A high-efficiency sun-proof and heat-insulating composite solar film and preparation method thereof
By using a composite solar film composed of polyvinyl alcohol and modified nanoparticles, the problem of insufficient performance of the existing thermal insulation film is solved, efficient ultraviolet and infrared shielding is achieved, mechanical properties and weather resistance are enhanced, and energy consumption and pollution are reduced. .
Patent Information
- Application Number
- CN202411105805.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-13
AI Technical Summary
The existing thermally insulated solar films have limited performance in blocking infrared and ultraviolet rays, and are prone to aging, fading, and bubbles, resulting in increased temperature in the car, increased energy consumption, and affects aesthetics and service life.
It is composed of polyvinyl alcohol, polyvinylpyrrolidone, 2-hydroxy-4-methoxybenzophenone, silane-modified nanotitanium dioxide, fluorinated polyurethane, stearic acid-modified nanoindium tin oxide and antioxidants The composite solar film improves ultraviolet absorption and infrared reflection properties through the dispersion of modified nanoparticles and the combination of hydrophobic materials.
It significantly improves the shielding effect of ultraviolet and infrared, enhances mechanical properties and weather resistance, reduces aging and pollution, maintains long-term adhesion and transparency, and reduces energy consumption.
Smart Images

Figure CN118638455B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of automobile heat-insulating films, and in particular relates to a highly efficient sun-proof and heat-insulating composite solar film and a preparation method thereof. Background Art
[0002] Solar film, also known as thermal insulation film, is a transparent film applied to car or building windows to reduce harmful radiation in sunlight, improve comfort and save energy. It not only blocks ultraviolet (UV) and infrared (IR), but also improves the appearance and safety of windows. Car solar film is a thin film material used on car windows. Its main function is to block ultraviolet rays in sunlight, reduce the temperature inside the car, and provide a certain degree of privacy protection. This film is usually composed of a multi-layer composite material, including but not limited to a transparent plastic film, an ultraviolet absorption layer, a metal or metal oxide coating, and an adhesive layer. However, the existing thermal insulation solar film technology still has obvious shortcomings in many aspects. First, the thermal insulation performance of traditional solar films is limited, and it cannot effectively block a large amount of infrared and ultraviolet rays, causing the internal temperature of the vehicle to rise rapidly under strong sunlight, increasing the burden on the air conditioning system, and thus increasing energy consumption. For example, dyed film: This film is a transparent plastic film with dye added to it, and the dye absorbs part of the light to achieve a heat insulation effect; however, the thermal insulation performance of dyed film is weak, and it may fade over time, especially in high temperatures in summer, and it cannot effectively reduce the temperature inside the car. After a long period of strong sunlight and environmental changes, common thermal insulation films are prone to aging, fading, bubbling or peeling, which not only affects the appearance of the vehicle, but also increases the cost of maintenance and replacement. Especially under extreme climate conditions, such as high or low temperature environments, the performance of thermal insulation films declines more significantly. In addition, some low-quality films will fade, bubble, etc. after long-term exposure to ultraviolet rays, affecting the appearance and service life. Therefore, based on the above problems, it is extremely necessary to develop a highly efficient sun-proof and heat-insulating composite solar film. Summary of the invention
[0003] In view of the defects of the prior art, the object of the present invention is to provide a highly efficient sun-proof and heat-insulating composite solar film and a preparation method thereof.
[0004] The technical effect described in the present invention is achieved through the following technical solution: The present invention proposes a highly efficient sun-proof and heat-insulating composite solar film, which is composed of a base polymer A and a functional polymer B.
[0005] Preferably, the matrix polymer A comprises the following raw materials: polyvinyl alcohol, polyvinyl pyrrolidone, 2-hydroxy-4-methoxybenzophenone, and silane-modified nano titanium dioxide.
[0006] Preferably, the functional polymer B comprises the following raw materials: fluorinated modified polyurethane, stearic acid modified nano indium tin oxide, and antioxidant.
[0007] Preferably, the specific preparation steps of the silane-modified nano-titanium dioxide are as follows:
[0008] A1: Disperse nano-titanium oxide in a 50wt% ethanol solution, and mix evenly by 30W ultrasonic treatment to obtain a 2wt% nano-titanium oxide solution; add 3-aminopropyltriethoxysilane to the 50wt% ethanol solution, stir and mix evenly to obtain a coupling agent solution;
[0009] A2: Add the nano titanium dioxide solution prepared in step A1 to the coupling agent solution prepared in step A1, heat in a water bath to control the temperature at 30-50°C, stir and react for 8-18h, add 0.1M acetic acid solution to neutralize the reaction, centrifuge, filter, wash with deionized water for 3-5 times, and vacuum dry at 80°C to constant weight to obtain silane-modified nano titanium dioxide.
[0010] Preferably, the volume ratio of 3-aminopropyltriethoxysilane to the ethanol solution in step A1 is 1:10-15.
[0011] Preferably, the volume ratio of the nano-titanium oxide solution and the coupling agent solution in step A2 is 1:1-2; the volume of the acetic acid solution is 1 times the volume of the 3-aminopropyltriethoxysilane in step A1.
[0012] Preferably, the specific preparation steps of the stearic acid-modified nano indium tin oxide are as follows:
[0013] B1: Treat nano-indium tin oxide in a vacuum drying oven at 60°C for 12 hours to obtain pretreated nano-indium tin oxide; add octadecanoic acid to a 60wt% ethanol solution, heat it to 60°C in a water bath, stir and mix well to obtain a modified solution;
[0014] B2: Add the pretreated nano indium tin oxide prepared in step A1 to the modified solution prepared in step A1, perform 30W ultrasonic treatment for 30 min, heat in a water bath to 50-70° C., stir to react for 2-4 h, centrifuge, filter, wash with ethanol 3-5 times, and vacuum dry at 60° C. to constant weight to obtain stearic acid modified nano indium tin oxide.
