A production method for corrosion-resistant and high-efficiency non-oriented silicon steel
Through alloy composition design and process control, a variety of beneficial elements are added, the corrosion resistance and electromagnetic performance problems of non-oriented silicon steel in corrosion environments are solved, and the high-efficiency corrosion resistance and electromagnetic performance are improved, which meets the efficiency of motor manufacturing. need.
Patent Information
- Application Number
- CN202411124981.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-16
AI Technical Summary
Existing non-oriented silicon steels are prone to damage in corrosion environments and are difficult to meet the requirements of efficient corrosion resistance and electromagnetic performance. Especially in the context of low-carbon green development, motors are developing towards efficient high power density, and more corrosion-resistant materials are needed.
Through alloy composition design and process control, a variety of beneficial elements such as lanthanide rare earths, copper, phosphorus and boron are added to control the alloy composition and process conditions to produce non-oriented silicon steel with excellent electromagnetic properties and corrosion resistance, including Si: 0.5% ~3.35%, Al: 0.25% to 1.5%, Mn: 0.15% to 1.0%, La: 0.06% to 0.15%, Cu: 0.08% to 0.50%, Sn and/or Sb: 0.035% to 0.15%, P: 0.012%~0.15%, B: 0.002%~0.010%, to improve the cleanliness and corrosion resistance of steel.
It significantly improves the corrosion resistance and electromagnetic properties of silicon steel, meets the manufacturing needs of motors in special industries, and improves production efficiency and market competitiveness under the original alloy conditions.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cold-rolled non-oriented silicon steel production, and in particular to a production method of corrosion-resistant and high-efficiency non-oriented silicon steel. Background Art
[0002] Cold-rolled non-oriented silicon steel is an important metallic soft magnetic material, widely used in the manufacture of iron cores of various motors, and is a functional carrier for the conversion of electromagnetic and mechanical energy. As various industries develop towards automation, electrification, and intelligence, various functional motors are developing rapidly, driving the improvement of the functionality of non-oriented silicon steel materials.
[0003] In the context of low-carbon green development, it is an inevitable trend for motors to develop in the direction of high efficiency and high power density; in many application fields, new requirements are put forward for the functional characteristics of non-oriented electrical steel such as high efficiency and corrosion resistance in response to different special working conditions (silicon steel products are prone to corrosion on the surface or matrix fracture due to the silicon component). For example, some companies will gradually evolve the base and housing as motor components from cast iron and steel plate stamping to plastic sealing, until the stator core is used as the housing and base, or the stator and rotor are directly embedded in the corresponding mechanical equipment according to the working conditions; in corrosive environments such as marine engineering and oil and gas fields, in order to prevent the motor stator and rotor from rusting and losing functionality, the iron core is dipped in paint for corrosion protection, electrophoretic coating, etc. to increase its corrosion resistance; or the specific electromagnetic functionality of the motor stator and rotor is sacrificed, and high-priced "stainless steel" raw materials with magnetic properties are purchased as substitutes.
[0004] By 2023, my country's non-oriented electrical steel output and production capacity will exceed 12 million tons, and the production capacity will exceed 14 million tons, which means that my country has become a major electrical steel industry country. Faced with the severe situation of oversupply of non-oriented silicon steel, the development and production of efficient, personalized and differentiated non-oriented silicon steel products has become a means for many companies to enhance their competitiveness, and will also become one of the priority development directions of the electrical steel industry.
