A 560MPa grade cold stamping steel for automobile axle housing and its production method
By adjusting chemical composition and production process, the yield strength and tensile strength of the steel for automotive axle shells for 560MPa grade cold stamping is improved, and the problem of low elongation is solved, and excellent molding performance and cold stamping effect are achieved, which meets the Demand for driving axle shells for load-loaded vehicles.
Patent Information
- Application Number
- CN202411124968.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-16
AI Technical Summary
The existing 560MPa-grade cold stamping car axle shell has a low elongation, which leads to its unsatisfactory molding performance and cold stamping effect, which cannot meet the needs of the load-loaded vehicle drive axle shell.
By adjusting the chemical composition and production process of the steel plate, the chemical composition of the steel plate is C: 0.095%~0.183%, Si: 0.25%~0.45%, Mn: 1.65%~2.25%, etc., and the structure is ferrite and martensite. , residual austenite and bainite, and adopt RH+LF smelting, heating, rolling and cooling processes, including laminar cooling + ultra-fast cooling cooling mode to improve the yield strength, tensile strength and transverse direction of the steel plate. Longitudinal impact power.
The yield strength of the steel plate is ≥560MPa, tensile strength ≥675MPa, transverse elongation A50≥36%, lateral impact power of -40℃ ≥222J, longitudinal impact power of -40℃ ≥256J, and transverse cold bend 180°D= a qualified, significantly improving the forming performance and mechanical properties.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal materials, and in particular relates to a 560MPa grade cold stamping automobile bridge housing steel and a production method thereof. The steel plate of the invention is mainly suitable for manufacturing cold stamping automobile bridge housing steel. Background Art
[0002] The automobile axle housing is one of the main components of the automobile driving system. It supports the weight of the frame and the assemblies at the rear of the frame, and protects the components of the transmission system. In the manufacturing field of the axle housing industry, there are two completely different product manufacturing methods: stamping and welding axle housings and casting axle housings. With the development of axle housing manufacturing technology and the need to reduce automobile weight and energy, especially for the axle housing driven by a truck, 12~16mm thick hot-rolled steel plates have been used to make stamping and welding axle housings, replacing the casting axle housings with complex manufacturing processes, low production efficiency, heavy weight and high cost.
[0003] The Chinese patent application with application number 202210450179.5 discloses a 600MPa grade automobile bridge housing steel for hot stamping and a production method thereof, wherein the chemical composition is C0.240% to 0.335%, Si0.08% to 0.65%, Mn1.75% to 2.25%, Al0.010% to 0.065%, Nb0.046% to 0.085%, Ti0.052%~0.102%, V0.054%~0.102%, Cr0.10%~0.46%, Mo0.12%~0.26%, B0.0014%~0.0035%, La+Ce0.033%~0.042%, Ca0.0014%~0.0050%, P≤0.010%, S≤0.005%, N≤0.003%. Steel plate yield strength ≥600MPa, tensile strength ≥780MPa, transverse elongation A 50 ≥28%. This bridge housing steel can only be used for the production of hot stamping parts, not for the production of cold stamping parts.
