A method for preparing a self-repairing modified polyurethane coating for car cover

By reacting under nitrogen conditions to form a modified polyurethane emulsion and applying it on a tinplate sheet, the crack problem of the polyurethane coating under the action of the environment is solved, and the self-healing, antibacterial and flame retardant properties of the polyurethane coating are improved, forming a Excellent performance coating for car clothes.

CN118638467BActive Publication Date: 2024-11-19TIANJIN DINGRENHESHI NEW MATERIAL TECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410685035.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-30
Publication Date
2024-11-19
Estimated Expiration
2044-05-30

AI Technical Summary

Technical Problem

The existing polyurethane coatings are prone to cracks under the action of mechanical, thermal, ultraviolet rays, etc., resulting in material failure. The traditional repair methods cannot meet the material repair requirements, and the existing self-repaired polyurethane coatings fail to improve the flame retardant effect.

Method used

Using the reaction of isofluron diisocyanate, modified quaternary ammonium diol intermediate, dibutyltin bislaurate and other raw materials under nitrogen conditions, dihydroxymethylpropionic acid, hydroquinone and triethylamine are added. A modified polyurethane emulsion is formed, and a self-repaired modified polyurethane coating is obtained by drying the car coat, which is coated on the tinplate sheet, and the flame retardant and self-healing properties are improved using phosphorus, nitrogen and dynamic covalent bonds.

Benefits of technology

The prepared polyurethane coating has excellent self-healing properties, antibacterial properties and flame retardant properties. It forms a dense protective layer through the formation of phosphoric acid and flame retardant gas, hinders oxygen contact with the material, improves flame retardant effect, and passes through the quaternary ammonium salt. Electrostatic action achieves antibacterial effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118638467B_ABST
    Figure CN118638467B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of coatings, and discloses a method for preparing a self-repairing modified polyurethane coating for car clothing, the present invention uses N-(4-hydroxyphenyl) maleimide and phenylphosphoryl dichloride as raw materials, and through substitution reaction, obtains a phosphorus-containing bismaleimide intermediate, and uses N, N-bis(3-aminopropyl)-2-furanmethylamine, α-lipoic acid, 4-chloro-1-butanol, etc. as raw materials, and through amidation reaction, quaternization reaction, obtains a furan-containing quaternary ammonium salt intermediate. Using phosphorus-containing bismaleimide intermediates and furan-containing quaternary ammonium salt intermediates, modified quaternary ammonium salt diol intermediates are synthesized, and then using isophorone diisocyanate, modified quaternary ammonium salt diol intermediates, polycarbonate diols, etc. as raw materials, a modified polyurethane emulsion is obtained, which is applied to a tinplate sheet, dried, and a self-repairing modified polyurethane coating for car clothing is obtained. The polyurethane coating prepared by the present invention has excellent self-repairing performance, antibacterial performance, and flame retardant performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, and in particular to a method for preparing a self-repairing modified polyurethane coating for vehicle covers. Background Art

[0002] Polyurethane, also known as polyurethane, is a nitrogen-containing heterochain polymer. As a high-performance coating material, it is widely used in furniture, medical, electronics and other fields. However, in daily processing and practical applications, polyurethane coating materials are easily affected by mechanical, thermal, ultraviolet radiation and other environmental factors, which will cause cracks inside and lose their protective properties. If they are not repaired, the cracks will further extend, causing material failure and shortening their service life. However, the use of traditional repair methods such as bonding and welding to repair the material cannot meet the requirements of material repair. Self-healing materials can self-repair like organisms by imitating the self-healing mechanism of organisms, thereby extending the life of the material, making the material more reliable and durable, and having a wider range of applications. Therefore, exploring coating materials with self-healing properties has become a key issue.

[0003] With the continuous progress and development of science and technology, self-repair systems are divided into intrinsic self-repair and external self-repair. External self-repair, as the name suggests, refers to the addition of external repair agents to achieve the purpose of repair; intrinsic self-repair uses the chemical bonds contained in the polymer to break or recombine under the stimulation of external light or heat, and completes the self-repair of polymer materials without the need to add additional repair agents or catalysts in the matrix. It has better research value than external self-repair.

