A maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil and its preparation and application
Through the synergistic effect of components such as EDTA-piperazine modified graphene oxide, a maintenance solution for the surface of electrolytic cells for electrolytic copper foil was developed, which solved the problem of oxidized scale layers on the anode plate cells and achieved extended equipment life and energy efficiency. The consumption is reduced, the cleaning process is simplified, the production stability and the service life of the anode plate are improved.
Patent Information
- Application Number
- CN202411090670.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-09
AI Technical Summary
During the production process of electrolytic copper foil, the oxide scale layer on the surface of the anode plate tank leads to reduced conductivity, high energy consumption, and short equipment life. In addition, traditional cleaning methods damage the tank body, affecting production stability and accuracy.
Develop a maintenance solution for the surface of electrolytic cells for electrolytic copper foil, consisting of EDTA-piperazine modified graphene oxide, corrosion inhibitors, accelerators, penetrating agents and inhibitors. Through complexing, corrosion inhibition, promotion and penetration Function, synergistically remove the oxidized scale layer, and is environmentally friendly and energy-saving.
It effectively removes the oxidized scale layer, extends the service life of the equipment, reduces energy consumption, maintains the integrity of the tank matrix, increases the service life of the anode plate, simplifies operation, and creates a friendly operating environment.
Smart Images

Figure CN118639243B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of electrolytic copper foil and metal surface treatment, in particular to a maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil and the preparation and application thereof. Background Art
[0002] Copper foil is the main basic material for new energy lithium-ion power batteries, standard electronic circuit boards, 5G signals, artificial intelligence manufacturing, military industry, and aerospace. The manufacturing of copper foil is divided into electrolytic copper foil and rolled copper foil. Mainly due to different production equipment, processes, and applications, the technical requirements of copper foil are gradually increasing. The thinnest copper foil is 3~4 microns, and the thickest copper foil is 108 microns. At present, lithium-ion power battery copper foil is manufactured and produced by electrochemical electrodeposition. The main equipment is the cathode roller as the carrier cathode for copper deposition, the anode tank is a full titanium welded tank body as the storage of copper sulfate, additives and other solutions, and the anode plate is mainly a precious metal iridium titanium-based electrode, which is installed in the anode tank body in an arc shape. The electrolyte flows rapidly from the center of the tank body from bottom to top. During the power-on process, the anode plate discharges and the cathode copper ions are deposited. The current is transmitted to the tank body through the copper busbar, and the tank body conducts electricity to the anode plate. During this process, the contact surface between the anode plate and the tank body is non-softly fitted, and the gap causes the tank body to heat up and generate an oxide layer, mainly PbSO4, PbO2, PbO, etc., which has extremely poor conductivity, extremely high energy consumption, and the anode plate is corroded by electric shock, which seriously affects the continuous and stable production of electrolytic copper foil, reduces the qualified rate, and increases the unit manufacturing cost of the anode plate. And as the anode plate is disassembled during the electrolysis process, the traditional method is to use a scouring pad dipped in strong acid treatment or various mechanical grinding arc plates, which will damage the tank body in the long run, deform the slot shape, shorten the life, and the installation accuracy will become worse and worse.
[0003] Therefore, in order to solve the problem of oxide scale layer on the surface of anode plate tank in the process of electrolytic copper foil, an environmentally friendly and energy-saving maintenance method for oxide scale layer on the surface of anode tank of electrolytic copper foil is developed, which is beneficial to realize the industrial value in the field of copper foil, extend the service life and precision of its equipment, and at the same time improve the service life of anode plate and reduce various energy waste problems. Summary of the invention
[0004] The present invention proposes a maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil, and the preparation and application thereof. The maintenance liquid consists of a complexing agent, a corrosion inhibitor, a promoter, a penetrant and an inhibitor, wherein the complexing agent is EDTA-piperazine modified graphene oxide. The maintenance liquid has the characteristics of not damaging the cell body matrix, being environmentally friendly and energy-saving, and having no strong corrosion. The application of the maintenance liquid also has the advantages of being simple and easy, and being operator-friendly.
[0005] In order to achieve the above technical goals, the following technical solutions are adopted:
[0006] A maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil, comprising the following components in parts by weight: 25-85 parts of a complexing agent, 5-15 parts of a corrosion inhibitor, 8-35 parts of an accelerator, 15-28 parts of a penetrant, and 12-18 parts of an inhibitor;
[0007] The complexing agent is prepared from the following components in parts by weight: 10-20 parts of piperazine-modified graphene oxide, 60-70 parts of Na2EDTA, wherein the Na2EDTA is an analytically pure reagent;
[0008] The piperazine-modified graphene oxide is prepared from the following raw materials in parts by weight: 15-25 parts of graphite powder, 22.5-50 parts of K2Cr2O7, 17-22 parts of anhydrous piperazine, and 24-30 parts of 3-chloropropyltriethoxysilane, wherein the K2Cr2O7 is an analytical reagent, the purity of anhydrous piperazine is 99%, and the purity of 3-chloropropyltriethoxysilane is 98%.
[0009] Further, the preparation of the complexing agent comprises the following steps:
[0010] P1, take graphite powder and add it to 98wt% H2SO4, put it in an ice water bath, keep the temperature at 5~10℃, ultrasonically oscillate for 15min until dispersed, slowly add K2Cr2O7 and keep the temperature <10℃, stir at 300rpm for 2~3h, heat to 30~40℃ and continue stirring for 1~1.5h, add deionized water, heat to 80~90℃ and keep warm for 40~60min, then add 30wt% H2O2, continue to react for 10min, filter to obtain insoluble matter, wash with 5wt% hydrochloric acid and deionized water in turn, and then dry in an oven for 20h at 60℃ to obtain graphene oxide;
[0011] P2, dispersing the graphene oxide prepared in step P1 in toluene, and ultrasonically dispersing for 20 to 30 minutes to obtain a mixture A, and then dispersing anhydrous piperazine and 3-chloropropyltriethoxysilane in toluene, and ultrasonically dispersing at room temperature for 40 to 60 minutes to obtain a mixture B;
[0012] P3, adding the mixture B obtained in step P2 to the mixture A, stirring the mixture under reflux for 18-24 hours, the stirring speed is 200-300 rpm, the reaction temperature is 70-90°C, cooling to room temperature after the reaction is completed, and centrifuging at a speed of 4000-6000 rpm for 10 minutes to obtain a solid product, washing it with ethanol three times in sequence, and drying it in an oven at 60°C for 24 hours to obtain piperazine-modified graphene oxide;
[0013] P4, dissolve Na2EDTA in deionized water, and ultrasonicate for 15 minutes until it is dissolved to obtain a Na2EDTA aqueous solution, then take the piperazine-modified graphene oxide prepared in step P3 and add it to the Na2EDTA aqueous solution, ultrasonically homogenize for 30-40 minutes, react at room temperature for 20-24 hours, transfer to a centrifuge after the reaction, and centrifuge at a speed of 6000-8000 rpm for 5-10 minutes to obtain a product, wash the product with deionized water and ethanol three times in sequence, and then dry it in an oven at 70°C for 6 hours to obtain EDTA-piperazine-modified graphene oxide, which is the complexing agent.
[0014] Preferably, the concentration of the graphite powder in H2SO4 in step P1 is 15-25 g / L, the mass ratio of graphite powder to K2Cr2O7 is 1:1.5-2, and the volume ratio of H2SO4 to deionized water and H2O2 is 1:1:0.2-0.4.
[0015] Preferably, in step P2, the concentration of graphene oxide in toluene in the mixture A is 45-50 g / L, the concentration of anhydrous piperazine in toluene in the mixture B is 0.2-0.25 mol / L, the concentration of 3-chloropropyltriethoxysilane in toluene is 0.1-0.15 mol / L, the molar ratio of anhydrous piperazine to 3-chloropropyltriethoxysilane is 1:0.5, and the ratio of the toluene dosage of the mixture A to the mixture B is 1:1.