[0005] With the rapid development of metallurgical technology, on the basis of continuous improvement of steel cleanliness, many products have continuously improved their functionality through diverse micro-alloying or multi-element main alloy element design under the original steel composition system. Summary of the invention
[0006] The present invention provides a method for producing corrosion-resistant and high-efficiency non-oriented silicon steel. Under modern mainstream production process conditions, based on improving the cleanliness of steel and adding a variety of beneficial elements, the composite and synergistic effects of various elements are exerted to produce silicon steel products with excellent electromagnetic properties and corrosion resistance.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] A method for producing corrosion-resistant and high-efficiency non-oriented silicon steel, including alloy composition design and process control; wherein:
[0009] 1) Alloy composition design; in corrosion-resistant and high-efficiency non-oriented silicon steel, by mass percentage, including Si: 0.5% ~ 3.35%, Als: 0.25% ~ 1.5%, Mn: 0.15% ~ 1.0%, control C ≤ 0.0027%, S ≤ 0.0015%, N ≤ 0.0015%, Nb + V + Ti ≤ 0.0035%, La: 0.06% ~ 0.15%, Cu: 0.08% ~ 0.50%, Sn and / or Sb: 0.035% ~ 0.15%, P: 0.012% ~ 0.15%, B: 0.002% ~ 0.010%; the balance is Fe and impurities;
[0010] 2) Process control;
[0011] The molten steel meeting the alloy composition requirements is cast into billets, heated to 1000℃~1180℃ for hot rolling, and then cold rolled to obtain cold-rolled steel plates meeting the thickness specification requirements. The cold-rolled steel plates are continuously annealed with an average heating temperature of 780~1000℃ to obtain corrosion-resistant and high-efficiency non-oriented silicon steel products.
[0012] Furthermore, the thickness of the corrosion-resistant and high-efficiency non-oriented silicon steel product is ≤1.0 mm.
[0013] Compared with the prior art, the present invention has the following beneficial effects:
[0014] 1) Under the conditions of modern mainstream production technology, based on improving the cleanliness of steel and adding a variety of beneficial elements, the composite and synergistic effects of various elements are brought into play to produce silicon steel products with excellent electromagnetic properties and corrosion resistance.
[0015] 2) The corrosion resistance of the silicon steel products produced has been greatly improved, meeting the manufacturing needs of motors in special industries;
[0016] 3) Under the original conditions of silicon and aluminum content in the main alloy, high-efficiency silicon steel varieties can be produced, effectively improving the company's market competitiveness. DETAILED DESCRIPTION
[0017] The present invention discloses a method for producing corrosion-resistant and high-efficiency non-oriented silicon steel, including alloy composition design and process control; wherein:
[0018] 1) Alloy composition design; in corrosion-resistant and high-efficiency non-oriented silicon steel, the main alloy components include Si: 0.5%~3.35%, Als: 0.25%~1.5%, Mn: 0.15%~1.0% by mass percentage; on this basis, control C≤0.0027%, S≤0.0015%, N≤0.0015%, Nb+V+Ti≤0.0035%; in addition, add La: 0.06%~0.15%, Cu: 0.08%~0.50%, Sn and / or Sb: 0.035%~0.15%, P: 0.012%~0.15%, B: 0.002%~0.010%; the balance is Fe and impurities;
[0019] 2) Process control;
[0020] The molten steel meeting the alloy composition requirements is cast into billets, heated to 1000℃~1180℃ for hot rolling, and then cold rolled to obtain cold-rolled steel plates meeting the thickness specification requirements. The cold-rolled steel plates are continuously annealed with an average heating temperature of 780~1000℃ to obtain corrosion-resistant and high-efficiency non-oriented silicon steel products.
[0021] Furthermore, the thickness of the corrosion-resistant and high-efficiency non-oriented silicon steel product is ≤1.0 mm.