[0004] For example, the patent with application publication number CN 113789114 A discloses a self-healing antibacterial polyurethane coating and a preparation method thereof. The invention uses modified graphene, amino silicone oil, etc. as raw materials, and the prepared polyurethane material has good antibacterial and self-healing effects, but does not improve the flame retardant effect of the polyurethane coating. Summary of the invention

[0005] 1. Technical issues to be resolved

[0006] In view of the deficiencies in the prior art, the present invention provides a method for preparing a self-repairing modified polyurethane coating for car covers. The polyurethane coating prepared by the present invention has excellent self-repairing properties, antibacterial properties and flame retardant properties.

[0007] (II) Technical solution

[0008] A method for preparing a self-repairing modified polyurethane coating for a car cover, the preparation method comprising:

[0009] (1) Under nitrogen conditions, isophorone diisocyanate, a modified quaternary ammonium salt diol intermediate, and 0.1-0.3% of dibutyltin dilaurate are added to polycarbonate diol, stirred and dispersed, and reacted at 80-90° C. for 2-4 hours. Dimethylolpropionic acid and hydroquinone are then added thereto and the reaction is continued for 3-8 hours. After the reaction is completed, triethylamine is added thereto for neutralization, and deionized water is added thereto, stirred and dispersed to obtain a modified polyurethane emulsion.

[0010] (2) The tinplate sheet is polished with 8000-mesh sandpaper, washed with deionized water, and dried. The modified polyurethane emulsion is coated on the tinplate sheet and dried in an oven at 80° C. for 24-30 hours to obtain a self-repairing modified polyurethane coating for car covers.

[0011] Preferably, in the step (1), the usage ratio of isophorone diisocyanate, modified quaternary ammonium salt diol intermediate, polycarbonate diol, dimethylol propionic acid, hydroquinone and triethylamine is (40-70) g: (5-15) g: 100 g: (5-8) g: (2-8) g: (5-10) mL.

[0012] Preferably, in step (1), the preparation method of the modified quaternary ammonium salt diol intermediate is as follows:

[0013] S1. Add N-(4-hydroxyphenyl)maleimide and triethylamine to tetrahydrofuran solvent, stir and disperse, then add phenylphosphoryl dichloride, react at 60-70°C for 20-48h. After the reaction is completed, filter, rotary evaporate, wash with deionized water, and dry to obtain a phosphorus-containing bismaleimide intermediate.

[0014] S2. Add N,N-di(3-aminopropyl)-2-furanmethylamine and α-lipoic acid to tetrahydrofuran solvent, stir and disperse, then add 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 4-dimethylaminopyridine, stir and react at 20-35°C for 12-24h. After the reaction is completed, wash with saturated sodium chloride solution and dry to obtain intermediate 1.

[0015] S3. Add the intermediate 1, 4-chloro-1-butanol to acetonitrile solvent, stir and disperse, heat to 60-70°C, react for 12-24h, and after the reaction, distill under reduced pressure, wash with ethanol, and dry to obtain a furan quaternary ammonium salt intermediate.

[0016] S4. Add the phosphorus-containing bismaleimide intermediate to tetrahydrofuran solvent, stir and disperse, then add the furan-containing quaternary ammonium salt intermediate thereto, stir and react at 60-70° C. for 24-48 hours. After the reaction is completed, wash with ethyl acetate and dry to obtain a modified quaternary ammonium salt diol intermediate.

[0017] Preferably, in step S1, the molar ratio of N-(4-hydroxyphenyl)maleimide, triethylamine and phenylphosphoryl dichloride is 2-2.4:2.2-2.8:1.

[0018] Preferably, in step S2, the molar ratio of N,N-bis(3-aminopropyl)-2-furanmethylamine, α-lipoic acid, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, and 4-dimethylaminopyridine is 1:2.5-4:3-3.5:0.1-0.3.

[0019] Preferably, in step S3, the molar ratio of the intermediate 1 to 4-chloro-1-butanol is 1:1-1.5.

[0020] Preferably, in step S4, the molar ratio of the phosphorus-containing bismaleimide intermediate to the furanic quaternary ammonium salt intermediate is 1:2-3.