[0016] Preferably, in step P4, the concentration of Na2EDTA in deionized water is 60-70 g / L, and the concentration of piperazine-modified graphene oxide in deionized water is 10-20 g / L.
[0017] Furthermore, a method for preparing a maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil is as follows: 25-85 g / L of a complexing agent, 5-15 g / L of a corrosion inhibitor, 8-35 g / L of a promoter, 15-28 g / L of a penetrant and 12-18 g / L of an inhibitor are dissolved in water, stirred at 400 rpm for 10-20 min until the mixture is uniformly mixed, and compounded to obtain the maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil.
[0018] Preferably, the corrosion inhibitor is one of ethylene glycol, hydroxyethylene diphosphonic acid, ethylenediamine tetramethylene phosphonic acid and sodium oxalate.
[0019] Preferably, the promoter is one of octanol polyoxyethylene ether and dimethyltriamine pentaacetic acid, and the inhibitor is one of S-carboxyethyl isothiourea betaine, citric acid / sodium citrate, and acetic acid / sodium acetate.
[0020] Preferably, the penetrant is one of sodium dodecyl sulfate, hexadecyl dimethyl ammonium bromide, octylphenol polyoxyethylene ether, and isooctyl alcohol polyoxyethylene ether.
[0021] Furthermore, the application of a maintenance liquid on the surface of an electrolytic cell for electrolytic copper foil comprises the following steps:
[0022] S1, dismantle all the old anode plates in the anode tank after use, and when an oxide scale layer appears on the surface of the anode tank, use a high-pressure water gun to wash away the residual sulfuric acid, copper sulfate crystals, and organic additives in the anode tank, and dry them in a ventilated place at room temperature to obtain an anode tank without residue, wherein the anode tank is one of a back-pull type and an embedded type;
[0023] S2, dispersing a complexing agent in water to a concentration of 75-90 g / L, adding citric acid to adjust the pH to 4-6, obtaining a complexing agent solution, immersing the anode tank without residue obtained in step S1 in the complexing agent solution, soaking for 60-120 min under ultrasonic treatment, and taking out to obtain a pretreated anode tank;
[0024] S3, wearing plastic gloves and protective clothing, dip a rag in the maintenance liquid on the surface of the electrolytic copper foil electrolytic cell, and repeatedly wipe the pre-treated anode cell until the surface color changes from a variety of oxidation colors to the bright white color of titanium metal, and the pre-treated anode cell is dried at room temperature to obtain an anode cell with the oxide scale layer removed;
[0025] S4, use a rag dipped in clean water to repeatedly wipe the surface of the anode tank to remove the oxide scale layer, remove the maintenance liquid, and rinse it with a high-pressure water gun for 3 times. Ventilate and dry it to obtain the maintained anode tank.
[0026] The beneficial effects achieved by the present invention are as follows:
[0027] The present invention provides a maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil, and the preparation and application thereof. The maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil consists of a complexing agent, a corrosion inhibitor, a accelerator, a penetrant and an inhibitor. The maintenance liquid is obtained by mixing and homogenizing the components. The maintenance liquid is simple to use, does not damage the cell body matrix, is environmentally friendly and energy-saving, has no strong corrosion, and can effectively remove the oxide scale layer on the surface of the electrolytic cell for electrolytic copper foil.
[0028] Firstly, EDTA-piperazine modified graphene oxide was prepared as a complexing agent. This material is a graphene-based nanomaterial. Thanks to the inherent characteristics of graphene, it has a high specific surface area, good mechanical properties and chemical stability. Unmodified graphene itself has a good adsorption effect on lead ions due to electrostatic attraction and surface complexation. Graphene oxide is obtained by functionalizing graphene. The surface of graphene oxide has a large number of hydroxyl and carboxyl groups, which can improve its selectivity. Secondly, piperazine is used to further modify graphene oxide, and piperazine groups are grafted on graphene oxide. The modification of graphene oxide by piperazine is achieved by opening the epoxy group and introducing amino functional groups on graphene oxide, which can provide more active sites. Lead ions are attracted by the free nitrogen of piperazine and the hydroxyl groups of graphene oxide. Therefore, piperazine functionalization can improve the selectivity of graphene oxide. Graphene oxide has a synergistic effect in enhancing adsorption, among which the synergistic auxiliary effect between NH, -OH and -COOH groups is the main reason for the enhanced adsorption of lead ions. Furthermore, Na2EDTA is used to further functionalize piperazine-modified graphene. EDTA is a commonly used complexing agent. Its introduction here can not only combine with graphene oxide to change its porosity, but also combine with lead ions to form a chelate complex, so that the active sites are further increased. The adsorption activity of EDTA-piperazine-modified graphene oxide for lead ions comes from the electrostatic interaction between graphene oxide and lead ions, the complexation between EDTA and lead ions, and the interaction between piperazine groups and lead ions, which further improves the synergistic effect. At the same time, pH has a significant effect on the adsorption effect. When the pH is low, due to a large amount of H + The presence of lead ions and H + Competition occurs, resulting in a decrease in adsorption efficiency. At high pH, the adsorption rate is still reduced due to the conversion of lead ions into hydroxides. Too low or too high pH is not conducive to the removal of oxides. Finally, the chelating agent, corrosion inhibitor, promoter, penetrant and inhibitor are compounded. While deconstructing the surface oxides, the corrosion inhibitor can reduce the corrosion of the titanium-based anode tank during the cleaning process. The promoter can promote the reaction between the oxide scale layer and the maintenance solution and accelerate the removal efficiency. The penetrant can cause the maintenance solution to penetrate into the bottom of the oxide layer and accelerate dissolution. The inhibitor can ensure the cleaning effect.
[0029] The maintenance liquid for the surface of the electrolytic cell for electrolytic copper foil provided by the present invention, as well as the preparation and application thereof, has the advantages of being easy to use, energy-saving and environmentally friendly, having a good maintenance effect, and being friendly to operators. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions therein, the following briefly introduces the drawings required for use in the descriptions of the embodiments and comparative examples. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0031] Figure 1 The curve of the degree of removal of the oxide scale layer by the maintenance liquid changes with the pH;
[0032] Figure 2 It is an image of the back-pull electrolyzer body and its before and after maintenance;
[0033] Figure 3 It is an image of the embedded electrolyzer body and its before and after maintenance;
[0034] in, Figure 2 (a) is a schematic diagram of a back-pull electrolytic cell body, (b) is a diagram of a back-pull electrolytic cell body before maintenance, and (c) is a diagram of a back-pull electrolytic cell body after maintenance; Figure 3 (a) is a schematic diagram of the embedded electrolytic cell body, (b) is the embedded electrolytic cell body before maintenance, and (c) is the embedded electrolytic cell body after maintenance. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. The described embodiments are part of the embodiments of the present invention, but not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] Example 1: A maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil, comprising the following components in parts by weight: 55 parts of a complexing agent, 10 parts of a corrosion inhibitor, 21.5 parts of an accelerator, 21.5 parts of a penetrant, and 15 parts of an inhibitor;
[0037] The complexing agent is prepared from the following components in parts by weight: 15 parts of piperazine-modified graphene oxide, 65 parts of Na2EDTA, wherein the Na2EDTA is an analytically pure reagent;
[0038] Piperazine-modified graphene oxide is prepared from the following raw materials in parts by weight: 20 parts of graphite powder, 36 parts of K2Cr2O7, 17 parts of anhydrous piperazine, and 24 parts of 3-chloropropyltriethoxysilane, wherein the K2Cr2O7 is an analytical reagent, the purity of anhydrous piperazine is 99%, and the purity of 3-chloropropyltriethoxysilane is 98%.