[0015] Preferably, the ratio of the amount of octadecanoic acid to the ethanol solution in step B1 is 0.1-0.2 g:10 mL.
[0016] Preferably, the ratio of the amount of the pretreated nano-indium tin oxide to the modified solution in step B2 is 1 g:20 mL.
[0017] Preferably, the specific preparation steps of the fluorinated modified polyurethane are as follows:
[0018] C1: Add polyurethane to dimethylformamide, heat to 50°C in a water bath, stir evenly, and obtain a polyurethane solution with a concentration of 10wt%; slowly add 1H,1H,2H,2H-perfluorodecyltrimethoxysilane to the polyurethane solution, and add dibutyltin dilaurate at the same time, heat to 80-90°C in a water bath, stir to react for 3-4h, and after the reaction is completed, stand at room temperature for 24-48h, and vacuum dry at 80°C to constant weight to obtain fluorinated modified polyurethane.
[0019] Preferably, in step C1, the ratio of the amount of the polyurethane to 1H,1H,2H,2H-perfluorodecyltrimethoxysilane is 10 g:0.5 mL; and the amount of dibutyltin dilaurate is 0.5-1% of the mass of the polyurethane.
[0020] Preferably, the antioxidant is any one of 2,6-di-tert-butyl-4-methylphenol, triphenyl phosphate, 2,2,6,6-tetramethylpiperidinol and tetraethylenepentamine.
[0021] Preferably, another aspect of the present invention is to provide a method for preparing a highly efficient sun-proof and heat-insulating composite solar film, and the specific preparation steps are as follows:
[0022] S1: Add polyvinyl alcohol to deionized water, heat in a water bath to 80-90°C, and stir at 300 rpm to dissolve evenly to obtain a polyvinyl alcohol solution; add polyvinyl pyrrolidone to the polyvinyl alcohol solution, continue to dissolve evenly at the above temperature and stirring speed, then add 2-hydroxy-4-methoxybenzophenone and silane-modified nano-titanium dioxide, stir and disperse evenly to obtain component solution A;
[0023] S2: adding fluorinated modified polyurethane to the ethanol solution, heating in a water bath to 50-60°C, stirring at 500 rpm to dissolve evenly, adding stearic acid-modified nano-indium tin oxide and antioxidant, and dispersing evenly by 30W ultrasonic treatment to obtain component solution B;
[0024] S3: coating the component solution A prepared in step S1 on the cleaned glass substrate with a coating thickness of 50-100 μm, a pre-curing temperature of 80-100°C, a relative humidity of 50%, and a time of 10-15 min to obtain a substrate coating; coating the component solution B prepared in step S2 for a second time with a coating thickness of 20-30 μm, and microwave curing with the parameters set to 800 W for initial treatment for 3-5 min, then 1000 W for treatment for 5 min, and naturally cooling to room temperature after the treatment to obtain a composite solar film.
[0025] Preferably, in step S1, the ratio of the amount of polyvinyl alcohol, polyvinyl pyrrolidone and deionized water is 1g:15mL:0.5g; the amount of 2-hydroxy-4-methoxybenzophenone is 1-2% of the mass of polyvinyl alcohol; and the amount of silane-modified nano-titanium dioxide is 3-5% of the mass of polyvinyl alcohol.
[0026] Preferably, the ratio of the amount of the fluorinated modified polyurethane to the ethanol solution in step S2 is 1 g:15 mL; the mass amount of the stearic acid-modified nano indium tin oxide is 2-5% of the mass of the fluorinated modified polyurethane; and the mass amount of the antioxidant is 0.5% of the mass of the fluorinated modified polyurethane.
[0027] The beneficial effects of the present invention are as follows:
[0028] The present invention utilizes the hydrophilicity of polyvinyl alcohol (PVA) to improve the dispersibility of the ultraviolet absorber (2-hydroxy-4-methoxybenzophenone) in the matrix, ensures that it is evenly distributed in the film, thereby improving the ultraviolet absorption efficiency and ensuring a long-term stable shielding effect. The hydrophilic polyvinyl alcohol matrix can improve the interface bonding between nanoparticles (TiO2) and the matrix, and the nanoparticles modified by hydrophilic silane form a strong interaction with the hydrophilic matrix, thereby improving the dispersibility and stability, thereby enhancing the mechanical and optical properties of the composite material. The hydrophilicity of polyvinyl alcohol also enhances the wettability of the film, making the film easier to combine with substrates such as glass, enhancing adhesion, reducing separation caused by humidity changes, and maintaining long-term adhesion. Polyvinyl alcohol itself is transparent and hygroscopic, which helps to improve the transparency and wettability of the composite film, and after adding the ultraviolet absorber, it can effectively absorb ultraviolet rays. The wide ultraviolet absorption range of TiO2 further enhances the shielding effect, and the scattering effect of the nanoparticles helps to improve the optical haze without affecting the transparency.