[0021] (III) Beneficial technical effects

[0022] The present invention uses N-(4-hydroxyphenyl) maleimide and phenylphosphoryl dichloride as raw materials, and obtains a phosphorus-containing bismaleimide intermediate through a substitution reaction under the catalytic reaction of triethylamine. Uses N,N-bis(3-aminopropyl)-2-furanmethylamine and α-lipoic acid as raw materials, and undergoes an amidation reaction under the catalysis of EDC and DMAP to obtain an intermediate 1, and uses the tertiary amine group contained therein to undergo a quaternization reaction with 4-chloro-1-butanol to obtain a furan quaternary ammonium salt intermediate. Using the phosphorus-containing bismaleimide intermediate and the furan quaternary ammonium salt intermediate, a modified quaternary ammonium salt diol intermediate is synthesized, and then using isophorone diisocyanate, a modified quaternary ammonium salt diol intermediate, a polycarbonate diol, etc. as raw materials, a modified polyurethane emulsion is prepared, and then the emulsion is coated on a tinplate sheet and dried to obtain a self-repairing modified polyurethane coating for car covers.

[0023] The polyurethane coating prepared by the present invention contains phosphorus and nitrogen. When burning, the phosphorus can generate strong dehydrating substances such as phosphoric acid and metaphosphoric acid by heat, promote the dehydration and carbonization of the material, form a dense protective layer on the surface of the material, isolate the contact between oxygen and the material, and hinder the transfer of heat. The nitrogen contained therein generates non-flammable gas by heat, which can dilute the flammable gas in the air. The two elements complement each other and jointly improve the flame retardant effect.

[0024] The quaternary ammonium salt contained in the polyurethane coating prepared by the present invention has good antibacterial effect. This is because the positively charged groups contained in the quaternary ammonium salt can be adsorbed to the surface of microbial bacteria with negative charges through electrostatic action, combine with the phospholipid bilayer in the cell plasma membrane, destroy the cell plasma membrane, cause bacterial cell death, and achieve good antibacterial effect.

[0025] The polyurethane coating prepared by the present invention contains disulfide bonds and DA bonds, both of which are dynamic covalent bonds. When they are added to the polyurethane coating, when the material is damaged, the reversible dynamic chemical bonds contained therein are rearranged, which can promote the movement and reaction of the internal chain segments and thus promote the damage repair, further improving the self-repairing performance of the polyurethane coating. The polyurethane coating prepared by the present invention has excellent antibacterial properties, flame retardant properties and self-repairing properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a preparation route for phosphorus-containing bismaleimide intermediates;

[0027] Figure 2 It is a preparation route for furan quaternary ammonium salt intermediates. DETAILED DESCRIPTION

[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Example 1

[0030] (1) 0.2 mol of N-(4-hydroxyphenyl)maleimide and 0.26 mol of triethylamine were added to 100 mL of tetrahydrofuran solvent, stirred and dispersed, and then 0.1 mol of phenylphosphoryl dichloride was added thereto. The mixture was reacted at 65° C. for 24 h. After the reaction was completed, the mixture was filtered, rotary evaporated, washed with deionized water, and dried to obtain a phosphorus-containing bismaleimide intermediate.

[0031] (2) 40 mmol of N,N-bis(3-aminopropyl)-2-furanmethylamine and 150 mmol of α-lipoic acid were added to 100 mL of tetrahydrofuran solvent and dispersed by stirring. Then, 130 mmol of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 8 mmol of 4-dimethylaminopyridine were added thereto. The mixture was stirred at 25° C. for 24 h. After the reaction was completed, the mixture was washed with saturated sodium chloride solution and dried to obtain intermediate 1.

[0032] (3) 0.1 mol of intermediate 1 and 0.12 mol of 4-chloro-1-butanol were added to 100 mL of acetonitrile solvent, stirred and dispersed, heated to 65° C., and reacted for 15 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with ethanol, and dried to obtain a furan quaternary ammonium salt intermediate.

[0033] (4) 60 mmol of the phosphorus-containing bismaleimide intermediate was added to 100 mL of tetrahydrofuran solvent, stirred and dispersed, and then 120 mmol of the furan-containing quaternary ammonium salt intermediate was added thereto. The mixture was stirred and reacted at 60° C. for 48 h. After the reaction was completed, the mixture was washed with ethyl acetate and dried to obtain a modified quaternary ammonium salt diol intermediate.

[0034] (5) Under nitrogen conditions, 20 g of isophorone diisocyanate, 2.5 g of a modified quaternary ammonium salt diol intermediate, and 0.1% of dibutyltin dilaurate were added to 50 g of a polycarbonate diol, and the mixture was dispersed with stirring. The mixture was reacted at 85° C. for 3 h, and then 4 g of dimethylolpropionic acid and 2 g of hydroquinone were added thereto and the reaction was continued for 8 h. After the reaction was completed, 5 mL of triethylamine was added thereto for neutralization, and then 180 g of deionized water was added thereto and the mixture was dispersed with stirring to obtain a modified polyurethane emulsion.