[0004] The Chinese patent application with application number 202010623646.0 discloses a 620MPa-grade cold-stamped steel plate for automobile axle housing and a preparation method thereof, wherein the chemical composition of the steel plate is formulated according to the following mass fractions: C≤0.10%, Si≤0.45%, Mn≤1.60%, P≤0.010%, S≤0.005%, V≤0.060%, Nb≤0.060%, Als≤0.035%, and the remainder is Fe. The present invention improves the strength and comprehensive performance indicators of the axle housing manufacturing material, with a yield strength of ≥520MPa, a tensile strength of ≥620MPa, and an elongation of ≥23%. The steel plate has a high strength, but an elongation of only 23%. Its elongation and forming properties are both low, and the cold stamping effect is not ideal. Summary of the invention
[0005] The purpose of the present invention is to provide a 560MPa grade cold stamping automobile bridge housing steel and a production method thereof. In view of the development needs of the automobile steel field, the 560MPa grade cold stamping automobile bridge housing steel of the present invention has a yield strength of ≥560MPa, a tensile strength of ≥675MPa, and a transverse elongation A 50 ≥36%, -40℃ transverse impact energy ≥222J, -40℃ longitudinal impact energy ≥256J, and transverse cold bending 180°D=a is qualified.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A 560MPa grade cold stamping automobile bridge housing steel, the chemical composition of the steel is as follows by weight percentage: C: 0.095%-0.183%, Si: 0.25%-0.45%, Mn: 1.65%-2.25%, Al: 0.35%-0.55%, Nb: 0.020%-0.130%, V: 0.025%-0.110%, Ti: 0.025%-0.045%, Cr: 0.02%-0. 54%, W: 0.025% ~ 0.210%, Ni: 0.08% ~ 0.22%, Cu: 0.21% ~ 0.51%, rare earth elements (La + Ce): 0.010% ~ 0.018%, Ca: 0.0011% ~ 0.0030%, Mg: 0.0015% ~ 0.1150%, and limit P ≤ 0.012%, S ≤ 0.005%, N ≤ 0.002%, the balance is Fe and unavoidable impurities.
[0008] The structure of the steel is as follows: ferrite accounts for 25% to 50% by volume, martensite accounts for 30% to 60% by volume, retained austenite accounts for 4% to 12% by volume, and bainite accounts for 4% to 13% by volume.
[0009] Steel plate yield strength ≥560MPa, tensile strength ≥675MPa, transverse elongation A 50 ≥36%, -40℃ transverse impact energy ≥222J, -40℃ longitudinal impact energy ≥256J, and transverse cold bending 180°D=a qualified hot-rolled plate.
[0010] The main functions of the components of the 560MPa grade cold stamping automobile axle housing steel in the present invention are:
[0011] C: Carbon ensures the strength of the steel plate through solid solution strengthening and is also used to expand the austenite zone. Free carbon can have a good stabilizing effect on austenite, thereby improving the formability of the steel plate. It is also the most economical element to improve the strength of the material. If the carbon content is too low, the mechanical properties of the steel plate in the present invention cannot be obtained. If the content is too high, the steel plate will become brittle and there is a risk of delayed fracture. It is also unfavorable to the welding performance, plasticity and toughness of the steel plate. Therefore, the optimal range of carbon in the present invention is 0.095% to 0.183%.
[0012] Si: Silicon is a solid solution strengthening element, which can improve the strength of the steel plate by solid solution strengthening in ferrite. At the same time, it can also inhibit the decomposition of residual austenite and the precipitation of carbides, reduce inclusions in steel, and also has the effect of improving the hardenability of the steel plate. However, if the silicon content is too low, it will not have a strengthening effect, and if the content is too high, it will affect the hot rolling surface quality, and a large amount of iron oxide scale and welding performance will appear. Therefore, the silicon content in the present invention is 0.25% to 0.45%.
[0013] Mn: Manganese can form substitutional solid solution in steel, play a strong role in solid solution strengthening, and is also an austenite stabilizing element in steel, expanding the austenite zone, reducing the critical quenching speed of steel, and can also refine the grains, so that the yield strength and tensile strength increase linearly. The content of this element increases the strength of steel within a certain range while hardly reducing the plasticity and toughness of steel, and can also improve the hardenability of steel. However, if the manganese content is too low, the supercooled austenite is unstable, and the processing properties such as plasticity and toughness of the steel plate are reduced. If the manganese content is too high, the welding performance of the steel plate will deteriorate, and the production cost will increase. At the same time, the carbon equivalent of the steel will also increase, and the uniformity of the steel plate organization will deteriorate during the smelting and hot rolling process, which is easy to cause serious banded structure defects in the organization. Therefore, the manganese content is selected to be 1.65% to 2.25%.
[0014] P: Phosphorus can increase the formation temperature of the α phase and expand the temperature range of the α phase. However, excessive phosphorus content will deteriorate the workability of the steel plate and have an adverse effect on plasticity, toughness and fatigue properties. In order to obtain a higher elongation, the upper limit is set at 0.012%.