[0029] The present invention uses polyurethane as a hydrophobic material to prevent water penetration, reduce the hygroscopic expansion of the film, and maintain the stability of the film. Indium tin oxide (ITO) metal oxide nanoparticles are added to the polyurethane to reflect near-infrared rays, reduce heat penetration, and improve the heat insulation effect; the high refractive index of the nanoparticles helps to form a multilayer interference structure, further enhancing the infrared reflection ability. Polyurethane also has good weather resistance and chemical resistance, resistance to ultraviolet aging and environmental erosion, and the addition of antioxidants can further improve its weather resistance; after the surface is modified by fluorine-containing compounds, the hydrophobicity of the polyurethane is improved, water droplet adhesion and pollution are reduced, and the cleanliness and self-cleaning ability are enhanced. In addition, silane-modified nanoparticles improve dispersibility and interface bonding, enhance the mechanical and optical properties of the composite material, and improve weather resistance and anti-fouling properties. Stearic acid-modified nano-ITO and nano-TiO2 can form complementary shielding and scattering effects in the composite material; ITO can effectively reflect near-infrared rays, and TiO2 has a wide ultraviolet absorption range. The combination of the two can significantly improve the optical shielding effect of the material. The combination of stearic acid-modified nano-ITO and polyurethane can significantly improve the waterproofness and mechanical properties of the composite material; polyurethane itself has good elasticity and toughness, and stearic acid-modified nano-ITO enhances its hydrophobicity and weather resistance, making the material more suitable for outdoor use; in addition, the infrared reflection ability of nano-ITO combined with the thermal insulation effect of polyurethane can significantly improve the thermal insulation performance of the composite material.
[0030] The present invention utilizes the good mechanical strength and toughness of polyvinyl alcohol and further improves its performance by blending polyvinyl pyrrolidone (PVP). Fluorinated modified polyurethane has a high elastic modulus and toughness, which enhances the tear resistance and wear resistance of the composite film, and provides a buffering effect to reduce external force damage. The hydrophobic surface reduces the adhesion of dust and dirt, facilitates cleaning and maintenance, and maintains the aesthetics of the film. The biodegradable properties of polyvinyl alcohol help reduce environmental pollution, while the production process using aqueous solvents reduces VOC emissions; fluoride modification can reduce the release of harmful substances, and combined with the biodegradability of polyvinyl alcohol and the aqueous production process, it embodies environmental advantages. By combining the matrix polymer polyvinyl alcohol, functional polymer polyurethane and composite nanoparticles, the composite solar film exhibits excellent thermal insulation, weather resistance, mechanical properties, safety and environmental friendliness. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0032] Figure 1It is a melting point test diagram of the composite solar film prepared in Examples 2 to 3 of the present invention and Comparative Examples 1 to 4;
[0033] Figure 2 It is a test chart of chemical stability of the composite solar films prepared in Examples 2 to 3 of the present invention and Comparative Examples 1 to 4. DETAILED DESCRIPTION
[0034] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. It should be noted that, unless otherwise specified, the raw materials involved in the present invention are purchased through conventional commercial channels.
[0035] Embodiment 1: A highly efficient sun-proof and heat-insulating composite solar film, composed of a base polymer A and a functional polymer B. The base polymer A is composed of the following raw materials: polyvinyl alcohol, polyvinyl pyrrolidone, 2-hydroxy-4-methoxybenzophenone, and silane-modified nano titanium dioxide; the functional polymer B is composed of the following raw materials: fluorinated modified polyurethane, stearic acid-modified nano indium tin oxide, and an antioxidant.
[0036] 1. Preparation of silane-modified nano-titanium dioxide:
[0037] A1: Disperse nano-titanium oxide in a 50wt% ethanol solution, and mix evenly by 30W ultrasonic treatment to obtain a 2wt% nano-titanium oxide solution; add 20mL of 3-aminopropyltriethoxysilane to 200mL of the 50wt% ethanol solution, stir and mix evenly to obtain a coupling agent solution;
[0038] A2: Add 100 mL of the nano titanium dioxide solution prepared in step A1 to 100 mL of the coupling agent solution prepared in step A1, heat in a water bath to control the temperature at 30°C, stir and react for 18 hours, add 60 mL of 0.1 M acetic acid solution to neutralize the reaction, centrifuge, filter, wash with deionized water 3 times, and vacuum dry at 80°C to constant weight to obtain silane-modified nano titanium dioxide;
[0039] 2. Preparation of stearic acid modified nano indium tin oxide:
[0040] B1: Treat nano-indium tin oxide in a vacuum drying oven at 60°C for 12 hours to obtain pretreated nano-indium tin oxide; add 2 g of octadecanoic acid to 200 mL of 60 wt% ethanol solution, heat to 60°C in a water bath, stir and mix well to obtain a modified solution;
[0041] B2: Add 10 g of the pretreated nano-indium tin oxide prepared in step A1 to 200 mL of the modified solution prepared in step A1, perform 30 W ultrasonic treatment for 30 min, heat to 50° C. in a water bath, stir and react for 4 h, centrifuge, filter, wash with ethanol 3 times, and vacuum dry at 60° C. to constant weight to obtain stearic acid-modified nano-indium tin oxide;
[0042] 3. Preparation of fluorinated modified polyurethane:
[0043] C1: Add 10g of polyurethane to 90mL of dimethylformamide, heat to 50°C in a water bath, stir evenly, and obtain a polyurethane solution with a concentration of 10wt%; slowly add 0.5mL of 1H,1H,2H,2H-perfluorodecyltrimethoxysilane to the polyurethane solution, and add 0.05g of dibutyltin dilaurate at the same time, heat to 80°C in a water bath, stir and react for 4h, and after the reaction is completed, stand at room temperature for 24h, and vacuum dry at 80°C to constant weight to obtain a fluorinated modified polyurethane;
[0044] 4. Preparation of high-efficiency sun-proof and heat-insulating composite solar film:
[0045] S1: Add 10g of polyvinyl alcohol to 150mL of deionized water, heat in a water bath to 80°C, and stir at 300rpm to dissolve evenly to obtain a polyvinyl alcohol solution; add 5g of polyvinyl pyrrolidone to the polyvinyl alcohol solution, continue to dissolve evenly at the above temperature and stirring speed, then add 0.1g of 2-hydroxy-4-methoxybenzophenone and 0.3g of silane-modified nano-titanium dioxide, stir and disperse evenly to obtain component solution A;
[0046] S2: Add 10 g of fluorinated modified polyurethane to 150 mL of ethanol solution, heat to 50°C in a water bath, stir at 500 rpm to dissolve evenly, add 0.2 g of stearic acid-modified nano-indium tin oxide and 0.05 g of 2,6-di-tert-butyl-4-methylphenol, and disperse evenly by 30 W ultrasonic treatment to obtain component solution B;
[0047] S3: coating the component solution A prepared in step S1 on the cleaned glass substrate with a coating thickness of 50 μm, a pre-curing temperature of 80°C, a relative humidity of 50%, and a time of 10 min to obtain a substrate coating; coating the component solution B prepared in step S2 for a second time with a coating thickness of 20 μm, and microwave curing with the parameters set to 800 W for initial treatment for 3 min, then 1000 W for treatment for 5 min, and naturally cooling to room temperature after the treatment to obtain a composite solar film.