[0039] The preparation of the complexing agent comprises the following steps:
[0040] P1, add graphite powder to 98wt% H2SO4, the concentration of graphite powder in H2SO4 is 20g / L, put it in an ice water bath, keep the temperature at 5℃, ultrasonically oscillate for 15min until dispersed, slowly add K2Cr2O7 and keep the temperature at 6℃, the mass ratio of graphite powder to K2Cr2O7 is 1:1.8, stir at 300rpm for 2h, heat to 30℃ and continue stirring for 1h, add deionized water, heat to 80℃ and keep warm for 60min, then add 30wt% H2O2, the volume ratio of H2SO4 to deionized water and H2O2 is 1:1:0.3, continue to react for 10min, filter to obtain insoluble matter, wash with 5wt% hydrochloric acid and deionized water in turn, and then dry in an oven for 20h at 60℃ to obtain graphene oxide;
[0041] P2, taking the graphene oxide prepared in step P1 and dispersing it in toluene, the concentration of graphene oxide in toluene is 50 g / L, and ultrasonically dispersing it for 20 minutes to obtain a mixture A, and then taking anhydrous piperazine and 3-chloropropyltriethoxysilane and dispersing them in toluene, and ultrasonically dispersing them at room temperature for 40 minutes to obtain a mixture B, the concentration of anhydrous piperazine in toluene is 0.2 mol / L, the concentration of 3-chloropropyltriethoxysilane in toluene is 0.1 mol / L, the molar ratio of anhydrous piperazine to 3-chloropropyltriethoxysilane is 1:0.5, and the ratio of the amount of toluene used in the mixture A to the mixture B is 1:1;
[0042] P3, adding the mixture B obtained in step P2 to the mixture A, stirring the mixture under reflux for 18 hours, the stirring speed is 200 rpm, the reaction temperature is 70°C, cooling to room temperature after the reaction is completed, and centrifuging at a speed of 4000 rpm for 10 minutes to obtain a solid product, washing it with ethanol three times in sequence, and drying it in an oven at 60°C for 24 hours to obtain piperazine-modified graphene oxide;
[0043] P4, dissolve Na2EDTA in deionized water, the concentration of Na2EDTA in deionized water is 65g / L, and ultrasonicate for 15min until it is dissolved to obtain a Na2EDTA aqueous solution, then take the piperazine-modified graphene oxide prepared in step P3 and add it to the Na2EDTA aqueous solution, the concentration of piperazine-modified graphene oxide in deionized water is 15g / L, ultrasonicate for 30min, react at room temperature for 20h, transfer to a centrifuge after the reaction, centrifuge at 6000rpm for 10min to obtain a product, wash the product with deionized water and ethanol three times in sequence, and then dry it in an oven at 70°C for 6h to obtain EDTA-piperazine-modified graphene oxide, which is the complexing agent.
[0044] A method for preparing a maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil comprises the following steps: dissolving 55 g / L of EDTA-piperazine modified graphene oxide as a complexing agent, 10 g / L of hydroxyethylidene diphosphonic acid as a corrosion inhibitor, 21.5 g / L of octanol polyoxyethylene ether as a promoter, 21.5 g / L of sodium dodecyl sulfonate as a penetrant, and 15 g / L of S-carboxyethyl isothiourea betaine as an inhibitor in water, stirring at 400 rpm for 10 min until the mixture is uniformly mixed, and compounding to obtain the maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil.
[0045] The application of a maintenance liquid on the surface of an electrolytic cell for electrolytic copper foil comprises the following steps:
[0046] S1, all the used anode plates in the back-pull anode tank are disassembled, and when an oxide scale layer appears on the surface of the anode tank, the residual sulfuric acid, copper sulfate crystals, and organic additives in the anode tank are washed with a high-pressure water gun, and then dried in a ventilated place at room temperature to obtain an anode tank without residue;
[0047] S2, dispersing a complexing agent in water at a concentration of 75 g / L, and then adding citric acid to adjust the pH to 4 to obtain a complexing agent solution, immersing the anode tank without residue obtained in step S1 in the complexing agent solution, infiltrating for 60 minutes under ultrasonic treatment, and taking it out to obtain a pretreated anode tank;
[0048] S3, wearing plastic gloves and protective clothing, dip a rag in the maintenance liquid on the surface of the electrolytic copper foil electrolytic cell, and repeatedly wipe the pre-treated anode cell until the surface color changes from a variety of oxidation colors to the bright white color of titanium metal, and the pre-treated anode cell is dried at room temperature to obtain an anode cell with the oxide scale layer removed;
[0049] S4, use a rag dipped in clean water to repeatedly wipe the surface of the anode tank to remove the oxide scale layer, remove the maintenance liquid, and rinse it with a high-pressure water gun for 3 times. Ventilate and dry it to obtain the maintained anode tank.
[0050] Example 2: A maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil, comprising the following components in parts by weight: 55 parts of a complexing agent, 10 parts of a corrosion inhibitor, 21.5 parts of an accelerator, 21.5 parts of a penetrant, and 15 parts of an inhibitor;
[0051] The complexing agent is prepared from the following components in parts by weight: 15 parts of piperazine-modified graphene oxide, 65 parts of Na2EDTA, wherein the Na2EDTA is an analytically pure reagent;
[0052] Piperazine-modified graphene oxide is prepared from the following raw materials in parts by weight: 20 parts of graphite powder, 36 parts of K2Cr2O7, 22 parts of anhydrous piperazine, and 30 parts of 3-chloropropyltriethoxysilane, wherein the K2Cr2O7 is an analytical reagent, the purity of anhydrous piperazine is 99%, and the purity of 3-chloropropyltriethoxysilane is 98%.
[0053] The preparation of the complexing agent comprises the following steps:
[0054] P1, add graphite powder to 98wt% H2SO4, the concentration of graphite powder in H2SO4 is 20g / L, put it in an ice water bath, keep the temperature at 10℃, ultrasonically oscillate for 15min until dispersed, slowly add K2Cr2O7 and keep the temperature at 9℃, the mass ratio of graphite powder to K2Cr2O7 is 1:1.8, stir at 300rpm for 3h, heat to 40℃ and continue stirring for 1.5h, add deionized water, heat to 90℃ and keep warm for 40min, then add 30wt% H2O2, the volume ratio of H2SO4 to deionized water and H2O2 is 1:1:0.3, continue to react for 10min, filter to obtain insoluble matter, wash with 5wt% hydrochloric acid and deionized water in turn, and then dry in an oven for 20h at 60℃ to obtain graphene oxide;
[0055] P2, taking the graphene oxide prepared in step P1 and dispersing it in toluene, the concentration of graphene oxide in toluene is 50 g / L, and ultrasonically dispersing it for 30 minutes to obtain a mixture A, and then taking anhydrous piperazine and 3-chloropropyltriethoxysilane and dispersing them in toluene, and ultrasonically dispersing them at room temperature for 60 minutes to obtain a mixture B, the concentration of anhydrous piperazine in toluene is 0.25 mol / L, the concentration of 3-chloropropyltriethoxysilane in toluene is 0.125 mol / L, the molar ratio of anhydrous piperazine to 3-chloropropyltriethoxysilane is 1:0.5, and the ratio of the amount of toluene used in the mixture A to the mixture B is 1:1;
[0056] P3, adding the mixture B obtained in step P2 to the mixture A, stirring the mixture under reflux for 24 hours, the stirring speed is 300 rpm, the reaction temperature is 90°C, cooling to room temperature after the reaction is completed, and centrifuging at a speed of 6000 rpm for 10 minutes to obtain a solid product, washing it with ethanol three times in sequence, and drying it in an oven at 60°C for 24 hours to obtain piperazine-modified graphene oxide;
[0057] P4, take Na2EDTA and dissolve it in deionized water, the concentration of Na2EDTA in deionized water is 65g / L, ultrasonicate for 15min until it is dissolved to obtain a Na2EDTA aqueous solution, then take the piperazine-modified graphene oxide prepared in step P3 and add it to the Na2EDTA aqueous solution, the concentration of piperazine-modified graphene oxide in deionized water is 15g / L, ultrasonicate for 40min, react at room temperature for 24h, transfer to a centrifuge after the reaction is completed, centrifuge at 8000rpm for 5min to obtain a product, wash the product with deionized water and ethanol three times in sequence, and then dry it in an oven at 70°C for 6h to obtain EDTA-piperazine-modified graphene oxide, which is the complexing agent.