[0015] S: Sulfur forms sulfide inclusions such as MnS, which become the starting point of cracks and deteriorate the processing performance, seriously affecting the formability of the steel sheet. Therefore, the lower the content, the better, and its upper limit is set to 0.005%.
[0016] Al: Al is a commonly used deoxidizer in steel. It plays a role in deoxidation and nitrogen determination during the smelting process, and can effectively improve the anti-oxidation performance of the steel plate. It can also inhibit the decomposition of residual austenite and the precipitation of carbides. However, too much aluminum will lead to a large number of aluminum inclusions, increase production costs, and cause difficulties in continuous casting production. Adding a certain amount of Al to steel can form AlN precipitation, which plays a certain role in refining grains, thereby improving the toughness and plasticity of the steel plate. Therefore, in the present invention, the Al content is limited to 0.35% to 0.55%.
[0017] Nb: Niobium plays a major role in steel fine grain strengthening and precipitation strengthening. It can also expand the rolling process window, improve the uniformity of steel coil performance, and refine the structure to improve the cold forming performance of steel plates. At high temperatures, niobium exists in austenite in a solid solution state, which can inhibit the growth of austenite grains and static and dynamic recrystallization during thermal deformation, and increase the recrystallization termination temperature, which can increase the final rolling temperature; at the same time, the precipitation of niobium carbonitride can also delay recrystallization and prevent the growth of austenite grains. It has obvious fine grain strengthening and precipitation strengthening effects, can effectively reduce the grade of banded structure of steel plates, and improve impact performance. Therefore, the optimal range of Nb content in the present invention is between 0.020% and 0.130%.
[0018] V: Vanadium has significant precipitation strengthening and fine grain strengthening effects. The effect of vanadium is mainly achieved by forming precipitates with carbon and nitrogen. In particular, the VN precipitation formed with nitrogen can greatly improve the strength of the steel plate. In addition, the addition of V can also be combined with H to improve the delayed fracture resistance of the steel plate. When the V content is high, the low-temperature toughness of the steel plate is significantly deteriorated, and the toughness of the welding heat affected zone is also deteriorated. Therefore, the V addition amount in the present invention is 0.025% to 0.110%.
[0019] Ti: Titanium can effectively delay the recrystallization of deformed austenite, prevent the growth of austenite grains, increase the recrystallization temperature of austenite, refine the grains, and improve the strength and toughness of steel. Moreover, Ti is a strong carbon and nitride forming element, which can combine with carbon and nitrogen to form stable and fine carbon and nitride, playing a significant role in grain refinement and precipitation strengthening. Therefore, the optimal range of Ti content in the present invention is between 0.025% and 0.045%.
[0020] Cr: It is a carbide-forming element that can delay pearlite transformation and improve the hardenability of steel, thus facilitating the formation of martensite structure, and refining the structure to achieve a strengthening effect. It can also stabilize the residual austenite. Too low chromium content will affect the hardenability of steel, while too high chromium content will increase production costs and also make the processing and formability of the material worse. The principle of selecting the chromium content is to promote the formation of martensite, so the chromium content of the present invention is selected between 0.02% and 0.54%.
[0021] W: Tungsten is the metal with the highest melting point. The WC formed has high hardness. Its role in steel is similar to that of molybdenum. It is better than molybdenum in enhancing wear resistance. Tungsten can also improve the hardenability of steel and effectively inhibit grain growth. When its content is less than 0.025%, the effect is slight. When it exceeds 0.210%, the brittleness increases. Therefore, the optimal range of W content in the present invention is between 0.025% and 0.210%.
[0022] Ni: The nickel element has no adverse effect on the hardenability and toughness of the welding heat affected zone of steel, and can improve the corrosion resistance and hardenability of steel, which is beneficial to the formation of martensitic structure. Therefore, the Ni content in the steel of the present invention is selected to be 0.08% to 0.22%.