[0035] (6) The tinplate sheet was polished with 8000-mesh sandpaper, washed with deionized water, and dried. The modified polyurethane emulsion was coated on the tinplate sheet and dried in an oven at 80° C. for 24 h to obtain a self-repairing modified polyurethane coating for car covers.

[0036] Example 2

[0037] (1) 0.24 mol of N-(4-hydroxyphenyl)maleimide and 0.22 mol of triethylamine were added to 100 mL of tetrahydrofuran solvent, stirred and dispersed, and then 0.1 mol of phenylphosphoryl dichloride was added thereto. The mixture was reacted at 70° C. for 48 h. After the reaction was completed, the mixture was filtered, rotary evaporated, washed with deionized water, and dried to obtain a phosphorus-containing bismaleimide intermediate.

[0038] (2) 40 mmol of N,N-bis(3-aminopropyl)-2-furanmethylamine and 120 mmol of α-lipoic acid were added to 100 mL of tetrahydrofuran solvent and dispersed by stirring. Then, 130 mmol of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 5 mmol of 4-dimethylaminopyridine were added thereto. The mixture was stirred at 25° C. for 24 h. After the reaction was completed, the mixture was washed with saturated sodium chloride solution and dried to obtain intermediate 1.

[0039] (3) 0.1 mol of intermediate 1 and 0.12 mol of 4-chloro-1-butanol were added to 100 mL of acetonitrile solvent, stirred and dispersed, heated to 65° C., and reacted for 20 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with ethanol, and dried to obtain a furan quaternary ammonium salt intermediate.

[0040] (4) 60 mmol of the phosphorus-containing bismaleimide intermediate was added to 100 mL of tetrahydrofuran solvent and dispersed by stirring. Then, 180 mmol of the furan-containing quaternary ammonium salt intermediate was added thereto and stirred for reaction at 70° C. for 24 h. After the reaction was completed, the mixture was washed with ethyl acetate and dried to obtain a modified quaternary ammonium salt diol intermediate.

[0041] (5) Under nitrogen conditions, 25 g of isophorone diisocyanate, 3 g of modified quaternary ammonium salt diol intermediate, and 0.3% of dibutyltin dilaurate were added to 50 g of polycarbonate diol, stirred and dispersed, and reacted at 80° C. for 4 h. Then, 2.5 g of dihydroxymethylpropionic acid and 1 g of hydroquinone were added thereto and the reaction was continued for 4 h. After the reaction was completed, 2.5 mL of triethylamine was added thereto for neutralization, and then 180 g of deionized water was added thereto and stirred and dispersed to obtain a modified polyurethane emulsion.

[0042] (6) The tinplate sheet was polished with 8000-mesh sandpaper, washed with deionized water, and dried. The modified polyurethane emulsion was coated on the tinplate sheet and dried in an oven at 80° C. for 26 h to obtain a self-repairing modified polyurethane coating for car covers.

[0043] Example 3

[0044] (1) 0.24 mol of N-(4-hydroxyphenyl)maleimide and 0.28 mol of triethylamine were added to 100 mL of tetrahydrofuran solvent, stirred and dispersed, and then 0.1 mol of phenylphosphoryl dichloride was added thereto. The mixture was reacted at 60° C. for 20 h. After the reaction was completed, the mixture was filtered, rotary evaporated, washed with deionized water, and dried to obtain a phosphorus-containing bismaleimide intermediate.

[0045] (2) 40 mmol of N,N-bis(3-aminopropyl)-2-furanmethylamine and 160 mmol of α-lipoic acid were added to 100 mL of tetrahydrofuran solvent and dispersed by stirring. Then, 140 mmol of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 5 mmol of 4-dimethylaminopyridine were added thereto. The mixture was stirred at 25° C. for 12 h. After the reaction was completed, the mixture was washed with saturated sodium chloride solution and dried to obtain intermediate 1.

[0046] (3) 0.1 mol of intermediate 1 and 0.15 mol of 4-chloro-1-butanol were added to 100 mL of acetonitrile solvent, stirred and dispersed, heated to 70° C., and reacted for 24 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with ethanol, and dried to obtain a furan quaternary ammonium salt intermediate.