[0058] A method for preparing a maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil comprises the following steps: dissolving 55 g / L of EDTA-piperazine modified graphene oxide as a complexing agent, 10 g / L of hydroxyethylidene diphosphonic acid as a corrosion inhibitor, 21.5 g / L of octanol polyoxyethylene ether as a promoter, 21.5 g / L of sodium dodecyl sulfonate as a penetrant, and 15 g / L of S-carboxyethyl isothiourea betaine as an inhibitor in water, stirring at 400 rpm for 20 min until the mixture is uniformly mixed, and compounding to obtain the maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil.
[0059] The application of a maintenance liquid on the surface of an electrolytic cell for electrolytic copper foil comprises the following steps:
[0060] S1, all the old anode plates in the embedded anode tank are removed, and when an oxide scale layer appears on the surface of the anode tank, the residual sulfuric acid, copper sulfate crystals, and organic additives in the anode tank are washed with a high-pressure water gun, and then dried in a ventilated place at room temperature to obtain an anode tank without residue;
[0061] S2, dispersing a complexing agent in water to a concentration of 90 g / L, and then adding citric acid to adjust the pH to 6 to obtain a complexing agent solution, immersing the anode tank without residue obtained in step S1 in the complexing agent solution, infiltrating for 120 min under ultrasonic treatment, and taking it out to obtain a pretreated anode tank;
[0062] S3, wearing plastic gloves and protective clothing, dip a rag in the maintenance liquid on the surface of the electrolytic copper foil electrolytic cell, and repeatedly wipe the pre-treated anode cell until the surface color changes from a variety of oxidation colors to the bright white color of titanium metal, and the pre-treated anode cell is dried at room temperature to obtain an anode cell with the oxide scale layer removed;
[0063] S4, use a rag dipped in clean water to repeatedly wipe the surface of the anode tank to remove the oxide scale layer, remove the maintenance liquid, and rinse it with a high-pressure water gun for 3 times. Ventilate and dry it to obtain the maintained anode tank.
[0064] Example 3: A maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil, comprising the following components in parts by weight: 55 parts of a complexing agent, 10 parts of a corrosion inhibitor, 21.5 parts of an accelerator, 21.5 parts of a penetrant, and 15 parts of an inhibitor;
[0065] The complexing agent is prepared from the following components in parts by weight: 15 parts of piperazine-modified graphene oxide, 65 parts of Na2EDTA, wherein the Na2EDTA is an analytically pure reagent;
[0066] Piperazine-modified graphene oxide is prepared from the following raw materials in parts by weight: 20 parts of graphite powder, 36 parts of K2Cr2O7, 19.5 parts of anhydrous piperazine, and 27.6 parts of 3-chloropropyltriethoxysilane, wherein the K2Cr2O7 is an analytical reagent, the purity of anhydrous piperazine is 99%, and the purity of 3-chloropropyltriethoxysilane is 98%.
[0067] The preparation of the complexing agent comprises the following steps:
[0068] P1, add graphite powder to 98wt% H2SO4, the concentration of graphite powder in H2SO4 is 20g / L, put it in an ice water bath, keep the temperature at 8℃, ultrasonically oscillate for 15min until dispersed, slowly add K2Cr2O7 and keep the temperature at 7℃, the mass ratio of graphite powder to K2Cr2O7 is 1:1.8, stir at 300rpm for 2.5h, heat to 35℃ and continue stirring for 1.25h, add deionized water, heat to 85℃ and keep warm for 50min, then add 30wt% H2O2, the volume ratio of H2SO4 to deionized water and H2O2 is 1:1:0.3, continue to react for 10min, filter to obtain insoluble matter, wash with 5wt% hydrochloric acid and deionized water in turn, and then dry in an oven for 20h at 60℃ to obtain graphene oxide;
[0069] P2, taking the graphene oxide prepared in step P1 and dispersing it in toluene, the concentration of graphene oxide in toluene is 50 g / L, and ultrasonically dispersing it for 25 minutes to obtain a mixture A, and then taking anhydrous piperazine and 3-chloropropyltriethoxysilane and dispersing them in toluene, and ultrasonically dispersing them at room temperature for 50 minutes to obtain a mixture B, the concentration of anhydrous piperazine in toluene is 0.23 mol / L, the concentration of 3-chloropropyltriethoxysilane in toluene is 0.115 mol / L, the molar ratio of anhydrous piperazine to 3-chloropropyltriethoxysilane is 1:0.5, and the ratio of the amount of toluene used in the mixture A to the mixture B is 1:1;
[0070] P3, adding the mixture B obtained in step P2 to the mixture A, stirring the mixture under reflux for 21 hours, the stirring speed is 250 rpm, the reaction temperature is 80°C, cooling to room temperature after the reaction is completed, and centrifuging at a speed of 5000 rpm for 10 minutes to obtain a solid product, washing it with ethanol three times in sequence, and drying it in an oven at 60°C for 24 hours to obtain piperazine-modified graphene oxide;
[0071] P4, take Na2EDTA and dissolve it in deionized water, the concentration of Na2EDTA in deionized water is 65g / L, ultrasonicate for 15min until it is dissolved to obtain a Na2EDTA aqueous solution, then take the piperazine-modified graphene oxide prepared in step P3 and add it to the Na2EDTA aqueous solution, the concentration of piperazine-modified graphene oxide in deionized water is 15g / L, ultrasonicate for 30min, react at room temperature for 22h, transfer to a centrifuge after the reaction is completed, centrifuge at a speed of 7000rpm for 8min to obtain a product, wash the product with deionized water and ethanol three times in sequence, and then dry it in an oven at 70°C for 6h to obtain EDTA-piperazine-modified graphene oxide, which is the complexing agent.
[0072] A method for preparing a maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil comprises the following steps: dissolving 55 g / L of EDTA-piperazine modified graphene oxide as a complexing agent, 10 g / L of ethylenediaminetetramethylenephosphonic acid as a corrosion inhibitor, 21.5 g / L of dimethyltriaminepentaacetic acid as a promoter, 21.5 g / L of hexadecyldimethylammonium bromide as a penetrant and 15 g / L of S-carboxyethylisothiourea betaine as an inhibitor in water, stirring at 400 rpm for 15 min until the mixture is uniformly mixed, and compounding to obtain the maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil.
[0073] The application of a maintenance liquid on the surface of an electrolytic cell for electrolytic copper foil comprises the following steps:
[0074] S1, all the used anode plates in the back-pull anode tank are disassembled, and when an oxide scale layer appears on the surface of the anode tank, the residual sulfuric acid, copper sulfate crystals, and organic additives in the anode tank are washed with a high-pressure water gun, and then dried in a ventilated place at room temperature to obtain an anode tank without residue;
[0075] S2, dispersing a complexing agent in water to a concentration of 82.5 g / L, and then adding citric acid to adjust the pH to 5 to obtain a complexing agent solution, immersing the anode tank without residue obtained in step S1 in the complexing agent solution, infiltrating for 90 minutes under ultrasonic treatment, and taking it out to obtain a pretreated anode tank;
[0076] S3, wearing plastic gloves and protective clothing, dip a rag in the maintenance liquid on the surface of the electrolytic copper foil electrolytic cell, and repeatedly wipe the pre-treated anode cell until the surface color changes from a variety of oxidation colors to the bright white color of titanium metal, and the pre-treated anode cell is dried at room temperature to obtain an anode cell with the oxide scale layer removed;
[0077] S4, use a rag dipped in clean water to repeatedly wipe the surface of the anode tank to remove the oxide scale layer, remove the maintenance liquid, and rinse it with a high-pressure water gun for 3 times. Ventilate and dry it to obtain the maintained anode tank.
