Method for preparing composite MOF carbon material from waste plastics, composite MOF carbon material and application thereof

The carbon material prepared by waste plastic is modified through plasma etching technology and combined with MOF materials, which solves the problems of poor controllability of carbon materials and insufficient interface bonding strength in the prior art, and improves the specific surface area and electrochemistry of the material Performance, achieving improvements in structural stability and cyclic performance.

CN118638425BActive Publication Date: 2024-11-26SHANGHAI FIRM LITHIUM NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411087908.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-26
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

In the prior art, carbon materials prepared by waste plastics have poor controllability, uneven pore structure, low surface area, and difficult to accurately regulate structure and performance, and the interface bonding strength between carbon materials and MOF materials is insufficient.

Method used

The carbon material prepared by waste plastic is modified and functionalized through plasma etching technology. Combined with MOF materials, the conductivity of carbon materials and the high surface area and controllability of MOF materials are used to react with crosslinking agent to form composite MOF carbon. Material.

Benefits of technology

The specific surface area and active sites of carbon materials are improved, the catalytic and electrochemical properties are enhanced, the problem of insufficient interface bonding strength between carbon materials and MOF materials is solved, and structural stability and cycling performance are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118638425B_ABST
    Figure CN118638425B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of lithium battery positive electrode materials, and specifically discloses a method for preparing a composite MOF carbon material from waste plastics, a composite MOF carbon material and its application; the method for preparing a composite MOF carbon material from waste plastics comprises the following steps: S1, crushing the waste plastics into plastic particles, calcining and carbonizing, ball milling, and drying to obtain a carbon material; S2, plasma etching the carbon material; S3, mixing and stirring the etched carbon material with the MOF material, and dispersing them in solvent A to form a mixed solution, adding a cross-linking agent to the mixed solution, heating and reacting, and obtaining the composite carbon material. Solvent A comprises one or more of water, ethanol, acetonitrile, dimethylformamide, and chloroform. By compounding the MOF material with the plasma-etched carbon material, the excellent pore structure and specific surface area of ​​the MOF material can be brought into the composite material, thereby improving the overall pore structure and specific surface area of ​​the composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium battery positive electrode materials, and in particular to a method for preparing a composite MOF carbon material from waste plastics, the composite MOF carbon material and applications thereof. Background Art

[0002] In today's society, the recycling and reuse of waste plastics has become a hot topic. At the same time, solid-state batteries, as a new type of high-energy density and high-safety battery technology, have broad application prospects in electric vehicles, drones and other fields. Reusing waste plastic resources into solid-state battery positive electrode materials can not only reduce the amount of waste and reduce environmental pollution, but also improve battery performance and life cycle.

[0003] Solid-state battery positive electrode materials usually use oxides or sulfides as the main materials, which have high theoretical specific capacity and energy density. However, they also have some problems, such as loose structure and capacity decay. Waste plastics, as a material with excellent mechanical properties and chemical stability, have been widely used in solid-state battery positive electrode materials. By adding waste plastics, the structural stability and mechanical strength of solid-state battery positive electrode materials can be enhanced, and the battery's cycle performance and capacity retention rate can be improved.

[0004] At present, many scientific research institutions and enterprises are conducting research and development on the application of waste plastic resources in solid-state battery positive electrode materials. For example, a research team at Northwestern University in the United States prepared a new type of solid-state battery positive electrode material by compounding waste polyethylene plastic with oxides, and achieved good performance. In addition, countries such as Japan and Germany have also made certain progress in the application of waste plastics in solid-state battery positive electrode materials. However, there are many problems with the carbon materials prepared from waste plastics in the existing technology:

[0005] 1) The controllability of carbon materials prepared from waste plastics is relatively poor, and it is difficult to achieve precise structure and performance regulation. They have a relatively simple pore structure, and the pore size and distribution are not uniform enough;

[0006] 2) Carbon materials prepared from waste plastics usually have a low specific surface area. Summary of the invention

[0007] In view of this, the purpose of the present invention is to provide a method for preparing composite MOF carbon materials from waste plastics, composite MOF carbon materials and applications; the present invention further processes the carbon materials prepared from waste plastics by plasma etching technology, thereby achieving the purpose of surface modification and functionalization, removing impurities and surface pollution, regulating pore structure, and improving surface activity. The plasma-etched carbon materials are further composited with MOF materials to make full use of their respective advantages, such as the conductivity and stability of carbon materials and the high surface area and controllability of MOF materials, so as to exert more comprehensive physical and chemical properties in the fields of catalysis, sensing, electrochemistry, etc.