[0047] (4) 60 mmol of the phosphorus-containing bismaleimide intermediate was added to 100 mL of tetrahydrofuran solvent and dispersed by stirring. Then, 150 mmol of the furan-containing quaternary ammonium salt intermediate was added thereto and stirred for reaction at 65° C. for 24 h. After the reaction was completed, the mixture was washed with ethyl acetate and dried to obtain a modified quaternary ammonium salt diol intermediate.

[0048] (5) Under nitrogen conditions, 22 g of isophorone diisocyanate, 5 g of a modified quaternary ammonium salt diol intermediate, and 0.2% of dibutyltin dilaurate were added to 50 g of a polycarbonate diol, and the mixture was dispersed with stirring. The mixture was reacted at 90° C. for 2 h, and then 4 g of dimethylolpropionic acid and 2 g of hydroquinone were added thereto and the reaction was continued for 3 h. After the reaction was completed, 4 mL of triethylamine was added thereto for neutralization, and then 180 g of deionized water was added thereto and the mixture was dispersed with stirring to obtain a modified polyurethane emulsion.

[0049] (6) The tinplate sheet was polished with 8000-mesh sandpaper, washed with deionized water, and dried. The modified polyurethane emulsion was coated on the tinplate sheet and dried in an oven at 80° C. for 25 h to obtain a self-repairing modified polyurethane coating for car covers.

[0050] Example 4

[0051] (1) 0.22 mol of N-(4-hydroxyphenyl)maleimide and 0.25 mol of triethylamine were added to 100 mL of tetrahydrofuran solvent, stirred and dispersed, and then 0.1 mol of phenylphosphoryl dichloride was added thereto. The mixture was reacted at 65° C. for 24 h. After the reaction was completed, the mixture was filtered, rotary evaporated, washed with deionized water, and dried to obtain a phosphorus-containing bismaleimide intermediate.

[0052] (2) 40 mmol of N,N-bis(3-aminopropyl)-2-furanmethylamine and 100 mmol of α-lipoic acid were added to 100 mL of tetrahydrofuran solvent and dispersed by stirring. Then, 140 mmol of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 12 mmol of 4-dimethylaminopyridine were added thereto. The mixture was stirred at 20° C. for 24 h. After the reaction was completed, the mixture was washed with saturated sodium chloride solution and dried to obtain intermediate 1.

[0053] (3) 0.1 mol of intermediate 1 and 0.1 mol of 4-chloro-1-butanol were added to 100 mL of acetonitrile solvent, stirred and dispersed, heated to 60° C., and reacted for 12 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with ethanol, and dried to obtain a furan quaternary ammonium salt intermediate.

[0054] (4) 60 mmol of the phosphorus-containing bismaleimide intermediate was added to 100 mL of tetrahydrofuran solvent and stirred for dispersion. Then, 150 mmol of the furan-containing quaternary ammonium salt intermediate was added thereto. The mixture was stirred for reaction at 65° C. for 38 h. After the reaction was completed, the mixture was washed with ethyl acetate and dried to obtain a modified quaternary ammonium salt diol intermediate.

[0055] (5) Under nitrogen conditions, 24 g of isophorone diisocyanate, 6 g of a modified quaternary ammonium salt diol intermediate, and 0.1% of dibutyltin dilaurate were added to 50 g of a polycarbonate diol, and the mixture was dispersed with stirring. The mixture was reacted at 85° C. for 3 h, and then 3 g of dimethylolpropionic acid and 2 g of hydroquinone were added thereto and the reaction was continued for 4 h. After the reaction was completed, 4 mL of triethylamine was added thereto for neutralization, and then 180 g of deionized water was added thereto and the mixture was dispersed with stirring to obtain a modified polyurethane emulsion.

[0056] (6) The tinplate sheet was polished with 8000-mesh sandpaper, washed with deionized water, and dried. The modified polyurethane emulsion was coated on the tinplate sheet and dried in an oven at 80° C. for 24 h to obtain a self-repairing modified polyurethane coating for car covers.

