microsphere material according to claim 1 or 2, characterized in that: The preparation method of the polymer microsphere material comprises the following steps: (1) The raw material components of the core layer are fully mixed and polymerized to obtain a core layer emulsion; (2) adding the raw material components of the transition layer to the core layer emulsion, and performing a second polymerization reaction to obtain a core emulsion coated with the transition layer; (3) Adding the raw material components of the shell layer to the core emulsion of the coating transition layer, performing a third polymerization reaction, and obtaining an emulsion containing the polymer microsphere material.
4. The method for preparing the polymer microsphere material according to claim 3, characterized in that: Includes at least one of the following features (a) to (c): (a) The polymerization reaction temperature is 55°C to 75°C, and the polymerization reaction holding time is 12h to 15h; (b) the temperature of the second polymerization reaction is 70° C. to 90° C., and the insulation time of the second polymerization reaction is 0.5 h to 3 h; (c) The temperature of the third polymerization reaction is 70° C. to 90° C., and the insulation time of the third polymerization reaction is 1 h to 3 h.
5. A separator for a secondary battery, characterized in that: The separator comprises the polymer microsphere material according to claim 1 or 2.
6. A secondary battery, characterized in that: The secondary battery includes the separator according to claim 5 .
Citation Information
Cited By
Polyacrylate emulsion as well as preparation method and application thereof
CN120329487A