[0048] Embodiment 2: A highly efficient sun-proof and heat-insulating composite solar film, composed of a base polymer A and a functional polymer B. The base polymer A is composed of the following raw materials: polyvinyl alcohol, polyvinyl pyrrolidone, 2-hydroxy-4-methoxybenzophenone, and silane-modified nano titanium dioxide; the functional polymer B is composed of the following raw materials: fluorinated modified polyurethane, stearic acid-modified nano indium tin oxide, and an antioxidant.
[0049] 1. Preparation of silane-modified nano-titanium dioxide:
[0050] A1: Disperse nano-titanium oxide in a 50wt% ethanol solution, and mix evenly by 30W ultrasonic treatment to obtain a 2wt% nano-titanium oxide solution; add 20mL of 3-aminopropyltriethoxysilane to 280mL of the 50wt% ethanol solution, stir and mix evenly to obtain a coupling agent solution;
[0051] A2: Add 100 mL of the nano titanium dioxide solution prepared in step A1 to 180 mL of the coupling agent solution prepared in step A1, heat in a water bath to control the temperature at 45°C, stir and react for 12 h, add 60 mL of 0.1 M acetic acid solution to neutralize the reaction, centrifuge, filter, wash with deionized water 5 times, and vacuum dry at 80°C to constant weight to obtain silane-modified nano titanium dioxide;
[0052] 2. Preparation of stearic acid modified nano indium tin oxide:
[0053] B1: Treat nano-indium tin oxide in a vacuum drying oven at 60°C for 12 hours to obtain pretreated nano-indium tin oxide; add 3.6 g of octadecanoic acid to 200 mL of 60 wt% ethanol solution, heat to 60°C in a water bath, stir and mix well to obtain a modified solution;
[0054] B2: Add 10 g of the pretreated nano-indium tin oxide prepared in step A1 to 200 mL of the modified solution prepared in step A1, perform 30 W ultrasonic treatment for 30 min, heat to 70° C. in a water bath, stir and react for 3 h, centrifuge, filter, wash with ethanol 5 times, and vacuum dry at 60° C. to constant weight to obtain stearic acid-modified nano-indium tin oxide;
[0055] 3. Preparation of fluorinated modified polyurethane:
[0056] C1: Add 10g of polyurethane to 90mL of dimethylformamide, heat to 50°C in a water bath, stir evenly, and obtain a polyurethane solution with a concentration of 10wt%; slowly add 0.5mL of 1H,1H,2H,2H-perfluorodecyltrimethoxysilane to the polyurethane solution, and add 0.08g of dibutyltin dilaurate at the same time, heat to 85°C in a water bath, stir and react for 3h, and after the reaction is completed, stand at room temperature for 36h, and vacuum dry at 80°C to constant weight to obtain a fluorinated modified polyurethane;
[0057] 4. Preparation of high-efficiency sun-proof and heat-insulating composite solar film:
[0058] S1: Add 10g of polyvinyl alcohol to 150mL of deionized water, heat in a water bath to 85°C, and stir at 300rpm to dissolve evenly to obtain a polyvinyl alcohol solution; add 5g of polyvinyl pyrrolidone to the polyvinyl alcohol solution, continue to dissolve evenly at the above temperature and stirring speed, then add 0.18g of 2-hydroxy-4-methoxybenzophenone and 0.45g of silane-modified nano-titanium dioxide, stir and disperse evenly to obtain component solution A;
[0059] S2: Add 10 g of fluorinated modified polyurethane to 150 mL of ethanol solution, heat in a water bath to 55°C, stir at 500 rpm to dissolve evenly, add 0.4 g of stearic acid-modified nano-indium tin oxide and 0.05 g of triphenyl phosphate, and disperse evenly by 30 W ultrasonic treatment to obtain component solution B;
[0060] S3: coating the component solution A prepared in step S1 on the cleaned glass substrate with a coating thickness of 60 μm, a pre-curing temperature of 90°C, a relative humidity of 50%, and a time of 12 min to obtain a substrate coating; coating the component solution B prepared in step S2 for a second time with a coating thickness of 25 μm, and microwave curing with the parameters set to 800 W for initial treatment for 4 min, then 1000 W for treatment for 5 min, and naturally cooling to room temperature after the treatment to obtain a composite solar film.