[0022] The production method of corrosion-resistant and efficient non-oriented silicon of the present invention is suitable for the production of cold-rolled non-oriented silicon steel series products with main alloy components of Si: 0.5% to 3.35%, Als: 0.25% to 1.5%, Mn: 0.15% to 1.0%, and finished product thickness specifications below 1.0 mm. The present invention mainly adopts the following technical measures:
[0023] 1. With the support of modern smelting and refining technology, the present invention controls the cleanliness of steel so as to give full play to the design function of microalloy; controls C≤0.0027% to ensure that no decarburization treatment is carried out during the heat treatment of the product, reduce the magnetic aging of the product, and ensure that the functional components of the product (such as the stator and rotor of the motor) can operate stably under relatively high temperature (motor operating temperature rise) conditions for a long time; controls S≤0.0015% to reduce sulfides and precipitates, and reduce the influence of sulfur on electromagnetic properties; controls N≤0.0015% to reduce nitrides and precipitates, reduce the lattice distortion of recrystallized structure, and reduce the influence of nitrogen on electromagnetic properties; controls Nb+V+Ti≤0.0035%. These three elements are harmful elements and are easy to form carbon nitrogen and composite fine precipitates, which affect favorable organizations and textures, affect magnetic domains, and deteriorate electromagnetic properties.
[0024] 2. Add lanthanide rare earth elements and control the La content at 0.06% to 0.15% to give full play to the corrosion resistance of rare earth elements on iron-based materials, while promoting the denaturation of inclusions and precipitates, promoting favorable organization and favorable texture components, and improving the electromagnetic properties of the product.
[0025] 3. Add copper element and control the Cu content within 0.08% to 0.50%; preferentially fix sulfur to form CuS particles, which play a role in compounding and coarsening sulfides; exert the corrosion resistance of copper element on iron-based materials; during the heat treatment of steel strip, Cu is enriched in the lower surface layer promoted by silicon, aluminum and rare earth elements, and exerts its corrosion resistance function.
[0026] 4. Add grain boundary segregation elements, such as Sn and / or Sb, and control their total content to 0.035% to 0.15%. Sn and Sb are the same type of elements with similar functions and effects. They can be added in combination or separately, and the total content can be controlled. By utilizing their characteristics of enrichment on the surface of grain boundary segregation, the precipitates formed by residual harmful elements in the steel can be reduced to pin the grain boundaries, improve the organization and texture; eliminate the influence of copper focusing on the grain boundaries on hot workability; strengthen the grain boundaries, improve product strength and improve processability; the most important role is to prevent copper from segregating at the grain boundaries and promote surface enrichment.
[0027] 5. Add phosphorus and control the P content at 0.012% to 0.15%. The synergistic effect of phosphorus and copper can improve the corrosion resistance. Under the inhibition of grain boundary segregation elements, the deterioration of cold working properties caused by phosphorus precipitation at the grain boundary is reduced, the processing accuracy during the stamping process of the stator and rotor is improved, the strength of the tooth yoke is increased, burrs are reduced, and the extension of "tip" corrosion is reduced.
[0028] 6. Add boron and control the B content within 0.002% to 0.010%; trace amounts of boron and nitrogen form precipitates and serve as the base nucleus of composite precipitates to improve the favorable organization and texture of the finished product; reduce stress sensitivity, reduce the influence of internal stress generated by hot and cold processing on magnetic properties, and indirectly eliminate stress effects; boron and phosphorus work synergistically to improve processing accuracy and reduce burrs.
[0029] The molten steel meeting the above alloy composition is cast into billets, and after heating, the furnace temperature is controlled at 1000-1180°C, hot rolled, and then cold rolled to the corresponding finished product specifications. The cold-rolled steel plate is continuously annealed in a continuous annealing unit, and the soaking temperature is controlled at 780-1000°C to complete the crystallization and grain growth process.
[0030] Compared with the same grade silicon steel products using main alloy elements, the corrosion-resistant and high-efficiency non-oriented silicon steel of the present invention has improved electromagnetic properties. A 48-hour salt spray test was carried out under laboratory conditions, and the rust spots were reduced by more than 95%, and the corrosion resistance was greatly improved.
[0031] In order to more intuitively embody the present invention, the embodiments of the present invention are further described in conjunction with examples. The following examples are only preferred specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any technical solution that can be obviously obtained by a person skilled in the art within the technical scope disclosed in the present invention, including simple changes or equivalent replacements, is within the protection scope of the present invention.