[0078] Example 4: A maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil, comprising the following components in parts by weight: 55 parts of a complexing agent, 10 parts of a corrosion inhibitor, 21.5 parts of an accelerator, 21.5 parts of a penetrant, and 15 parts of an inhibitor;
[0079] The complexing agent is prepared from the following components in parts by weight: 10 parts of piperazine-modified graphene oxide, 65 parts of Na2EDTA, wherein the Na2EDTA is an analytically pure reagent;
[0080] Piperazine-modified graphene oxide is prepared from the following raw materials in parts by weight: 20 parts of graphite powder, 36 parts of K2Cr2O7, 19.5 parts of anhydrous piperazine, and 27.6 parts of 3-chloropropyltriethoxysilane, wherein the K2Cr2O7 is an analytical reagent, the purity of anhydrous piperazine is 99%, and the purity of 3-chloropropyltriethoxysilane is 98%.
[0081] The preparation of the complexing agent comprises the following steps:
[0082] P1, add graphite powder to 98wt% H2SO4, the concentration of graphite powder in H2SO4 is 20g / L, put it in an ice water bath, keep the temperature at 8℃, ultrasonically oscillate for 15min until dispersed, slowly add K2Cr2O7 and keep the temperature at 7℃, the mass ratio of graphite powder to K2Cr2O7 is 1:1.8, stir at 300rpm for 2.5h, heat to 35℃ and continue stirring for 1.25h, add deionized water, heat to 85℃ and keep warm for 50min, then add 30wt% H2O2, the volume ratio of H2SO4 to deionized water and H2O2 is 1:1:0.3, continue to react for 10min, filter to obtain insoluble matter, wash with 5wt% hydrochloric acid and deionized water in turn, and then dry in an oven for 20h at 60℃ to obtain graphene oxide;
[0083] P2, taking the graphene oxide prepared in step P1 and dispersing it in toluene, the concentration of graphene oxide in toluene is 50 g / L, and ultrasonically dispersing it for 25 minutes to obtain a mixture A, and then taking anhydrous piperazine and 3-chloropropyltriethoxysilane and dispersing them in toluene, and ultrasonically dispersing them at room temperature for 50 minutes to obtain a mixture B, the concentration of anhydrous piperazine in toluene is 0.23 mol / L, the concentration of 3-chloropropyltriethoxysilane in toluene is 0.115 mol / L, the molar ratio of anhydrous piperazine to 3-chloropropyltriethoxysilane is 1:0.5, and the ratio of the amount of toluene used in the mixture A to the mixture B is 1:1;
[0084] P3, adding the mixture B obtained in step P2 to the mixture A, stirring the mixture under reflux for 21 hours, the stirring speed is 250 rpm, the reaction temperature is 80°C, cooling to room temperature after the reaction is completed, and centrifuging at a speed of 5000 rpm for 10 minutes to obtain a solid product, washing it with ethanol three times in sequence, and drying it in an oven at 60°C for 24 hours to obtain piperazine-modified graphene oxide;
[0085] P4, dissolve Na2EDTA in deionized water, the concentration of Na2EDTA in deionized water is 65g / L, ultrasonicate for 15min until it is dissolved to obtain a Na2EDTA aqueous solution, then take the piperazine-modified graphene oxide prepared in step P3 and add it to the Na2EDTA aqueous solution, the concentration of piperazine-modified graphene oxide in deionized water is 10g / L, ultrasonicate for 30min, react at room temperature for 22h, transfer to a centrifuge after the reaction is completed, centrifuge at 7000rpm for 8min to obtain a product, wash the product with deionized water and ethanol three times in sequence, and then dry it in an oven at 70°C for 6h to obtain EDTA-piperazine-modified graphene oxide, which is the complexing agent.
[0086] The steps of preparing a maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil and applying the maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil are consistent with those of Example 3.
[0087] Example 5: A maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil, comprising the following components in parts by weight: 55 parts of a complexing agent, 10 parts of a corrosion inhibitor, 21.5 parts of an accelerator, 21.5 parts of a penetrant, and 15 parts of an inhibitor;
[0088] The complexing agent is prepared from the following components in parts by weight: 20 parts of piperazine-modified graphene oxide, 65 parts of Na2EDTA, wherein the Na2EDTA is an analytically pure reagent;
[0089] Piperazine-modified graphene oxide is prepared from the following raw materials in parts by weight: 20 parts of graphite powder, 36 parts of K2Cr2O7, 19.5 parts of anhydrous piperazine, and 27.6 parts of 3-chloropropyltriethoxysilane, wherein the K2Cr2O7 is an analytical reagent, the purity of anhydrous piperazine is 99%, and the purity of 3-chloropropyltriethoxysilane is 98%.
[0090] The preparation of the complexing agent comprises the following steps:
[0091] P1, add graphite powder to 98wt% H2SO4, the concentration of graphite powder in H2SO4 is 20g / L, put it in an ice water bath, keep the temperature at 8℃, ultrasonically oscillate for 15min until dispersed, slowly add K2Cr2O7 and keep the temperature at 7℃, the mass ratio of graphite powder to K2Cr2O7 is 1:1.8, stir at 300rpm for 2.5h, heat to 35℃ and continue stirring for 1.25h, add deionized water, heat to 85℃ and keep warm for 50min, then add 30wt% H2O2, the volume ratio of H2SO4 to deionized water and H2O2 is 1:1:0.3, continue to react for 10min, filter to obtain insoluble matter, wash with 5wt% hydrochloric acid and deionized water in turn, and then dry in an oven for 20h at 60℃ to obtain graphene oxide;
[0092] P2, taking the graphene oxide prepared in step P1 and dispersing it in toluene, the concentration of graphene oxide in toluene is 50 g / L, and ultrasonically dispersing it for 25 minutes to obtain a mixture A, and then taking anhydrous piperazine and 3-chloropropyltriethoxysilane and dispersing them in toluene, and ultrasonically dispersing them at room temperature for 50 minutes to obtain a mixture B, the concentration of anhydrous piperazine in toluene is 0.23 mol / L, the concentration of 3-chloropropyltriethoxysilane in toluene is 0.115 mol / L, the molar ratio of anhydrous piperazine to 3-chloropropyltriethoxysilane is 1:0.5, and the ratio of the amount of toluene used in the mixture A to the mixture B is 1:1;
[0093] P3, adding the mixture B obtained in step P2 to the mixture A, stirring the mixture under reflux for 21 hours, the stirring speed is 250 rpm, the reaction temperature is 80°C, cooling to room temperature after the reaction is completed, and centrifuging at a speed of 5000 rpm for 10 minutes to obtain a solid product, washing it with ethanol three times in sequence, and drying it in an oven at 60°C for 24 hours to obtain piperazine-modified graphene oxide;
[0094] P4, take Na2EDTA and dissolve it in deionized water, the concentration of Na2EDTA in deionized water is 65g / L, ultrasonicate for 15min until it is dissolved to obtain a Na2EDTA aqueous solution, then take the piperazine-modified graphene oxide prepared in step P3 and add it to the Na2EDTA aqueous solution, the concentration of piperazine-modified graphene oxide in deionized water is 20g / L, ultrasonicate for 30min, react at room temperature for 22h, transfer to a centrifuge after the reaction is completed, centrifuge at 7000rpm for 8min to obtain a product, wash the product with deionized water and ethanol three times in sequence, and then dry it in an oven at 70°C for 6h to obtain EDTA-piperazine-modified graphene oxide, which is the complexing agent.