[0023] Cu: Copper can also expand the austenite phase, improve the weather resistance of steel, improve the weldability of steel, and effectively improve the corrosion resistance of steel. However, when the Cu content is high, it causes hot brittleness and deteriorates the surface performance of the steel plate. In addition, at a certain Cu content, it is beneficial to the strength and hot workability of the steel plate, effectively reduces the hot rolling edge crack tendency of the steel plate, and significantly improves the surface quality of the steel plate. Cu also has the effect of reducing work hardening and improving the plasticity of the steel plate. Therefore, the copper content of the present invention is selected to be 0.21% to 0.51%.
[0024] Rare earth elements (La+Ce): Rare earth has strong deoxidation and desulfurization capabilities. The spherical sulfides or sulfur oxides formed replace the long strip manganese sulfide inclusions, which can improve the plasticity and anisotropy of the steel plate. Rare earth can improve the fatigue performance of the steel plate and improve the welding performance of the steel plate. Rare earth has a strong affinity with other impurity elements in steel, which can reduce the content of sulfur, oxygen, phosphorus, hydrogen and other elements in the steel and eliminate their harmful effects. Therefore, the present invention limits the rare earth (La+Ce) content to 0.010% to 0.018%.
[0025] Ca: Calcium can change the morphology of steel sulfide (MnS), prevent the formation of long strips of MnS inclusions, and improve the plasticity, toughness and fatigue properties of the steel plate. Therefore, the present invention controls the Ca content to 0.0011% to 0.0030%.
[0026] Mg: Magnesium is a good deoxidizer, desulfurizer and spheroidizer in steel. Magnesium can reduce the number of inclusions in steel, reduce their size, make their distribution uniform and improve their morphology. A trace amount of magnesium can improve the size and distribution of carbides in steel and promote the fine and uniform carbide particles. Therefore, the present invention controls the Mg content to 0.0015% to 0.1150%.
[0027] N: As for the N content in steel, the lower the N content, the better. However, too low a content will lead to production difficulties and increase costs. Therefore, in the present invention, the N content is ≤0.002%.
[0028] A method for preparing 560MPa grade cold stamping steel for automobile axle housing, comprising smelting, heating, rolling and cooling, specifically comprising:
[0029] 1) Smelting: RH+LF process is adopted, H and O contents are strictly controlled, H≤0.0002%, O≤0.0015%, calcium treatment is carried out in the refining process, electromagnetic stirring and light pressure reduction technology are used in the continuous casting process, and the billet pulling speed is ≤1.1m / min.
[0030] 2) Heating: Directly heat the continuous casting slab with a thickness of (160-240) mm and a width of (1450-2030) mm and heat it in a walking beam heating furnace. The heating temperature is 1300-1330°C and the holding time is 182-210 minutes. The furnace pressure is always controlled in a slightly positive pressure state in the dynamic state, and the positive pressure value is controlled at 3-15 Pa to reduce oxidation and burning. Appropriate heating temperature and appropriate holding time can make the alloy elements in the slab completely dissolved, the slab composition is uniform, and play a role in controlling the original austenite grain size.
[0031] 3) Rolling and cooling: The rough rolling adopts the rolling process of 3+3 mode (R1 adopts 3 rolling passes, R2 adopts 3 rolling passes), a total of 6 rolling passes, the rough rolling outlet temperature is 1125~1180℃, the intermediate billet thickness is 44~65mm, and the width is 1450~2030mm. The intermediate billet is insulated with a heat preservation cover before entering the hot rolling and finishing mill to reduce the temperature drop of the intermediate billet on the delayed roller and the temperature difference between the head, tail and plate width directions. The finishing rolling is 7-stand continuous rolling, high-pressure water descaling before finishing rolling, the finishing rolling inlet temperature is not higher than 1125℃, the final rolling temperature is 750~865℃, and the laminar cooling + ultra-fast cooling cooling mode is adopted after final rolling. The laminar cooling rate is about 15~25℃ / s. After cooling to 650~745℃, ultra-fast cooling is carried out, and the cooling rate is ≥162℃ / s. The steel plate is cooled to 305~405℃ and then coiled. The laminar cooling to 650-745℃ aims to make ferrite precipitate quickly, while suppressing grain growth, the ferrite content is guaranteed, so that the ferrite grains are refined. The ultra-fast cooling to 305-405℃ aims to make martensite precipitate quickly and in large quantities, while suppressing grain growth, the martensite content is guaranteed, so that the martensite grains are refined. The convexity control accuracy of the steel plate is ±40μm, the flatness is controlled within 18I, the thickness control accuracy is ±40μm, the finished product thickness is 5-18mm, and the thickness tolerance is controlled within ±0.1mm.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] 1) The addition of Cr can improve the strength and toughness of the steel plate, delay the pearlite transformation, and improve the hardenability of the steel, which is beneficial to the formation of martensite structure, refine the structure, strengthen it, and stabilize the retained austenite.