[0032]
Example 1
[0033] In this example, by using Comparative Example 1 and Example 1, the typical non-oriented low-grade products 65W1000 and 65W1000N are taken as examples to compare the chemical composition, production process and product performance of the products.
[0034] Comparative Example 1 produces 65W1000 product; the chemical composition of the product is Si: 0.53%, Als: 0.18%, Mn: 0.265%, P: 0.005%, C: 0.0035%, S: 0.0041%, N: 0.0021%, Nb+V+Ti: 0.0058% by mass; the remainder is Fe and impurities.
[0035] In Comparative Example 1, molten steel meeting the above chemical composition is cast into ingots, the furnace temperature after heating is 1165°C, and after hot rolling, it is cold rolled to a finished product specification of 0.65 mm in thickness. The cold-rolled steel plate is continuously annealed in a continuous annealing unit, and the soaking temperature is controlled at 820°C to complete the crystallization and grain growth process.
[0036] In Comparative Example 1, the electromagnetic properties of the non-oriented silicon steel product are as follows: iron loss P15 / 50 is 6.35 W / kg, and magnetic induction B5000 is 1.721 T.
[0037] Embodiment 1 produces 65W1000N product; The chemical composition in steel is Si: 0.58%, Als: 0.28%, Mn: 0.291%, P: 0.105%, C: 0.0025%, S: 0.0011%, N: 0.0013%, Nb+V+Ti: 0.0032%, Ia: 0.081%, Cu: 0.11%, Sn: 0.065%, B: 0.0031%; The balance is Fe and impurities.
[0038] The molten steel meeting the above chemical composition is cast into ingots, and the furnace temperature after heating is 1145°C. After hot rolling, it is cold rolled to a finished product specification of 0.65mm thickness. The cold-rolled steel plate is continuously annealed in a continuous annealing unit, and the soaking temperature is controlled at 820°C to complete the crystallization and grain growth process.
[0039] In Example 1, the electromagnetic properties of the non-oriented silicon steel product are as follows: iron loss P15 / 50 is 5.65 W / kg, and magnetic induction B5000 is 1.752 T.
[0040] Conclusion: Example 1 and Comparative Example 1 have the same main alloy composition. On this basis, the non-oriented silicon steel product of Example 1 achieves high performance, that is, it reaches the indicators of low iron loss and high magnetic induction. Under the conditions of accelerated corrosion treatment in the laboratory, the 65W1000N product produced in Example 1 has basically no rust spots, while the 65W1000 product produced in Comparative Example 1 has obvious rust spot distribution.
[0041]
Example 2
[0042] In this example, by using Comparative Example 2 and Example 2, typical non-oriented medium grade products 50W600 and 50W600N are taken as examples to compare the chemical composition, production process and product performance of the products.
[0043] Comparative Example 2 produces 50W600 product; the chemical composition of the product is Si: 1.21%, Als: 0.38%, Mn: 0.255%, P: 0.006%, C: 0.0033%, S: 0.0035%, N: 0.0020%, Nb+V+Ti: 0.0061% by mass; the remainder is Fe and impurities.
[0044] In Comparative Example 2, molten steel meeting the above chemical composition is cast into ingots, the furnace temperature after heating is 1155°C, and the ingots are cold rolled to a finished product specification of 0.50 mm in thickness. The cold rolled steel sheets are subjected to a continuous annealing unit with the soaking temperature controlled at 870°C to complete the crystallization and grain growth process.
[0045] In Comparative Example 2, the electromagnetic properties of the non-oriented silicon steel product are as follows: iron loss P15 / 50 is 4.35 W / kg, and magnetic induction B5000 is 1.681 T.
[0046] Example 2 produces 50W600N products; the chemical composition of the steel is Si: 1.32%, Als: 0.48%, Mn: 0.295%, P: 0.095%, C: 0.0023%, S: 0.0012%, N: 0.0012%, Nb+V+Ti: 0.0033%, Ia: 0.095%, Cu: 0.19%, Sn: 0.085%, B: 0.0042%; the remainder is Fe and impurities.