[0008] The objective of the present invention is achieved through the following technical solutions:

[0009] <First aspect>

[0010] A method for preparing a composite MOF carbon material from waste plastics comprises the following steps:

[0011] S1, crushing, calcining, carbonizing and ball milling waste plastics to obtain carbon materials;

[0012] S2, the carbon material is subjected to plasma etching treatment;

[0013] S3. The etched carbon material is mixed and stirred with the MOF material, and dispersed in solvent A to form a mixed solution. A cross-linking agent is added to the mixed solution, and the mixture is heated for reaction to obtain the composite MOF carbon material. The solvent A includes one or more of water, ethanol, acetonitrile, dimethylformamide, and chloroform. The cross-linking agent includes 3-aminopropyltrimethoxysilane (APTES) and / or methyltrimethoxysilane (MTMS).

[0014] In step S1, after the waste plastics are collected, they are initially treated by washing (the washing agent is selected from one or more of water, ethanol, acetone, hydrochloric acid solution, and sodium hydroxide solution; the mass ratio of the waste plastics to the washing agent is 1:50-1:100) to ensure that dirt and impurities are completely removed, and then crushed by a crusher (the crusher power is 1 kW-30 kW). Drying conditions: vacuum drying oven at 30 o C-100 o C, drying time 1h-30h, to obtain dry plastic particles.

[0015] In step S1, the calcination and carbonization step is as follows: the plastic particles are placed in an inert atmosphere at 200 o C-1000 o Calcination time is 1h-12h at 400 °C, and the heating rate is 0.1 °C / min-5 °C / min. After calcination, the material is taken out, cooled to room temperature, and ball milled to obtain uniform particle size and surface smoothness. Calcination can be carried out in a tubular furnace.

[0016] In step S1, the ball milling conditions are: ball to material ratio (10-60): (1-10), ball milling speed 100rpm-1000rpm, and ball milling time 4h-12h. In step S2, the etching conditions are: gas pressure 10-100 Pa, gas flow rate 20-100 sccm, power 30-200 W, and etching time 2-30 min.

[0017] Etching gas includes one or more of hydrogen fluoride, F2

[0018] In step S3, the method for preparing the MOF material comprises the following steps:

[0019] The metal ions and organic ligands were dissolved in solvent B and heated at 100 °C under an inert atmosphere. o C-150 o C for 12h-72h, centrifuge (centrifuge 2-5 times), collect precipitate, wash, dry (drying time 5h-12h), and obtain the MOF material; the solvent B includes one or more of dimethylformamide, dimethyl sulfoxide, methanol, ethanol, and xylene. The precipitated product is usually micron-sized MOF crystal particles. The MOF crystals separated at last usually need to be washed to remove residual solvent and impurities, and then vacuum dried or dried at an appropriate temperature to obtain the final MOF product.

[0020] The metal ions include one or more of copper ions (Cu), zinc ions (Zn), aluminum ions (Al), iron ions (Fe), ruthenium ions (Ru), nickel ions (Ni), and cobalt ions (Co);

[0021] And / or, the organic ligand includes: one or more of phthalic acid, isophthalic acid, oxydi(p-hydroxybenzoic acid), and 2-methylimidazole.

[0022] Preferably, the metal ions include one or more of copper ions (Cu), iron ions (Fe), ruthenium ions (Ru), nickel ions (Ni), and cobalt ions (Co).

[0023] Preferably, the organic ligand includes one or more of phthalic acid and isophthalic acid.

[0024] And / or, the molar ratio of metal ion to organic ligand is 1:1-1:5.

[0025] In step S3, the mass ratio of the carbon material after etching to the MOF material is 1:1-1:5.

[0026] And / or, in step S3, the heating reaction conditions are: reacting at a temperature of 25° C.-90° C. for 6 h-24 h under stirring.

[0027] Waste plastics include polyethylene (PE), polypropylene (PP), polyvinyl chloride (PVC), polystyrene (PS), polyethylene terephthalate (PET), and polycarbonate (PC).

[0028] <Second Aspect>

[0029] The composite MOF carbon material prepared by the method described above also falls within the protection scope of the present invention.