[0095] The steps of preparing a maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil and applying the maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil are consistent with those of Example 3.
[0096] Example 6: A maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil, comprising the following components in parts by weight: 55 parts of a complexing agent, 10 parts of a corrosion inhibitor, 21.5 parts of an accelerator, 21.5 parts of a penetrant, and 15 parts of an inhibitor;
[0097] The complexing agent is prepared from the following components in parts by weight: 20 parts of piperazine-modified graphene oxide, 60 parts of Na2EDTA, wherein the Na2EDTA is an analytically pure reagent;
[0098] Piperazine-modified graphene oxide is prepared from the following raw materials in parts by weight: 20 parts of graphite powder, 36 parts of K2Cr2O7, 19.5 parts of anhydrous piperazine, and 27.6 parts of 3-chloropropyltriethoxysilane, wherein the K2Cr2O7 is an analytical reagent, the purity of anhydrous piperazine is 99%, and the purity of 3-chloropropyltriethoxysilane is 98%.
[0099] The preparation of the complexing agent comprises the following steps:
[0100] P1, add graphite powder to 98wt% H2SO4, the concentration of graphite powder in H2SO4 is 20g / L, put it in an ice water bath, keep the temperature at 8℃, ultrasonically oscillate for 15min until dispersed, slowly add K2Cr2O7 and keep the temperature at 7℃, the mass ratio of graphite powder to K2Cr2O7 is 1:1.8, stir at 300rpm for 2.5h, heat to 35℃ and continue stirring for 1.25h, add deionized water, heat to 85℃ and keep warm for 50min, then add 30wt% H2O2, the volume ratio of H2SO4 to deionized water and H2O2 is 1:1:0.3, continue to react for 10min, filter to obtain insoluble matter, wash with 5wt% hydrochloric acid and deionized water in turn, and then dry in an oven for 20h at 60℃ to obtain graphene oxide;
[0101] P2, taking the graphene oxide prepared in step P1 and dispersing it in toluene, the concentration of graphene oxide in toluene is 50 g / L, and ultrasonically dispersing it for 25 minutes to obtain a mixture A, and then taking anhydrous piperazine and 3-chloropropyltriethoxysilane and dispersing them in toluene, and ultrasonically dispersing them at room temperature for 50 minutes to obtain a mixture B, the concentration of anhydrous piperazine in toluene is 0.23 mol / L, the concentration of 3-chloropropyltriethoxysilane in toluene is 0.115 mol / L, the molar ratio of anhydrous piperazine to 3-chloropropyltriethoxysilane is 1:0.5, and the ratio of the amount of toluene used in the mixture A to the mixture B is 1:1;
[0102] P3, adding the mixture B obtained in step P2 to the mixture A, stirring the mixture under reflux for 21 hours, the stirring speed is 250 rpm, the reaction temperature is 80°C, cooling to room temperature after the reaction is completed, and centrifuging at a speed of 5000 rpm for 10 minutes to obtain a solid product, washing it with ethanol three times in sequence, and drying it in an oven at 60°C for 24 hours to obtain piperazine-modified graphene oxide;
[0103] P4, dissolve Na2EDTA in deionized water, the concentration of Na2EDTA in deionized water is 60g / L, and ultrasonicate for 15min until it is dissolved to obtain a Na2EDTA aqueous solution, then take the piperazine-modified graphene oxide prepared in step P3 and add it to the Na2EDTA aqueous solution, the concentration of piperazine-modified graphene oxide in deionized water is 20g / L, ultrasonicate for 30min, react at room temperature for 22h, transfer to a centrifuge after the reaction, centrifuge at 7000rpm for 8min to obtain a product, wash the product with deionized water and ethanol three times in sequence, and then dry it in an oven at 70°C for 6h to obtain EDTA-piperazine-modified graphene oxide, which is the complexing agent.
[0104] The steps of preparing a maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil and applying the maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil are consistent with those of Example 3.
[0105] Example 7: A maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil, comprising the following components in parts by weight: 55 parts of a complexing agent, 10 parts of a corrosion inhibitor, 21.5 parts of an accelerator, 21.5 parts of a penetrant, and 15 parts of an inhibitor;
[0106] The complexing agent is prepared from the following components in parts by weight: 20 parts of piperazine-modified graphene oxide, 70 parts of Na2EDTA, wherein the Na2EDTA is an analytically pure reagent;
[0107] Piperazine-modified graphene oxide is prepared from the following raw materials in parts by weight: 20 parts of graphite powder, 36 parts of K2Cr2O7, 19.5 parts of anhydrous piperazine, and 27.6 parts of 3-chloropropyltriethoxysilane, wherein the K2Cr2O7 is an analytical reagent, the purity of anhydrous piperazine is 99%, and the purity of 3-chloropropyltriethoxysilane is 98%.
[0108] The preparation of the complexing agent comprises the following steps:
[0109] P1, add graphite powder to 98wt% H2SO4, the concentration of graphite powder in H2SO4 is 20g / L, put it in an ice water bath, keep the temperature at 8℃, ultrasonically oscillate for 15min until dispersed, slowly add K2Cr2O7 and keep the temperature at 7℃, the mass ratio of graphite powder to K2Cr2O7 is 1:1.8, stir at 300rpm for 2.5h, heat to 35℃ and continue stirring for 1.25h, add deionized water, heat to 85℃ and keep warm for 50min, then add 30wt% H2O2, the volume ratio of H2SO4 to deionized water and H2O2 is 1:1:0.3, continue to react for 10min, filter to obtain insoluble matter, wash with 5wt% hydrochloric acid and deionized water in turn, and then dry in an oven for 20h at 60℃ to obtain graphene oxide;
[0110] P2, taking the graphene oxide prepared in step P1 and dispersing it in toluene, the concentration of graphene oxide in toluene is 50 g / L, and ultrasonically dispersing it for 25 minutes to obtain a mixture A, and then taking anhydrous piperazine and 3-chloropropyltriethoxysilane and dispersing them in toluene, and ultrasonically dispersing them at room temperature for 50 minutes to obtain a mixture B, the concentration of anhydrous piperazine in toluene is 0.23 mol / L, the concentration of 3-chloropropyltriethoxysilane in toluene is 0.115 mol / L, the molar ratio of anhydrous piperazine to 3-chloropropyltriethoxysilane is 1:0.5, and the ratio of the amount of toluene used in the mixture A to the mixture B is 1:1;
[0111] P3, adding the mixture B obtained in step P2 to the mixture A, stirring the mixture under reflux for 21 hours, the stirring speed is 250 rpm, the reaction temperature is 80°C, cooling to room temperature after the reaction is completed, and centrifuging at a speed of 5000 rpm for 10 minutes to obtain a solid product, washing it with ethanol three times in sequence, and drying it in an oven at 60°C for 24 hours to obtain piperazine-modified graphene oxide;
[0112] P4, dissolve Na2EDTA in deionized water, the concentration of Na2EDTA in deionized water is 70g / L, and ultrasonicate for 15min until it is dissolved to obtain a Na2EDTA aqueous solution, then take the piperazine-modified graphene oxide prepared in step P3 and add it to the Na2EDTA aqueous solution, the concentration of piperazine-modified graphene oxide in deionized water is 20g / L, ultrasonically homogenize for 30min, react at room temperature for 22h, transfer to a centrifuge after the reaction, centrifuge at 7000rpm for 8min to obtain a product, wash the product with deionized water and ethanol three times in sequence, and then dry it in an oven at 70°C for 6h to obtain EDTA-piperazine-modified graphene oxide, which is the complexing agent.