[0061] Example 3: A highly efficient sun-proof and heat-insulating composite solar film, composed of a base polymer A and a functional polymer B. The base polymer A is composed of the following raw materials: polyvinyl alcohol, polyvinyl pyrrolidone, 2-hydroxy-4-methoxybenzophenone, and silane-modified nano titanium dioxide; the functional polymer B is composed of the following raw materials: fluorinated modified polyurethane, stearic acid-modified nano indium tin oxide, and an antioxidant.
[0062] 1. Preparation of silane-modified nano-titanium dioxide:
[0063] A1: Disperse nano-titanium oxide in a 50wt% ethanol solution, and mix evenly by 30W ultrasonic treatment to obtain a 2wt% nano-titanium oxide solution; add 20mL of 3-aminopropyltriethoxysilane to 250mL of the 50wt% ethanol solution, stir and mix evenly to obtain a coupling agent solution;
[0064] A2: Add 100 mL of the nano titanium dioxide solution prepared in step A1 to 150 mL of the coupling agent solution prepared in step A1, heat in a water bath to control the temperature at 40°C, stir and react for 12 h, add 60 mL of 0.1 M acetic acid solution to neutralize the reaction, centrifuge, filter, wash with deionized water 4 times, and vacuum dry at 80°C to constant weight to obtain silane-modified nano titanium dioxide;
[0065] 2. Preparation of stearic acid modified nano indium tin oxide:
[0066] B1: Treat nano-indium tin oxide in a vacuum drying oven at 60°C for 12 hours to obtain pretreated nano-indium tin oxide; add 3 g of octadecanoic acid to 200 mL of 60 wt% ethanol solution, heat to 60°C in a water bath, stir and mix well to obtain a modified solution;
[0067] B2: Add 10 g of the pretreated nano-indium tin oxide prepared in step A1 to 200 mL of the modified solution prepared in step A1, perform 30 W ultrasonic treatment for 30 min, heat to 60° C. in a water bath, stir and react for 3 h, centrifuge, filter, wash with ethanol 4 times, and vacuum dry at 60° C. to constant weight to obtain stearic acid-modified nano-indium tin oxide;
[0068] 3. Preparation of fluorinated modified polyurethane:
[0069] C1: Add 10g of polyurethane to 90mL of dimethylformamide, heat to 50°C in a water bath, stir evenly, and obtain a polyurethane solution with a concentration of 10wt%; slowly add 0.5mL of 1H,1H,2H,2H-perfluorodecyltrimethoxysilane to the polyurethane solution, and add 0.06g of dibutyltin dilaurate at the same time, heat to 85°C in a water bath, stir and react for 3h, and after the reaction is completed, stand at room temperature for 40h, and vacuum dry at 80°C to constant weight to obtain a fluorinated modified polyurethane;
[0070] 4. Preparation of high-efficiency sun-proof and heat-insulating composite solar film:
[0071] S1: Add 10g of polyvinyl alcohol to 150mL of deionized water, heat in a water bath to 80°C, and stir at 300rpm to dissolve evenly to obtain a polyvinyl alcohol solution; add 5g of polyvinyl pyrrolidone to the polyvinyl alcohol solution, continue to dissolve evenly at the above temperature and stirring speed, then add 0.15g of 2-hydroxy-4-methoxybenzophenone and 0.4g of silane-modified nano-titanium dioxide, stir and disperse evenly to obtain component solution A;
[0072] S2: Add 10 g of fluorinated modified polyurethane to 150 mL of ethanol solution, heat in a water bath to 50°C, stir at 500 rpm to dissolve evenly, add 0.3 g of stearic acid-modified nano-indium tin oxide and 0.05 g of tetraethylene pentamine, and disperse evenly by 30 W ultrasonic treatment to obtain component solution B;
[0073] S3: coating the component solution A prepared in step S1 on the cleaned glass substrate with a coating thickness of 80 μm, a pre-curing temperature of 80°C, a relative humidity of 50%, and a time of 12 min to obtain a substrate coating; coating the component solution B prepared in step S2 for a second time with a coating thickness of 25 μm, and microwave curing with the parameters set to 800 W for initial treatment for 4 min, then 1000 W for treatment for 5 min, and naturally cooling to room temperature after the treatment to obtain a composite solar film.
[0074] Example 4: A highly efficient sun-proof and heat-insulating composite solar film, composed of a base polymer A and a functional polymer B. The base polymer A is composed of the following raw materials: polyvinyl alcohol, polyvinyl pyrrolidone, 2-hydroxy-4-methoxybenzophenone, and silane-modified nano titanium dioxide; the functional polymer B is composed of the following raw materials: fluorinated modified polyurethane, stearic acid-modified nano indium tin oxide, and an antioxidant.