[0030] <Third Aspect>

[0031] The present invention provides a method for preparing a composite positive electrode material, comprising the following steps:

[0032] The ternary cathode material is dispersed in solvent C to form a dispersion, and the composite MOF carbon material as described above is added to the dispersion. o C-1000 o C, stirring at 100-600 rpm for 2h-24h, filtering, drying the filter residue, calcining, cooling to room temperature and vacuum drying (drying at 80-100℃ for 3-6h) to obtain a composite positive electrode material; solvent C includes one or more of ethanol, methanol, and water. Calcination is carried out in a muffle furnace at a calcination temperature of 100 o C-1000 o C, calcination time 1h-12h.

[0033] The ternary material includes one or more of NCM811, NCM523, and NCM622.

[0034] The mass ratio of the ternary material to the composite MOF carbon material is (90-99):(10-1).

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] 1. Carbon materials prepared from waste plastics usually have good mechanical properties and stability. They have a simple pore structure, but the pore size and distribution are not uniform enough. The surface morphology and chemical properties of carbon materials can be controlled by plasma etching technology for surface treatment of carbon materials. By injecting the required etching gas, such as fluorine gas (F2), into the processing chamber, -F groups can also be introduced to increase the microscopic concave-convex structure and pore structure of the material, thereby increasing the specific surface area of ​​the material, which is beneficial to improving the adsorption performance and catalytic performance; thereby improving the stability of the interface between the positive electrode material and the electrolyte.

[0037] 2. Biomass carbon has a unique porous structure, contains oxygen, nitrogen and other elements, has more active sites and is cheap and easy to obtain. Metal-organic framework materials (MOF) are also a type of porous materials with rich and diverse morphologies, high specific surface area, chemical controllability and structural stability. Biomass carbon and MOF functional composite materials can be prepared by simple hydrothermal reactions. Biomass carbon and MOF functional composite materials have a larger specific surface area and more active sites than biomass carbon or MOF alone, and exhibit many excellent properties.

[0038] 3. In order to solve the problem of insufficient interface bonding strength between carbon materials and MOF, the present invention introduces a cross-linking agent to prepare a structurally stable composite MOF carbon material. It is verified in an all-solid-state battery system that the structure can remain stable after 300 cycles.

[0039] 4. Carbon materials made from waste plastics can make full use of waste plastic resources and realize resource reuse and recycling. By compounding with MOF materials, waste plastics can be converted into composite materials with high added value, realizing the effective utilization of waste plastic resources and conforming to the concept of sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0041] Figure 1 SEM image of the positive electrode material coated with carbon material carbonized from waste plastic;

[0042] Figure 2 This is the SEM spectrum of the carbon material after plasma etching;

[0043] Figure 3 This is a 300-cycle charge-discharge cycle diagram of Example 1 at 1.0 C. DETAILED DESCRIPTION

[0044] The present invention is described in detail below in conjunction with embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, some adjustments and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0045] Preparation Example 1

[0046] 1. Preparation of carbon materials from carbonized waste plastics

[0047] 1.1 Preprocessing

[0048] 1000g of the collected waste plastic polyethylene (polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyester, polycarbonate, polyamide, etc.) was initially treated by washing with water to ensure that dirt and impurities were completely removed, and then crushed with a 1000W crusher and then passed through a 1000W crusher. o C for 1 h to obtain plastic particles.

[0049] 1.2 Carbonization treatment: Place the plastic particles in a tube furnace, in an inert atmosphere (argon), 500 o C for 3 hours with a heating rate of 5°C / min. Then, the carbonized plastic sample was taken out and cooled to room temperature. Finally, the obtained material was ball milled at a ball-to-material ratio of 10:1 and a speed of 500 rpm for 4 hours to obtain an uneven and rough carbon material.

[0050] Figure 1 This is an SEM image of the positive electrode material coated with carbon material carbonized from waste plastic.

[0051] 2. Plasma etching technology to treat carbon materials from waste plastics

[0052] First, start the plasma etching equipment (Dezhu Xinyuan, SI500) and preheat and calibrate according to the manufacturer's instructions. Check whether the vacuum pump and gas supply system are working properly. Then select hydrogen fluoride etching gas. Set the gas pressure of the etching chamber to 50Pa, the gas flow rate to 50 sccm, and the power to 60W.

[0053] After the parameters are set, 1g of the carbon material sample prepared in step 1.2 is placed in the etching chamber to ensure that the sample surface is evenly exposed to the plasma, the etching process is started, and the changes on the sample surface are monitored. After the etching is completed (etching time is 30 min), the etching process is stopped and the equipment is turned off. The sample is taken out and washed with deionized water to remove possible residual gases and impurities, and a plasma-etched carbon material of 1μm-10μm is obtained. Figure 2 This is the SEM spectrum of the carbon material after plasma etching.