[0113] The steps of preparing a maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil and applying the maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil are consistent with those of Example 3.
[0114] Example 8: A maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil, comprising the following components in parts by weight: 25 parts of a complexing agent, 5 parts of a corrosion inhibitor, 8 parts of an accelerator, 15 parts of a penetrant, and 12 parts of an inhibitor;
[0115] The complexing agent is prepared from the following components in parts by weight: 15 parts of piperazine-modified graphene oxide, 65 parts of Na2EDTA, wherein the Na2EDTA is an analytically pure reagent;
[0116] Piperazine-modified graphene oxide is prepared from the following raw materials in parts by weight: 20 parts of graphite powder, 36 parts of K2Cr2O7, 19.5 parts of anhydrous piperazine, and 27.6 parts of 3-chloropropyltriethoxysilane, wherein the K2Cr2O7 is an analytical reagent, the purity of anhydrous piperazine is 99%, and the purity of 3-chloropropyltriethoxysilane is 98%.
[0117] The preparation method and steps of the complexing agent are consistent with those in Example 3.
[0118] A method for preparing a maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil comprises the following steps: dissolving 25 g / L of EDTA-piperazine modified graphene oxide as a complexing agent, 5 g / L of ethylenediaminetetramethylenephosphonic acid as a corrosion inhibitor, 8 g / L of dimethyltriaminepentaacetic acid as a promoter, 15 g / L of hexadecyldimethylammonium bromide as a penetrant and 12 g / L of S-carboxyethylisothiourea betaine as an inhibitor in water, stirring at 400 rpm for 15 min until the mixture is uniformly mixed, and compounding to obtain the maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil.
[0119] The steps of applying a maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil are consistent with those of Example 3.
[0120] Example 9: A maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil, comprising the following components in parts by weight: 85 parts of a complexing agent, 15 parts of a corrosion inhibitor, 35 parts of an accelerator, 28 parts of a penetrant, and 18 parts of an inhibitor;
[0121] The complexing agent is prepared from the following components in parts by weight: 15 parts of piperazine-modified graphene oxide, 65 parts of Na2EDTA, wherein the Na2EDTA is an analytically pure reagent;
[0122] Piperazine-modified graphene oxide is prepared from the following raw materials in parts by weight: 20 parts of graphite powder, 36 parts of K2Cr2O7, 19.5 parts of anhydrous piperazine, and 27.6 parts of 3-chloropropyltriethoxysilane, wherein the K2Cr2O7 is an analytical reagent, the purity of anhydrous piperazine is 99%, and the purity of 3-chloropropyltriethoxysilane is 98%.
[0123] The preparation method and steps of the complexing agent are consistent with those in Example 3.
[0124] A method for preparing a maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil comprises the following steps: dissolving 85 g / L of EDTA-piperazine modified graphene oxide as a complexing agent, 15 g / L of ethylenediaminetetramethylenephosphonic acid as a corrosion inhibitor, 35 g / L of dimethyltriaminepentaacetic acid as a promoter, 28 g / L of hexadecyldimethylammonium bromide as a penetrant and 18 g / L of S-carboxyethylisothiourea betaine as an inhibitor in water, stirring at 400 rpm for 15 min until the mixture is uniformly mixed, and compounding to obtain the maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil.
[0125] The steps of applying a maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil are consistent with those of Example 3.
[0126] Comparative Example 1:
[0127] Based on Example 3, the difference is that piperazine is not used to modify the graphene oxide, and only Na2EDTA is used for modification. The remaining steps and methods are consistent with Example 3.
[0128] Comparative Example 2:
[0129] Based on Example 3, the difference is that Na2EDTA is not used for further functionalization modification, and only piperazine is used to modify the graphene oxide, and the remaining steps and methods are consistent with Example 3.
[0130] Comparative Example 3:
[0131] Based on Example 3, the difference is that graphene oxide is directly used without any modification treatment, and the remaining steps and methods are consistent with Example 3.
[0132] Experimental example:
[0133] 1. Cleaning and maintenance experiment:
[0134] The maintenance liquid prepared in each embodiment and comparative example is used to clean and maintain the anode tank that has been used for a long time and has formed an oxide scale layer on the surface according to the application method of the maintenance liquid. The selected anode tank should have similar use conditions and usage, and the thickness of the surface scale layer is also similar. The oxide scale layer on the surface of the anode tank is cleaned according to the same steps and cleaning and maintenance parameters, and observed with the naked eye under natural light. The cleaning degree is graded according to the color change and residual degree of the surface oxide scale layer, A is a removal rate of >95%, B is a removal rate of >90%, C is a removal rate of >80%, D is a removal rate of >65%, E is a removal rate of >45%, and F is a removal rate of <45%.
[0135] The removal rates of the oxide scale layer by the maintenance solutions prepared in the embodiments and comparative examples are shown in Table 1.
[0136] 2. Cleaning and maintenance experiments at different pH values:
[0137] Taking Example 3 as a benchmark, in the application of the maintenance liquid on the surface of the electrolytic cell for electrolytic copper foil, the pH is set to 2, 4, 6, 8, and 10, respectively, and the maintenance liquid is compounded according to the parameters and conditions of Example 3, and the anode cell that has been used for a long time and has formed an oxide scale layer on the surface is cleaned and maintained according to the application method of the maintenance liquid, and the cleaning and maintenance experiment is carried out and the cleaning degree is graded according to Experimental Example 1.
[0138] Taking Example 3 as a reference, the oxide scale removal rate of the maintenance solution at different pH values is shown in Table 2 and Figure 1 Shown
[0139] Table 1. Cleaning degree of oxide scale layer by maintenance solution prepared in each embodiment and comparative example
[0140]
[0141] Table 2. Cleaning degree of oxide scale layer by maintenance solution at different pH values based on Example 3
[0142]
[0143] In the application of the maintenance liquid on the surface of the electrolytic cell for electrolytic copper foil, the pH is set to 2, 4, 6, 8, and 10, and the maintenance liquid is compounded according to the parameters and conditions of Comparative Examples 1, 2, and 3. The anode cell that has been used for a long time and has formed an oxide scale layer on the surface is cleaned and maintained according to the application method of the maintenance liquid. The cleaning and maintenance experiment is carried out and the cleaning degree is graded according to Experimental Example 1. The oxide scale layer removal rates of the maintenance liquids of Comparative Examples 1, 2, and 3 at different pH values are shown in Tables 3, 4, and 5.