[0057] Example 5

[0058] (1) 0.22 mol of N-(4-hydroxyphenyl)maleimide and 0.25 mol of triethylamine were added to 100 mL of tetrahydrofuran solvent, stirred and dispersed, and then 0.1 mol of phenylphosphoryl dichloride was added thereto. The mixture was reacted at 65° C. for 24 h. After the reaction was completed, the mixture was filtered, rotary evaporated, washed with deionized water, and dried to obtain a phosphorus-containing bismaleimide intermediate.

[0059] (2) 40 mmol of N,N-bis(3-aminopropyl)-2-furanmethylamine and 150 mmol of α-lipoic acid were added to 100 mL of tetrahydrofuran solvent and dispersed by stirring. Then, 120 mmol of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 4 mmol of 4-dimethylaminopyridine were added thereto. The mixture was stirred at 35° C. for 12 h. After the reaction was completed, the mixture was washed with saturated sodium chloride solution and dried to obtain intermediate 1.

[0060] (3) 0.1 mol of intermediate 1 and 0.12 mol of 4-chloro-1-butanol were added to 100 mL of acetonitrile solvent, stirred and dispersed, heated to 65° C., and reacted for 24 h. After the reaction was completed, the mixture was distilled under reduced pressure, washed with ethanol, and dried to obtain a furan quaternary ammonium salt intermediate.

[0061] (4) 60 mmol of the phosphorus-containing bismaleimide intermediate was added to 100 mL of tetrahydrofuran solvent and dispersed by stirring. Then, 150 mmol of the furan-containing quaternary ammonium salt intermediate was added thereto and stirred for reaction at 65° C. for 24 h. After the reaction was completed, the mixture was washed with ethyl acetate and dried to obtain a modified quaternary ammonium salt diol intermediate.

[0062] (5) Under nitrogen conditions, 25 g of isophorone diisocyanate, 7.5 g of a modified quaternary ammonium salt diol intermediate, and 0.2% of dibutyltin dilaurate were added to 50 g of a polycarbonate diol, and the mixture was dispersed with stirring. The mixture was reacted at 85° C. for 3.5 h, and then 3 g of dimethylolpropionic acid and 2 g of hydroquinone were added thereto and the reaction was continued for 4 h. After the reaction was completed, 4 mL of triethylamine was added thereto for neutralization, and then 180 g of deionized water was added thereto and the mixture was dispersed with stirring to obtain a modified polyurethane emulsion.

[0063] (6) The tinplate sheet was polished with 8000-mesh sandpaper, washed with deionized water, and dried. The modified polyurethane emulsion was coated on the tinplate sheet and dried in an oven at 80° C. for 30 h to obtain a self-repairing modified polyurethane coating for car covers.

[0064] Comparative Example 1

[0065] The difference between this comparative example and Example 1 is that in step (5), butanediol is used instead of the modified quaternary ammonium salt diol intermediate.

[0066] Refer to GB / T2406-2009 and use an oxygen index meter to test the limiting oxygen index of the polyurethane coating.

[0067] Table 1: Limiting oxygen index of each embodiment and comparative example

[0068] LOI / % Example 1 26.8 Example 2 28.3 Example 3 28.9 Example 4 29.5 Example 5 30.0 Comparative Example 1 18.5

[0069] It can be seen from the table that the polyurethane coating prepared by the present invention has good flame retardant properties.

[0070] Refer to HG / T3950-2007, using Escherichia coli as the test microorganism

[0071] Table 2: Antibacterial performance test of each embodiment and comparative example

[0072] Antibacterial rate / % Example 1 76.85 Example 2 85.62 Example 3 90.90 Example 4 92.78 Example 5 97.99 Comparative Example 1 52.48

[0073] It can be seen from the table that the polyurethane coating prepared by the present invention has good antibacterial properties.

[0074] A scratch was made on the coating surface with a tool, and the cross-sectional area of ​​the scratch notch was measured using a 3D surface topography profile at 50°C and a UV intensity of 0.83 W / m 2After 12 hours of treatment, the repaired cross-sectional area was measured again to calculate the self-repairing efficiency. Self-repairing efficiency (%) = repaired scratch cross-sectional area / original scratch cross-sectional area.

[0075] Table 3: Self-repairing performance test of each embodiment and comparative example

[0076] Self-repair efficiency / % Example 1 56.8 Example 2 69.0 Example 3 82.9 Example 4 90.3 Example 5 94.7 Comparative Example 1 30.4

[0077] It can be seen from the table that the polyurethane coating prepared by the present invention has relatively excellent self-repairing performance.