[0054] 3. Preparation of MOF materials

[0055] First, 0.5 mol Cu(NO3)2·3H2O (121 mg) and 0.5 mol phthalic acid (83 mg) were dissolved in 10 mL of dimethylformamide solvent (99.8%+, Adamas), and stirred under an inert atmosphere (argon) for 120 min. oC for 36 hours. After the reaction is completed, the produced MOF crystals will precipitate. At this time, the precipitate can be separated by filtration by centrifugation at 10000 rpm / min for 3 times. Then, the final MOF product can be obtained by vacuum drying for 6 hours.

[0056] 4. Preparation of composite MOF carbon materials

[0057] The plasma-etched carbon material (1 g) prepared in step 2 was mixed evenly with the MOF powder (1 g) prepared in step 3, and 1 g of a cross-linking agent (methyltrimethoxysilane MTMS) was added and dispersed in 100 mL of a mixed solvent of ethanol and water (volume ratio 1:1). The mixture was heated at 60 ° C for 20 h to allow the cross-linking agent to work and fix the carbon material and MOF material together to form a composite structure. The material was cooled to room temperature, washed 3 times and dried for 8 h to finally form a composite MOF carbon material.

[0058] Comparative Example Preparation Example 1

[0059] The difference between this comparative preparation example and preparation example 1 is that the cross-linking agent in step 4 is replaced by p-hydroxybenzaldehyde.

[0060] Comparative Example Preparation Example 2

[0061] The difference between this comparative preparation example and preparation example 1 is that step 2 is omitted, that is, a carbon material that has not been plasma etched is used.

[0062] The specific steps are as follows:

[0063] Step 1, same as step 1 of Preparation Example 1;

[0064] Step 2, same as step 3 of Preparation Example 1;

[0065] Step 3: Mix the plasma-etched carbon material (1 g) prepared in step 1 and the MOF powder (1 g) prepared in step 3, add 1 g of a cross-linking agent (methyltrimethoxysilane MTMS), and disperse them in 100 mL of a mixed solvent of ethanol and water (volume ratio 1:1). Heat the mixture at 60 ° C for 20 h to allow the cross-linking agent to work and fix the carbon material and MOF material together to form a composite structure. Cool the material to room temperature, wash 3 times and dry for 8 h to finally form a composite MOF carbon material.

[0066] Example 1

[0067] 1. Preparation of ternary cathode materials coated with composite MOF carbon materials

[0068] Weigh 9 g of the ternary cathode material NCM811 and place it in an eggplant-shaped bottle. Add a stirrer and 50 mL of ethanol solvent to disperse it evenly. Then add 1 g of the composite MOF carbon material of step 4 of preparation example 1 to the solution. o C, stirred at 500 rpm for 120 min, filtered and dried, and the filter cake was then placed in a tubular furnace for calcination at 600 ° C for 10 h. The material was cooled to room temperature and taken out. After drying at 80 ° C in a vacuum drying oven for 4 h, a ternary positive electrode material coated with a composite MOF carbon material was obtained, which was finally transferred to a glove box for standby use.

[0069] 2. Preparation of composite cathode materials

[0070] The ternary positive electrode material (850 mg) coated with the composite MOF carbon material prepared in step 1 and the commercially purchased Li6PS5Cl (150 mg) were weighed into a 25 mL zirconia ball mill according to a mass ratio of 85:15. The total mass of the materials was 1 g, the ball-to-material ratio was controlled to be 30:1, and the diameter of the zirconia ball milling beads used was 3 mm. Then the sealed ball milling jar was fixed on a high-energy planetary ball mill and ball milled at 600 r / min for 8 hours; finally, the composite positive electrode material was obtained.

[0071] Example 2

[0072] The difference between Example 2 and Example 1 is that in step 2, NCM811 is replaced by NCM523.

[0073] Example 3

[0074] The difference between Example 3 and Example 1 is that in step 2, NCM811 is replaced by NCM622.

[0075] Comparative Example 1

[0076] The difference between this comparative example and Example 1 is that in step 1, the composite MOF carbon material of Preparation Example 1 is replaced by the composite MOF carbon material of Comparative Preparation Example 1.

[0077] Comparative Example 2

[0078] The difference between this comparative example and Example 1 is that in step 1, the composite MOF carbon material of Preparation Example 1 is replaced by the composite MOF carbon material of Comparative Preparation Example 2.