[0034] 2) The WC formed by W has high hardness, enhances wear resistance, improves the hardenability of steel, and effectively inhibits grain growth.
[0035] 3) Ni can improve the corrosion resistance and hardenability of steel, and is beneficial to the formation of martensitic structure.
[0036] 4) Cu can improve the weather resistance and weldability of steel, and can also effectively improve the corrosion resistance of steel. At a certain Cu content, it is beneficial to the strength and hot workability of the steel plate, effectively reduces the tendency of hot rolling edge cracking of the steel plate, and significantly improves the surface quality of the steel plate. Cu also has the effect of reducing work hardening and improving the plasticity of the steel plate.
[0037] 5) Rare earth elements (La+Ce) have strong deoxidation and desulfurization capabilities. The spherical sulfides or sulfur oxides formed replace the long strip-shaped manganese sulfide inclusions, which can improve the plasticity and anisotropy of the steel plate. Rare earths can improve the fatigue performance of the steel plate and improve the welding performance of the steel plate.
[0038] 6) The addition of Ca can change the morphology of steel sulfides and improve the plasticity, toughness and fatigue properties of the steel plate.
[0039] 7) The addition of Mg can reduce the number of inclusions in steel, reduce their size, make their distribution uniform, and improve their morphology. A trace amount of magnesium can improve the size and distribution of carbides in steel and promote the fine and uniform carbide particles.
[0040] 8) After rolling, the cooling mode of laminar cooling + ultra-fast cooling is adopted to obtain the various phase structures at different cooling stages.
[0041] 9) The microstructure of the steel of the present invention is ferrite, martensite, retained austenite and bainite. Under the coupling effect of transformation induced plasticity (TRIP) effect and coordinated deformation of the mixed microstructure of martensite and bainite, the formability of the steel plate is significantly improved during the forming process.
[0042] 10) The present invention has excellent mechanical properties, yield strength ≥560MPa, tensile strength ≥675MPa, transverse elongation A50 ≥36%, -40℃ transverse impact energy ≥222J, -40℃ longitudinal impact energy ≥256J, and transverse cold bending 180°D=a is qualified. DETAILED DESCRIPTION
[0043] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the specific implementation methods of the present invention are further described below in conjunction with examples. The following examples are used to specifically illustrate the contents of the present invention. These examples are only general descriptions of the contents of the present invention and do not limit the contents of the present invention.
[0044] The main process of the present invention is as follows:
[0045] The continuous casting slab with a thickness of (160-240) mm and a width of (1450-2030) mm is directly hot-transferred and hot-charged into a step-beam heating furnace for heating at a temperature of 1300-1330°C and a holding time of 182-210 min. The furnace pressure is always controlled in a slightly positive pressure state in the dynamic state, and the positive pressure value is controlled at 3-15 Pa to reduce oxidation and burning. The rough rolling adopts a 3+3 mode rolling process (R1 adopts 3 passes and R2 adopts 3 passes), with a total of 6 passes. The rough rolling outlet temperature is 1125-1180°C, the intermediate billet thickness is 44-65 mm, and the width is 1450-2030 mm. The intermediate billet is kept warm by a heat preservation cover before entering the hot rolling and finishing mill to reduce the temperature drop of the intermediate billet on the delayed roller and the temperature difference between the head and tail and the plate width direction. The finishing rolling is a 7-stand continuous rolling, and high-pressure water is used for descaling before finishing rolling. The finishing rolling inlet temperature is not higher than 1125°C The final rolling temperature is 750-865°C. After the final rolling, the cooling mode of laminar cooling + ultra-fast cooling is adopted. The laminar cooling rate is about 15-25°C / s. After cooling to 650-745°C, ultra-fast cooling is carried out. The cooling rate is ≥162°C / s. The steel plate is cooled to 305-405°C and then coiled. The convexity control accuracy of the steel plate is ±40μm, the flatness is controlled within 18I, the thickness control accuracy is ±40μm, the finished product thickness is 5-18mm, and the thickness tolerance is controlled within ±0.1mm.