[0078] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a self-repairing modified polyurethane coating for car covers, It is characterized in that The preparation method is: (1) under nitrogen conditions, isophorone diisocyanate, a modified quaternary ammonium salt diol intermediate, and 0.1-0.3% of dibutyltin dilaurate are added to polycarbonate diol, stirred and dispersed, reacted at 80-90° C. for 2-4 hours, and then dimethylolpropionic acid and hydroquinone are added thereto to continue the reaction for 3-8 hours. After the reaction is completed, triethylamine is added thereto for neutralization, and then deionized water is added thereto, stirred and dispersed to obtain a modified polyurethane emulsion, wherein the amount ratio of isophorone diisocyanate, modified quaternary ammonium salt diol intermediate, polycarbonate diol, dimethylolpropionic acid, hydroquinone, and triethylamine is (40-70) g:(5-15) g:100 g:(5-8) g:(2-8) g:(5-10) mL; (2) grinding the tinplate sheet with 8000-mesh sandpaper, washing with deionized water, and drying, coating the modified polyurethane emulsion on the tinplate sheet, and drying in an oven at 80° C. for 24-30 hours to obtain a self-repairing modified polyurethane coating for car covers; The preparation method of the modified quaternary ammonium salt diol intermediate is as follows: S1, adding N-(4-hydroxyphenyl)maleimide and triethylamine to tetrahydrofuran solvent, stirring and dispersing, then adding phenylphosphoryl dichloride thereto, reacting at 60-70° C. for 20-48 hours, filtering, rotary evaporating, washing with deionized water, and drying to obtain a phosphorus-containing bismaleimide intermediate; S2, adding N,N-di(3-aminopropyl)-2-furanmethylamine and α-lipoic acid to tetrahydrofuran solvent, stirring and dispersing, then adding 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 4-dimethylaminopyridine thereto, stirring and reacting at 20-35° C. for 12-24 hours, after the reaction is completed, washing with saturated sodium chloride solution, and drying to obtain intermediate 1; S3, adding the intermediate 1, 4-chloro-1-butanol to acetonitrile solvent, stirring and dispersing, heating to 60-70°C, reacting for 12-24h, and after the reaction, distilling under reduced pressure, washing with ethanol, and drying to obtain a furan quaternary ammonium salt intermediate; S4. Add the phosphorus-containing bismaleimide intermediate to tetrahydrofuran solvent, stir and disperse, then add the furan-containing quaternary ammonium salt intermediate thereto, stir and react at 60-70° C. for 24-48 hours. After the reaction is completed, wash with ethyl acetate and dry to obtain a modified quaternary ammonium salt diol intermediate.

2. The method for preparing the self-repairing modified polyurethane coating for car cover according to claim 1, It is characterized in that In step S1, the molar ratio of N-(4-hydroxyphenyl)maleimide, triethylamine and phenylphosphoryl dichloride is 2-2.4:2.2-2.8:

1.

3. The method for preparing the self-repairing modified polyurethane coating for car cover according to claim 1, It is characterized in that In step S2, the molar ratio of N,N-di(3-aminopropyl)-2-furanmethylamine, α-lipoic acid, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, and 4-dimethylaminopyridine is 1:2.5-4:3-3.5:0.1-0.

3.

4. The method for preparing the self-repairing modified polyurethane coating for car cover according to claim 1, It is characterized in that In step S3, the molar ratio of the intermediate 1 and 4-chloro-1-butanol is 1:1-1.

5.

5. The method for preparing the self-repairing modified polyurethane coating for car cover according to claim 1, It is characterized in that In step S4, the molar ratio of the phosphorus-containing bismaleimide intermediate to the furanic quaternary ammonium salt intermediate is 1:2-3.

Citation Information

Patent Citations

  • Self-repairing antibacterial polyurethane coating and preparation method thereof

    CN113789114A

  • Preparation method for UV-curing self-healing polyurethane based on furan-maleimide structure

    CN105348474A

  • Antibacterial mould-proof waterborne quaternary ammonium salt / polyurethane finishing material

    CN105694703A

  • Antibacterial polyester polyol, preparation method thereof and antibacterial polyurethane

    CN112592470A

  • Diquaternary ammonium salt-containing diol, preparation method thereof and application of diquaternary ammonium salt-containing diol in antibacterial self-extinction waterborne polyurethane coating

    CN114409553A