[0047] In Example 2, molten steel meeting the above chemical composition is cast into ingots, the furnace temperature after heating is 1155°C, and after hot rolling, it is cold rolled to a finished product specification of 0.50 mm in thickness. The cold-rolled steel sheet is continuously annealed in a continuous annealing unit, and the soaking temperature is controlled at 870°C to complete the crystallization and grain growth process.
[0048] In Example 2, the electromagnetic properties of the non-oriented silicon steel product are as follows: iron loss P15 / 50 is 3.95 W / kg, and magnetic induction B5000 is 1.722 T.
[0049] Conclusion: Example 2 and Comparative Example 2 have the same main alloy composition. On this basis, the non-oriented silicon steel product of Example 1 achieves high performance, that is, it reaches the indicators of low iron loss and high magnetic induction. Under the conditions of accelerated corrosion treatment in the laboratory, the 50W600N product produced in Example 2 has basically no rust spots, while the rust spot area of the 50W600 product produced in Comparative Example 2 reaches 21%.
[0050]
Example 3
[0051] In this example, by using Comparative Example 3 and Example 3, taking the typical non-oriented high-grade products 50W350 and 50W350N as examples, a comparison is made in terms of the chemical composition, production process and product performance of the products.
[0052] Comparative Example 3 produces 50W350 products; the chemical composition of the product is Si: 2.61%, Als: 0.51%, Mn: 0.285%, P: 0.005%, C: 0.0031%, S: 0.0021%, N: 0.0023%, Nb+V+Ti: 0.0067% by mass; the remainder is Fe and impurities.
[0053] In Comparative Example 3, molten steel meeting the above chemical composition is cast into ingots, the furnace temperature after heating is 1135°C, and the ingots are cold rolled to a finished product specification of 0.50 mm in thickness. The cold rolled steel sheets are placed in a continuous annealing unit with the soaking temperature controlled at 920°C to complete the crystallization and grain growth process.
[0054] In Comparative Example 3, the electromagnetic properties of the non-oriented silicon steel product are as follows: iron loss P15 / 50 is 2.91 W / kg, and magnetic induction B5000 is 1.671 T.
[0055] Example 3 produces 50W350N products; the chemical composition of the steel is Si: 2.65%, Als: 0.58%, Mn: 0.235%, P: 0.091%, C: 0.0020%, S: 0.0010%, N: 0.0011%, Nb+V+Ti: 0.0031%, Ia: 0.105%, Cu: 0.21%, Sn: 0.115%, B: 0.0072%; the balance is Fe and impurities.
[0056] In Example 3, molten steel meeting the above chemical composition is cast into ingots, the furnace temperature after heating is 1135°C, and after hot rolling, it is cold rolled to a finished product specification of 0.50 mm in thickness. The cold-rolled steel sheet is continuously annealed in a continuous annealing unit, and the soaking temperature is controlled at 820°C to complete the crystallization and grain growth process.
[0057] In Example 3, the electromagnetic properties of the non-oriented silicon steel product are as follows: iron loss P15 / 50 is 2.65 W / kg, and magnetic induction B5000 is 1.712 T.
[0058] Conclusion: Example 3 and Comparative Example 3 have the same main alloy composition. On this basis, the non-oriented silicon steel product of Example 1 achieves high performance, that is, it reaches the indicators of low iron loss and high magnetic induction. Under the conditions of accelerated corrosion treatment in the laboratory, individual rust spots are generated in the 50W350N product produced in Example 3, while the rust spot area of the 50W350 product produced in Comparative Example 3 reaches 29%.
[0059]
Example 4
[0060] In this example, by using Comparative Example 4 and Example 4, the typical non-oriented high-grade products 35W270 and 35W270N are taken as examples to compare the chemical composition, production process and product performance of the products.
[0061] Comparative Example 4 produces 35W270 product; the chemical composition of the product is Si: 3.05%, Als: 0.61%, Mn: 0.235%, P: 0.005%, C: 0.0033%, S: 0.0018%, N: 0.0020%, Nb+V+Ti: 0.0065% by mass; the remainder is Fe and impurities.