[0046] The specific composition, hot rolling process system, steel plate properties and tissue volume percentage of the six embodiments of the present invention are shown in Tables 1-4.
[0047] Table 1 Chemical composition of the examples of the present invention (wt, %)
[0048]
[0049] Table 2 Hot rolling process system of the embodiment of the present invention
[0050] serial number Continuous casting billet specifications / mm Billet drawing speed / m / min Heating temperature / ℃ Insulation time / min Heating furnace pressure / Pa Rough rolling outlet temperature / ℃ Intermediate billet specifications / mm Finishing rolling inlet temperature / ℃ Final rolling temperature / ℃ Laminar cooling temperature / ℃ Laminar cooling rate ℃ / s Coiling temperature / ℃ Ultra-fast cooling rate ℃ / s Example 1 160×1450 1.1 1310 189 3 1125 44×1450 1080 865 745 15 405 162 Example 2 195×1510 1.0 1300 190 5 1130 50×1510 1093 842 726 18 388 165 Example 3 200×1530 1.0 1320 183 10 1145 65×1530 1120 833 692 19 365 171 Example 4 215×1650 1.05 1315 200 9 1152 60×1650 1125 815 663 21 342 174 Example 5 220×1970 0.9 1325 182 7 1175 55×1970 1108 782 658 23 319 182 Example 6 240×2030 1.1 1330 210 15 1180 52×2030 1115 750 650 25 305 184
[0051] Table 3 Mechanical properties parameters of the embodiments of the present invention
[0052] serial number Steel plate thickness / mm Thickness control accuracy / μm Convexity control accuracy / μm Straightness Yield strength / MPa Tensile strength / MPa Transverse elongation (A50) / % Transverse impact value (-40℃) / J Longitudinal impact value (-40℃) / J Cold bending test 180° (horizontal) Example 1 5 +30 -40 18I 620 739 36.5 235 270 D=a qualified Example 2 10 -20 +30 17I 615 725 37.3 234 269 D=a qualified Example 3 6 -10 +10 15I 611 713 39.5 232 266 D=a qualified Example 4 12 +10 +25 16I 584 701 39.8 230 264 D=a qualified Example 5 15 +40 -5 18I 572 687 40.1 226 261 D=a qualified Example 6 18 -15 -10 14I 560 675 41.6 222 256 D=a qualified
[0053] Table 4 Tissue volume percentage in the embodiments of the present invention
[0054] serial number Ferrite Martensite Retained austenite bainite Example 1 25.8% 60.0% 7.1% 7.1% Example 2 39.8% 36.7% 10.5% 13.0% Example 3 50.0% 35.6% 4.3% 10.1% Example 4 34.8% 50.0% 4.0% 11.2% Example 5 27.5% 47.5% 12.0% 13.0% Example 6 39.7% 45.2% 6.6% 8.5%
[0055] In order to describe the present invention, the present invention is appropriately and fully illustrated by the examples in the above. The above implementation modes are only used to illustrate the present invention, but not to limit the present invention. Ordinary technicians in the relevant technical field can make various changes and modifications without departing from the spirit and scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made should be included in the protection scope of the present invention. The patent protection scope of the present invention should be defined by the claims.