[0144] Table 3. Cleaning degree of oxide scale layer by maintenance solution at different pH values based on Comparative Example 1
[0145]
[0146] Table 4. Cleaning degree of oxide scale layer by maintenance solution at different pH values based on Comparative Example 2
[0147]
[0148] Table 5. Cleaning degree of oxide scale layer by maintenance solution at different pH values based on Comparative Example 3
[0149]
[0150] According to the experimental examples, the cleaning degree of the oxide layer on the surface of the anode tank of the maintenance solution prepared in each embodiment and the comparative example under the same conditions and parameters is evaluated. From the evaluation results (such as Table 1), it can be seen that with the increase in the number of piperazine groups introduced, the cleaning rate of the oxide scale layer of the prepared maintenance solution increases. When the piperazine-modified graphene oxide is further functionalized with Na2EDTA, the increase in the amount of Na2EDTA and piperazine-modified graphene oxide is conducive to improving the cleaning performance of the complexing agent finally obtained on the oxide layer. Combined with Comparative Examples 1 to 3, it can also be obtained that Conclusion: The piperazine group, Na2EDTA functionalization and graphene oxide have a synergistic effect on the deconstruction of the oxide scale layer on the surface of the tank body. This is mainly due to the increase in the surface active sites of the complexing agent, which enhances the adsorption of lead ions by EDTA-piperazine modified graphene oxide. The superposition of interaction forces such as complexation and electrostatic interaction makes the oxide scale layer more thoroughly removed; In Experimental Example 2, the removal rate of the oxide scale layer by the maintenance liquid at different pH values is shown in Tables 2, 3, 4, 5 and 6. Figure 1 This result shows that pH has a significant effect on the degree of cleaning. When the pH is too low, a large amount of H + The lead ions are in a competitive relationship with the lead ions, and the lead ions are converted into hydroxides when the pH is high. Both of these will reduce the adsorption efficiency and affect the cleaning process of the oxide scale layer. Therefore, a reasonable pH is very important, and the cleaning process of the oxide scale layer prepared by the maintenance solutions of Comparative Examples 1, Comparative Examples 2, and Comparative Examples 3 under different pH conditions is significantly lower than that of Example 3; Finally, Figure 2 The images of the back-pull electrolytic cell and its maintenance before and after. Figure 3 These are images of the embedded electrolytic cell body and before and after maintenance. Regardless of whether it is a back-pull type or an embedded type, after the electrolytic cell body is cured with the maintenance liquid, the colored oxide scale layer on the surface is removed, and the bright white titanium base is re-exposed, indicating that the maintenance liquid has a significant effect on removing and cleaning the oxide scale layer.
[0151] The present invention and its embodiments are described above. The described embodiments are only some embodiments of the present invention, not all embodiments. The drawings are only one of many embodiments of the present invention. The detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but only represents the selected embodiments of the present invention. Based on this, other specific embodiments of the present invention obtained by those skilled in the art under the inspiration of the technical solution without creative labor should fall within the protection scope of the present invention.
Claims
1. A maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil, characterized in that: The maintenance liquid for the surface of the electrolytic cell for electrolytic copper foil is composed of the following components in parts by weight: 25-85 parts of complexing agent, 5-15 parts of corrosion inhibitor, 8-35 parts of accelerator, 15-28 parts of penetrant, and 12-18 parts of inhibitor; The complexing agent is prepared from the following components in parts by weight: 10-20 parts of piperazine-modified graphene oxide, 60-70 parts of Na2EDTA; The piperazine-modified graphene oxide is prepared from the following raw materials in parts by weight: 15-25 parts of graphite powder, 22.5-50 parts of K2Cr2O7, 17-22 parts of anhydrous piperazine, and 24-30 parts of 3-chloropropyltriethoxysilane; The preparation of the complexing agent comprises the following steps: P1, add graphite powder to 98wt% H2SO4, place in an ice water bath, ultrasonically oscillate until dispersed, slowly add K2Cr2O7, stir for 2-3h, heat to 30-40℃ and continue stirring, add deionized water, heat to 80-90℃ and keep warm for 40-60min, then add 30wt% H2O2, react, filter to obtain insoluble matter, wash with 5wt% hydrochloric acid and deionized water in turn, and dry to obtain graphene oxide; P2, dispersing the graphene oxide prepared in step P1 in toluene to obtain a mixture A, and then dispersing anhydrous piperazine and 3-chloropropyltriethoxysilane in toluene to obtain a mixture B; P3, adding the mixture B obtained in step P2 to the mixture A, stirring and reacting under reflux, centrifuging after the reaction is completed to obtain a solid product, washing it with ethanol in turn, and drying it to obtain piperazine-modified graphene oxide; P4, dissolving Na2EDTA in deionized water, ultrasonicating until it is dissolved to obtain a Na2EDTA aqueous solution, then adding the piperazine-modified graphene oxide prepared in step P3 to the Na2EDTA aqueous solution, ultrasonically homogenizing, reacting, centrifuging after the reaction to obtain a product, washing the product with deionized water and ethanol in turn, drying, and obtaining EDTA-piperazine-modified graphene oxide, which is the complexing agent; The corrosion inhibitor is one of ethylene glycol, hydroxyethylene diphosphonic acid, ethylenediamine tetramethylene phosphonic acid and sodium oxalate; The accelerator is one of octanol polyoxyethylene ether and dimethyltriamine pentaacetic acid, and the inhibitor is one of S-carboxyethyl isothiourea betaine, citric acid / sodium citrate, and acetic acid / sodium acetate; The penetrant is one of sodium dodecyl sulfate, hexadecyl dimethyl ammonium bromide, octylphenol polyoxyethylene ether, and isooctyl alcohol polyoxyethylene ether; The application of the electrolytic copper foil electrolytic cell surface maintenance liquid on the electrolytic cell surface comprises the following steps: S1, dismantle all the old anode plates in the anode tank after use, wherein the anode tank is one of a back-pull type and an embedded type, and when an oxide scale layer appears on the surface of the anode tank, use a high-pressure water gun to wash away the residual sulfuric acid, copper sulfate crystals, and organic additives in the anode tank, and dry them in a ventilated place at room temperature to obtain an anode tank without residue; S2, dispersing a complexing agent in water at a concentration of 75-90 g / L, adding citric acid to adjust the pH to 4-6, obtaining a complexing agent solution, immersing the anode tank without residue obtained in step S1 in the complexing agent solution, soaking under ultrasonic treatment, and taking out to obtain a pretreated anode tank; S3, wearing plastic gloves and protective clothing, dip a rag in the maintenance liquid on the surface of the electrolytic copper foil electrolytic cell, and repeatedly wipe the pre-treated anode cell until the surface color changes from a variety of oxidation colors to the bright white color of titanium metal, and the pre-treated anode cell is dried at room temperature to obtain an anode cell with the oxide scale layer removed; S4, use a rag dipped in clean water to repeatedly wipe the surface of the anode tank to remove the oxide scale layer, remove the maintenance liquid, and rinse it with a high-pressure water gun for 3 times. Ventilate and dry it to obtain the maintained anode tank.
2. The maintenance liquid for the surface of the electrolytic cell for electrolytic copper foil according to claim 1, characterized in that: The concentration of the graphite powder in H2SO4 in step P1 is 15-25 g / L, the mass ratio of graphite powder to K2Cr2O7 is 1:1.5-2, and the volume ratio of H2SO4 to deionized water and H2O2 is 1:1:0.2-0.
4.
3. The maintenance liquid for the surface of the electrolytic cell for electrolytic copper foil according to claim 2, characterized in that: In step P2, the concentration of graphene oxide in toluene in mixture A is 45-50 g / L, the concentration of anhydrous piperazine in toluene in mixture B is 0.2-0.25 mol / L, the concentration of 3-chloropropyltriethoxysilane in toluene is 0.1-0.15 mol / L, the molar ratio of anhydrous piperazine to 3-chloropropyltriethoxysilane is 1:0.5, and the ratio of the toluene dosage of mixture A to mixture B is 1:
1.
4. The maintenance liquid for the surface of the electrolytic cell for electrolytic copper foil according to claim 3, characterized in that: In step P4, the concentration of Na2EDTA in deionized water is 60-70 g / L, and the concentration of piperazine-modified graphene oxide in deionized water is 10-20 g / L.
5. A method for preparing a maintenance liquid for the surface of an electrolytic cell for electrolytic copper foil according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: dissolving 25-85 g / L of a complexing agent, 5-15 g / L of a corrosion inhibitor, 8-35 g / L of an accelerator, 15-28 g / L of a penetrant and 12-18 g / L of an inhibitor in water, stirring the mixture evenly, and compounding the surface maintenance liquid of the electrolytic cell for the electrolytic copper foil.
Citation Information
Patent Citations
Aluminum alloy raw material surface cleaning method
CN107513716A
Metal cleaning agent added with functional modified graphene and preparing method of metal cleaning agent
CN107513719A