[0062] In Comparative Example 4, molten steel meeting the above chemical composition is cast into ingots, the furnace temperature after heating is 1125°C, and the ingots are cold rolled to a finished product specification of 0.35 mm in thickness. The cold rolled steel sheets are subjected to a continuous annealing unit with the soaking temperature controlled at 960°C to complete the crystallization and grain growth process.
[0063] In Comparative Example 4, the electromagnetic properties of the non-oriented silicon steel product are as follows: iron loss P15 / 50 is 2.55 W / kg, and magnetic induction B5000 is 1.666 T.
[0064] Example 4 produces 35W270N products; the chemical composition of the steel is Si: 2.95%, Als: 0.68%, Mn: 0.224%, P: 0.098%, C: 0.0021%, S: 0.0009%, N: 0.0012%, Nb+V+Ti: 0.0028%, Ia: 0.135%, Cu: 0.41%, Sn: 0.221%, B: 0.0042%; the remainder is Fe and impurities.
[0065] In Example 4, molten steel meeting the above chemical composition is cast into ingots, the furnace temperature after heating is 1125°C, and after hot rolling, it is cold rolled to a finished product specification of 0.35 mm in thickness. The cold-rolled steel sheet is continuously annealed in a continuous annealing unit, and the soaking temperature is controlled at 960°C to complete the crystallization and grain growth process.
[0066] In Example 4, the electromagnetic properties of the non-oriented silicon steel product are as follows: iron loss P15 / 50 is 2.45 W / kg, and magnetic induction B5000 is 1.704 T.
[0067] Conclusion: Example 4 and Comparative Example 4 have the same main alloy composition. On this basis, the non-oriented silicon steel product of Example 1 achieves high performance, that is, it reaches the indicators of low iron loss and high magnetic induction. Under the conditions of accelerated corrosion treatment in the laboratory, the 35W270N product produced in Example 4 has some rust spots with an area of about 0.6%; while the rust spot area of the 35W270 product produced in Comparative Example 4 reaches 31%.
[0068] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for producing corrosion-resistant and high-efficiency non-oriented silicon steel, characterized in that: Including alloy composition design and process control; among which: 1) Alloy composition design; in corrosion-resistant and high-efficiency non-oriented silicon steel, by mass percentage, including Si: 0.5%~0.58% or 2.65%~3.35%, Als: 1.5%, Mn: 0.15%~1.0%, C≤0.0027%, S≤0.0015%, N≤0.0015%, Nb+V+Ti0.0028%~0.0035%, La: 0.06%~0.15%, Cu: 0.19%~0.50%, Sn and / or Sb: 0.035%~0.15%, P: 0.012%~0.15%, B: 0.002%~0.010%; the balance is Fe and unavoidable impurities; 2) Process control; The molten steel meeting the alloy composition requirements is cast into billets, heated to 1000°C ~ 1180°C for hot rolling, and then cold rolled to obtain cold-rolled steel plates meeting the thickness specification requirements. The cold-rolled steel plates are continuously annealed with an average heating temperature of 780 ~ 1000°C to obtain corrosion-resistant and high-efficiency non-oriented silicon steel products. The thickness of the corrosion-resistant and high-efficiency non-oriented silicon steel products is ≤1.0mm.
Citation Information
Patent Citations
Method for preparing low-grade non-oriented electrical steel processed by rare earth
CN102345001A
Preparation method of non-oriented silicon steel for direct drive wind turbine
CN109097687A
High-magnetic-induction non-oriented silicon steel and production method thereof
CN117721286A
Non-orientation electrical steel and its making process
CN1888111A
Non-oriented silicon steel and manufacturing process therefor
WO2013127048A1
Cited By
Preparation method of corrosion-resistant non-oriented silicon steel for motor in high-corrosion environment
CN123063669A