Claims
1. A 560MPa grade cold stamping automobile axle housing steel, characterized in that: The chemical composition of the steel is calculated by weight percentage: C 0.095%~0.183%, Si 0.25%~0.45%, Mn 1.65%~2.25%, Al 0.35%~0.55%, Nb 0.045%~0.130%, V 0.068%~0.110%, Ti 0.025%~0.045%, Cr 0.33%~0.54%, W 0.025%~0.210%, Ni 0.08%~0.22%, Cu 0.21%~0.51%, rare earth elements 0.010%~0.018%, Ca 0.0011%~0.0030%, Mg0.0015%~0.1150%, and limited P≤0.012%, S≤0.005%, N≤0.002%, the balance is Fe and unavoidable impurities; Steel plate yield strength ≥560MPa, tensile strength ≥675MPa, transverse elongation A 50 ≥36%, -40℃ transverse impact energy ≥222J, -40℃ longitudinal impact energy ≥256J, and transverse cold bending 180°D=a is qualified; The thickness of the finished steel plate is 5 to 18 mm; A method for preparing 560MPa grade cold stamping steel for automobile axle housing, comprising smelting, heating, rolling and cooling, specifically comprising: 1) Heating: The continuous casting slab is hot-transferred and hot-charged into the heating furnace for heating at a temperature of 1300-1330°C and a holding time of 182-210 minutes; 2) Rolling and cooling: The outlet temperature of rough rolling is 1125-1175°C, the inlet temperature of finishing rolling is not higher than 1125°C, the final rolling temperature is 750-865°C, and the cooling mode of laminar cooling + ultra-fast cooling is adopted after final rolling. The laminar cooling rate is 15-25°C / s. After cooling to 650-745°C, ultra-fast cooling is carried out, and the cooling rate is ≥162°C / s. The steel plate is cooled to 305-405°C and then coiled.
2. The 560MPa grade cold stamping automobile axle housing steel according to claim 1, characterized in that: The structure of the steel is as follows: ferrite accounts for 25% to 50% by volume, martensite accounts for 30% to 60% by volume, retained austenite accounts for 4% to 12% by volume, and bainite accounts for 4% to 13% by volume.
3. A method for preparing 560MPa grade cold stamping automobile bridge housing steel as claimed in claim 1 or 2, comprising smelting, heating, rolling and cooling, characterized in that: Specifically include: 1) Heating: The continuous casting slab is hot-transferred and hot-charged into the heating furnace for heating at a temperature of 1300-1330°C and a holding time of 182-210 minutes; 2) Rolling and cooling: The outlet temperature of rough rolling is 1125-1175°C, the inlet temperature of finishing rolling is not higher than 1125°C, the final rolling temperature is 750-865°C, and the cooling mode of laminar cooling + ultra-fast cooling is adopted after final rolling. The laminar cooling rate is 15-25°C / s. After cooling to 650-745°C, ultra-fast cooling is carried out, and the cooling rate is ≥162°C / s. The steel plate is cooled to 305-405°C and then coiled.
4. The method for preparing a 560MPa grade cold stamping automobile axle housing steel according to claim 3, characterized in that: The continuous casting slab has a size of (160-240) mm thick×(1450-2030) mm wide.
5. The method for preparing a 560MPa grade cold stamping automobile axle housing steel according to claim 3, characterized in that: The furnace pressure of the heating furnace is always controlled in a slightly positive pressure state in the dynamic state, and the positive pressure value is controlled in a range of 3 to 15 Pa.
6. The method for preparing a 560MPa grade cold stamping automobile axle housing steel according to claim 3, characterized in that: The intermediate billet before finish rolling and after rough rolling has a thickness of 44-65 mm and a width of 1450-2030 mm.
7. The method for preparing a 560MPa grade cold stamping automobile axle housing steel according to claim 3 or 6, characterized in that: The intermediate billet after rough rolling is kept warm by a heat preservation cover before entering the hot rolling and finishing mill, and is descaled by high-pressure water before finishing rolling.
8. The method for preparing a 560MPa grade cold stamping automobile axle housing steel according to claim 3, characterized in that: The convexity control accuracy of the steel plate is ±40μm, the flatness is controlled within 18I, and the thickness control accuracy is ±40μm.