[0075] 1. Preparation of silane-modified nano-titanium dioxide:
[0076] A1: Disperse nano-titanium oxide in a 50wt% ethanol solution, and mix evenly by 30W ultrasonic treatment to obtain a 2wt% nano-titanium oxide solution; add 20mL of 3-aminopropyltriethoxysilane to 300mL of the 50wt% ethanol solution, stir and mix evenly to obtain a coupling agent solution;
[0077] A2: Add 100 mL of the nano titanium dioxide solution prepared in step A1 to 200 mL of the coupling agent solution prepared in step A1, heat in a water bath to control the temperature at 50°C, stir and react for 8 hours, add 60 mL of 0.1 M acetic acid solution to neutralize the reaction, centrifuge, filter, wash with deionized water 5 times, and vacuum dry at 80°C to constant weight to obtain silane-modified nano titanium dioxide;
[0078] 2. Preparation of stearic acid modified nano indium tin oxide:
[0079] B1: Treat nano-indium tin oxide in a vacuum drying oven at 60°C for 12 hours to obtain pretreated nano-indium tin oxide; add 4 g of octadecanoic acid to 200 mL of 60 wt% ethanol solution, heat to 60°C in a water bath, stir and mix well to obtain a modified solution;
[0080] B2: Add 10 g of the pretreated nano-indium tin oxide prepared in step A1 to 200 mL of the modified solution prepared in step A1, perform 30 W ultrasonic treatment for 30 min, heat to 70° C. in a water bath, stir and react for 2 h, centrifuge, filter, wash with ethanol 5 times, and vacuum dry at 60° C. to constant weight to obtain stearic acid-modified nano-indium tin oxide;
[0081] 3. Preparation of fluorinated modified polyurethane:
[0082] C1: Add 10g of polyurethane to 90mL of dimethylformamide, heat to 50°C in a water bath, stir evenly, and obtain a polyurethane solution with a concentration of 10wt%; slowly add 0.5mL of 1H,1H,2H,2H-perfluorodecyltrimethoxysilane to the polyurethane solution, and add 0.1g of dibutyltin dilaurate at the same time, heat to 90°C in a water bath, stir to react for 3h, and after the reaction is completed, stand at room temperature for 48h, and vacuum dry at 80°C to constant weight to obtain a fluorinated modified polyurethane;
[0083] 4. Preparation of high-efficiency sun-proof and heat-insulating composite solar film:
[0084] S1: Add 10g of polyvinyl alcohol to 150mL of deionized water, heat in a water bath to 90°C, and stir at 300rpm to dissolve evenly to obtain a polyvinyl alcohol solution; add 5g of polyvinyl pyrrolidone to the polyvinyl alcohol solution, continue to dissolve evenly at the above temperature and stirring speed, then add 0.2g of 2-hydroxy-4-methoxybenzophenone and 0.5g of silane-modified nano-titanium dioxide, stir and disperse evenly to obtain component solution A;
[0085] S2: Add 10 g of fluorinated modified polyurethane to 150 mL of ethanol solution, heat to 60°C in a water bath, stir at 500 rpm to dissolve evenly, add 0.5 g of stearic acid-modified nano-indium tin oxide and 0.05 g of 2,2,6,6-tetramethylpiperidinol, and disperse evenly by 30 W ultrasonic treatment to obtain component solution B;
[0086] S3: coating the component solution A prepared in step S1 on the cleaned glass substrate with a coating thickness of 100 μm, a pre-curing temperature of 100°C, a relative humidity of 50%, and a time of 15 min to obtain a substrate coating; coating the component solution B prepared in step S2 for a second time with a coating thickness of 30 μm, and microwave curing with the parameters set to 800 W for initial treatment for 5 min, then 1000 W for treatment for 5 min, and naturally cooling to room temperature after the treatment to obtain a composite solar film.
[0087] Comparative Example 1: The operation of Comparative Example 1 is basically the same as that of Example 2, except that polyurethane is used instead of fluorinated modified polyurethane in Comparative Example 1.
[0088] Comparative Example 2: The operation of Comparative Example 2 is basically the same as that of Example 2, except that silane-modified nano-titanium dioxide is not added in Comparative Example 2.
[0089] Comparative Example 3: The operation of Comparative Example 3 is basically the same as that of Example 3, except that in Comparative Example 3, nano indium tin oxide is used instead of stearic acid-modified nano indium tin oxide.
[0090] Comparative Example 4: In Comparative Example 4, hydrophobic polymethyl methacrylate is used instead of polyvinyl alcohol as the base material. The difference between the preparation steps of Comparative Example 4 and Example 3 lies in the preparation of the highly efficient sun-proof and heat-insulating composite solar film. The specific preparation steps are as follows:
[0091] S1: Add 10g of polymethyl methacrylate to 90mL of acetone, heat to 60°C in a water bath, and stir at 300rpm to dissolve evenly to obtain a 10wt% polymethyl methacrylate solution; add 5g of polyvinyl pyrrolidone to the polyvinyl alcohol solution, heat to 60°C in a water bath, and stir to dissolve evenly, then add 0.15g of 2-hydroxy-4-methoxybenzophenone and 0.4g of silane-modified nano-titanium dioxide, stir and disperse evenly to obtain component solution A;
[0092] S2: 10 g of fluorinated modified polyurethane was added to 150 mL of ethanol solution, heated in a water bath to 50°C, stirred at 500 rpm to dissolve evenly, then 0.3 g of stearic acid-modified nano-indium tin oxide, 0.05 g of tetraethylene pentamine and 0.05 g of triphenyl phosphate were added, and dispersed evenly by 30 W ultrasonic treatment to obtain component solution B;
[0093] S3: coating the component solution A prepared in step S1 on the cleaned glass substrate with a coating thickness of 80 μm, pre-curing temperature of 65°C, relative humidity of 50%, and time of 25 min to obtain a substrate coating; coating the component solution B prepared in step S2 for a second time with a coating thickness of 25 μm, microwave curing, setting parameters to 800 W initial treatment for 4 min, then 1000 W treatment for 5 min, and naturally cooling to room temperature after the treatment to obtain a composite solar film.
[0094] Performance Test:
[0095] Melting point test: The composite solar film samples prepared in Examples 2 to 3 of the present invention and Comparative Examples 1 to 4 were placed in a DSC analysis sample tray for testing. The test temperature was set at 25 to 300°C, the heating rate was 10°C / min, and the melting point temperature was recorded. Each sample was tested three times and the average value was taken. The results are shown in the figure. Figure 1 shown.