[0079] Comparative Example 3

[0080] The difference between this comparative example and Example 1 is that the coating material directly adopts the carbon material obtained by plasma etching. That is, in step 1 of Example 1, the composite MOF carbon material is replaced by the plasma-etched carbon material prepared in step 2 of Preparation Example 1.

[0081] Effect test example

[0082] Weigh 100 mg of commercially purchased solid electrolyte (Li6PS5Cl) in a 10 mm stainless steel tableting mold, press the electrolyte sheet at a pressure of 180 MPa, then add 10 mg of the composite positive electrode material prepared in Examples 1-3 or Comparative Examples 1-3 to one side of the electrolyte, press it again at a pressure of 360 MPa, then demold it, load it into the battery test mold, then add a 9 mm lithium indium sheet (the thickness of the lithium sheet is 30 microns, and the thickness of the indium sheet is 100 microns) to the other side of the electrolyte sheet, and finally load the Al sheet current collector on the positive electrode side and the Cu current collector on the negative electrode side to complete the packaging. Take out the battery mold, put it in the battery fixture, and apply a pressure of 50 MPa to obtain a sandwich-type all-solid-state battery. The assembled full battery was subjected to a capacitor discharge test (room temperature 30 ° C, 0.1 C, 10 mg loading). The results are shown in Table 1.

[0083] Table 1

[0084] First cycle charging capacity Discharge capacity after 100 cycles Capacity retention rate after 100 cycles Example 1 200mAh / g 125 mAh / g 82% Example 2 195mAh / g 110mAh / g 80% Example 3 180mAh / g 109mAh / g 80% Comparative Example 1 184mAh / g 94mAh / g 51% Comparative Example 2 145mAh / g 80mAh / g 55% Comparative Example 3 160mAh / g 64mAh / g 40%

[0085] Figure 3 This is a 300-cycle charge-discharge cycle diagram of Example 1 at 1.0 C.

[0086] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. A method for preparing composite MOF carbon materials from waste plastics, characterized in that: The steps include: S1. Waste plastic polyethylene is crushed into plastic particles, calcined and carbonized, and ball-milled to obtain carbon materials; the calcination and carbonization steps are as follows: the plastic particles are calcined at 500° C. for 3 h in an inert atmosphere at a heating rate of 5° C. / min; S2, the carbon material is subjected to plasma etching treatment; plasma Etching conditions: etching gas is hydrogen fluoride; gas pressure 50Pa, gas flow 50 sccm, power 60W, etching time 30 min; S3, the etched carbon material and the MOF material are mixed and stirred, and dispersed in solvent A to form a mixed solution, a cross-linking agent is added to the mixed solution, and the mixture is reacted at 60° C. to obtain the composite MOF carbon material; the solvent A includes one or more of water, ethanol, acetonitrile, dimethylformamide, and chloroform; the cross-linking agent is methyltrimethoxysilane; In step S3, the method for preparing the MOF material comprises the following steps: Dissolve Cu(NO3)2·3H2O and organic ligand phthalic acid in solvent B, react for 12h-72h at 100°C-150°C in an inert atmosphere, centrifuge, collect precipitates, wash, dry, and obtain the MOF material; the molar ratio of Cu ions to organic ligands is 1:1-1:5; The solvent B includes one or more of dimethylformamide, dimethyl sulfoxide, methanol, ethanol, and xylene; The mass ratio of the carbon material to the MOF material after etching is 1:

1.

2. The method for preparing composite MOF carbon materials from waste plastics according to claim 1, characterized in that: In step S1, the ball milling conditions are as follows: ball to material ratio 10-60:1-10, ball milling speed 100rpm-1000rpm, and ball milling time 4h-12h.

3. The method for preparing composite MOF carbon materials from waste plastics according to claim 1, characterized in that: In step S3, the reaction conditions are: reacting for 6h-24h under stirring.

4. A composite MOF carbon material prepared by the method according to any one of claims 1 to 3.

5. A method for preparing a composite positive electrode material, characterized in that: The steps include: The ternary cathode material is dispersed in solvent C to form a dispersion, the composite MOF carbon material as claimed in claim 4 is added to the dispersion, stirred at 25°C-1000°C, 100-600rpm for 2h-24h, filtered, the filter residue is dried, calcined, cooled to room temperature and then vacuum dried to obtain a composite cathode material; the solvent C includes one or more of ethanol, methanol and water.

6. A composite positive electrode material prepared by the preparation method as claimed in claim 5.

7. Use of the composite positive electrode material as claimed in claim 6 in a lithium battery.