[0096] Depend on Figure 1The results show that the composite solar film prepared by the present invention can be stably used at a high temperature of 200°C. From the results of Comparative Example 1 and Example 2, it can be seen that the melting point is affected by the replacement of the fluorinated modified polyurethane; from the results of Comparative Example 3 and Example 3, it can be seen that stearic acid-modified ITO can effectively improve the thermal stability of the composite material.
[0097] Chemical stability test: The composite solar films prepared in Examples 2 to 3 and Comparative Examples 1 to 4 were immersed in a 5% NaOH solution for 72 hours, and the changes in light transmittance were recorded. The test results are shown in the figure. Figure 2 shown.
[0098] Depend on Figure 2 The results show that the composite solar film prepared by the present invention exhibits excellent corrosion resistance when immersed in chemicals, and the change in light transmittance is less than 5%.
[0099] Light transmittance test: According to the standard "ASTM D1003 Standard Test Method for Haze and Light Transmittance of Transparent Plastics", the ultraviolet blocking rate and infrared blocking rate of the composite solar films prepared in Examples 2 to 3 and Comparative Examples 1 to 4 were tested using an LS180 solar film tester. The test results are shown in Table 1;
[0100] Abrasion resistance: According to the standard "GB31849-2015 Automobile Film Glass", the haze caused by abrasion of the composite solar films prepared in Examples 2 to 3 and Comparative Examples 1 to 4 was tested using Taber@Abrasion Tester-1700 and YH1200 Haze Meter, respectively. The test results are shown in Table 1;
[0101] Aging resistance: According to the standard "GB31849-2015 Automobile Film Glass", the durability of the composite solar films prepared in Examples 2 to 3 and Comparative Examples 1 to 4 was tested respectively by using an oven with parameters set at 120°C for 200h. The test results are shown in Table 1.
[0102] Table 1. Composite solar film test performance results.
[0103]
[0104] It can be seen from the results in Table 1 that the composite solar film prepared by the present invention can effectively block ultraviolet rays and infrared rays, and has excellent aging resistance. Figure 2 From the results of Comparative Example 1 and Example 2 in Table 1, it can be seen that the fluorinated modified polyurethane has better weather resistance and heat resistance, and the synergy of polyurethane replacing fluorinated modified polyurethane is significantly affected; Figure 2From the results of Comparative Example 2 and Example 2 in Table 1, it can be seen that silane-modified nano-titanium dioxide can improve the weather resistance and heat resistance of the composite material. The absence of silane-modified nano-titanium dioxide significantly affects the ultraviolet and infrared blocking rates, and the synergistic effect between the silane-modified nano-titanium dioxide and the polyvinyl alcohol matrix is affected, and the weather resistance and heat resistance are significantly reduced. Figure 2 From the results of Comparative Example 3 and Example 3 in Table 1, it can be seen that stearic acid-modified ITO nanoparticles can improve the stability of the composite material, and it can improve the interface bonding between the nanoparticles and the matrix; when nano-ITO replaces stearic acid-modified ITO nanoparticles, the synergistic effect between the nano-ITO and the polyurethane is affected, resulting in significant effects on stability and weather resistance; from the results of Comparative Example 4 and Example 3, it can be seen that the hydrophilicity of polyvinyl alcohol can improve the dispersibility of the ultraviolet absorber in the matrix, while the hydrophobicity of polymethyl methacrylate cannot achieve the same effect, resulting in reduced dispersibility of the ultraviolet absorber.
[0105] Hydrophobicity test: The composite solar film materials prepared in the above-mentioned Examples 2-3 and Comparative Examples 1-4 were subjected to contact angle test. The larger the contact angle, the better the hydrophobic effect. A contact angle greater than 140° was recorded as A, a contact angle between 130 and 140° was recorded as B, and a contact angle less than 130° was recorded as C. All samples were tested at room temperature and 50% humidity. A 5 μL water droplet was used for each test. To ensure data reliability, each sample was subjected to 5 contact angle measurements, and the average value was taken as the final result. The test results are shown in Table 2.
[0106] Hydrophobic stability test: The test steps are basically the same as above. The test conditions are divided into three types. The first is tested at a high temperature of 85°C and a humidity of 50%; the second is tested at a humidity of 85% and room temperature; the third is tested at room temperature, a humidity of 50%, and an ultraviolet irradiation UV intensity of 0.5W / m²; the test time is 72h. The test results are shown in Table 2.
[0107] Table 2. Hydrophobicity and stability test results.
[0108]
[0109] It can be seen from the results in Table 2 that the composite solar film prepared by the present invention has excellent hydrophobicity, and also exhibits excellent hydrophobicity under high temperature, high humidity and ultraviolet light. It can be seen from the results of Comparative Example 1 and Example 2 that the polyurethane without fluorination modification is more likely to lose its hydrophobicity, especially under high humidity and ultraviolet light irradiation, the polyurethane absorbs water and degrades, resulting in reduced hydrophobicity; it can be seen from the results of Comparative Example 2 and Example 2 that the lack of silane-modified titanium dioxide makes the composite solar film more likely to absorb water, thereby reducing the hydrophobicity; it can be seen from the results of Comparative Example 3 and Example 3 that the unmodified nano indium tin oxide leads to a decrease in hydrophobicity under high humidity and ultraviolet light irradiation; it can be seen from the results of Comparative Example 4 and Example 3 that polymethyl methacrylate will age and its hydrophobicity will decrease under ultraviolet light.
[0110] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a highly efficient sun-proof and heat-insulating composite solar film, characterized in that: The composite solar film is composed of a matrix polymer A and a functional polymer B; the matrix polymer A comprises the following raw materials: Polyvinyl alcohol, polyvinyl pyrrolidone, 2-hydroxy-4-methoxybenzophenone, silane-modified nano titanium dioxide; the functional polymer B comprises the following raw materials: fluorinated modified polyurethane, stearic acid-modified nano indium tin oxide, and antioxidant; The specific preparation steps of the silane-modified nano titanium dioxide are as follows: A1: Dispersing nano-titanium oxide in an ethanol solution, and mixing evenly with ultrasonic treatment to obtain a nano-titanium oxide solution; adding 3-aminopropyltriethoxysilane to the ethanol solution, and stirring and mixing evenly to obtain a coupling agent solution; A2: adding the nano titanium dioxide solution prepared in step A1 to the coupling agent solution prepared in step A1, heating in a water bath to control the temperature, stirring the reaction, adding acetic acid solution to neutralize the reaction, centrifuging, filtering, washing with deionized water, and vacuum drying to constant weight to obtain silane-modified nano titanium dioxide; The volume ratio of 3-aminopropyltriethoxysilane to ethanol solution in step A1 is 1:10-15; The volume ratio of the nano-titanium oxide solution and the coupling agent solution in step A2 is 1:1-2; the volume of the acetic acid solution is 1 times the volume of the 3-aminopropyltriethoxysilane in step A1; The specific preparation steps of the stearic acid modified nano indium tin oxide are as follows: B1: Treat nano-indium tin oxide in a vacuum drying oven to obtain pretreated nano-indium tin oxide; add octadecanoic acid to the ethanol solution, heat in a water bath to control the temperature, stir and mix evenly to obtain a modified solution; B2: adding the pretreated nano-indium tin oxide prepared in step A1 to the modified solution prepared in step A1, and after ultrasonic treatment, heating in a water bath to control the temperature, stirring for reaction, and after the reaction is completed, centrifuging, filtering, washing with ethanol, and vacuum drying to constant weight to obtain stearic acid-modified nano-indium tin oxide; The ratio of the amount of octadecanoic acid to the ethanol solution in step B1 is 0.1-0.2 g:10 mL; The ratio of the amount of the pretreated nano-indium tin oxide to the modified solution in step B2 is 1 g: 20 mL; The specific preparation steps of the fluorinated modified polyurethane are as follows: C1: Add polyurethane to dimethylformamide, heat in a water bath to control the temperature, stir evenly to obtain a polyurethane solution; slowly add 1H,1H,2H,2H-perfluorodecyltrimethoxysilane to the polyurethane solution, and add dibutyltin dilaurate at the same time, heat in a water bath to control the temperature, stir to react, and after the reaction is completed, stand at room temperature, and vacuum dry to constant weight to obtain a fluorinated modified polyurethane; The ratio of the amount of polyurethane and 1H,1H,2H,2H-perfluorodecyltrimethoxysilane used in step C1 is 10g:0.5mL; the amount of dibutyltin dilaurate used is 0.5-1% of the mass of the polyurethane; The antioxidant is any one of 2,6-di-tert-butyl-4-methylphenol, triphenyl phosphate, 2,2,6,6-tetramethylpiperidinol and tetraethylenepentamine; The specific preparation steps of the composite solar film are as follows: S1: adding polyvinyl alcohol to deionized water, heating in a water bath to control the temperature, stirring and dissolving uniformly to obtain a polyvinyl alcohol solution; adding polyvinyl pyrrolidone to the polyvinyl alcohol solution, continuing to dissolve uniformly at the above temperature and stirring speed, and then adding 2-hydroxy-4-methoxybenzophenone and silane-modified nano-titanium dioxide, stirring and dispersing uniformly to obtain component solution A; S2: adding fluorinated modified polyurethane to the ethanol solution, heating in a water bath to control the temperature, stirring and dissolving uniformly, adding stearic acid-modified nano-indium tin oxide and antioxidant, and ultrasonically dispersing uniformly to obtain component solution B; S3: coating the component solution A prepared in step S1 on the cleaned glass substrate with a coating thickness of 50-100 μm, a pre-curing temperature of 80-100°C, a relative humidity of 50%, and a time of 10-15 min to obtain a substrate coating; coating the component solution B prepared in step S2 for a second time with a coating thickness of 20-30 μm, and microwave curing with the parameters set to 800 W for initial treatment for 3-5 min, then 1000 W for treatment for 5 min, and naturally cooling to room temperature after the treatment to obtain a composite solar film.
2. The method for preparing a highly efficient sun-proof and heat-insulating composite solar film according to claim 1, characterized in that: The ratio of the amount of polyvinyl alcohol, polyvinyl pyrrolidone and deionized water in step S1 is 1g:15mL:0.5g; the amount of 2-hydroxy-4-methoxybenzophenone is 1-2% of the mass of polyvinyl alcohol; and the amount of silane-modified nano-titanium dioxide is 3-5% of the mass of polyvinyl alcohol.
3. The method for preparing a highly efficient sun-proof and heat-insulating composite solar film according to claim 2, characterized in that: The ratio of the amount of the fluorinated modified polyurethane to the ethanol solution in step S2 is 1 g:15 mL; the mass amount of the stearic acid-modified nano indium tin oxide is 2-5% of the mass of the fluorinated modified polyurethane; and the mass amount of the antioxidant is 0.5% of the mass of the fluorinated modified polyurethane.