A high-strength composite fiber material and its application

By ultrasonication and modification of coconut fibers, combined with the hot pressing forming process, the problem of insufficient strength and impact resistance of existing high-strength composite fiber materials is solved, and the strength and tensile properties of the material are significantly improved. It is suitable for Manufacturing of composite materials.

CN118639434BActive Publication Date: 2024-12-03HUAIAN JINLIDA PACKAGE CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411112641.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-12-03
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The strength and impact resistance of existing high-strength composite fiber materials are poor, making it difficult to meet certain application needs.

Method used

By sonicating the coconut fibers and soaking them in the modified solution, using fluoride and silane compounds, the modifier in the modified solution reacts with the fiber surface to enhance the bond strength and interface bond between the fibers and the matrix material. High-strength composite fiber materials are prepared by hot press forming process.

Benefits of technology

It significantly improves the strength and tensile properties of composite fiber materials, enhances the interface combination between fiber and matrix materials, improves the overall strength and impact resistance of composite fiber sheets, and is relatively low in cost, and is suitable for the manufacturing of composite material products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a high-strength composite fiber material and its application, belonging to the technical field of organic polymer compounds. The method comprises the following steps: first, sodium fluoride and titanium aluminum carbide are added to hydrochloric acid for reaction, and then a solid is obtained by centrifugation and ultrasonic treatment. Next, coconut shell fiber is pretreated and mixed with the prepared modified solution to finally obtain a high-strength composite fiber material. The material is applied to the preparation of composite material boards. Compared with the prior art, the high-strength composite fiber material prepared by the invention has better strength characteristics, can play a reinforcing role in the composite fiber board, so that the composite fiber board has higher strength and tensile properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic polymer compounds, and in particular to a high-strength composite fiber material and application thereof. Background Art

[0002] A high-strength composite fiber material is a composite material composed of different types of fibers or different materials. This material combines fibers with different materials to make full use of their respective advantages to provide excellent strength, stiffness and durability.

[0003] The following are some common high-strength composite fiber materials and existing technologies for their applications: Carbon fiber is a high-strength, lightweight fiber material that is used in combination with different matrix materials (such as epoxy resin, polymer, etc.) to form high-strength composite materials. Carbon fiber composites are widely used in aerospace, automotive industry, sports equipment and construction. Glass fiber has high strength and stiffness and excellent electrical insulation properties. Glass fiber composites are widely used in construction, automotive industry, shipbuilding, wind energy and storage tanks. Aramid fiber is a high-strength, high-modulus synthetic fiber with excellent tensile strength and heat resistance. Aramid fiber composites are often used in bulletproof vests, aerospace, shipbuilding, sports equipment and automotive industries. Natural fibers (such as bamboo fiber, hemp fiber, wood fiber, etc.) are combined with polymer matrix materials to form natural fiber composites. This material has low cost, good renewability and low density, and is widely used in construction, furniture, packaging and automotive industries. Metal matrix composites combine metal matrix with fiber materials (such as carbon fiber, ceramic fiber, etc.) to provide high strength, high stiffness and heat resistance. Metal matrix composites are widely used in aerospace, automotive industry and military fields.

[0004] The application fields of these high-strength composite fiber materials include aerospace, automotive industry, construction, sports equipment, bulletproof vests, shipbuilding and storage tanks, etc. These materials play an important role in improving product performance, reducing weight, saving energy and protecting the environment, as well as improving safety.

[0005] China's authorized invention patent CN104441190B discloses a composite fiberboard material and its preparation method and use, wherein the composite fiberboard material includes wood cellulose, bamboo scraps, peanut shells, wheat bran, coconut shell fiber, urea-formaldehyde resin, bisphenol S epoxy resin, and 1,4-butene glycol. The fiberboard material preparation method includes the following steps: (1) crushing the raw materials; (2) drying the raw materials after grinding in step (1); (3) taking wood cellulose, bamboo scraps, peanut shells, wheat bran, and coconut shell fiber, and mechanically mixing them uniformly; (4) adding urea-formaldehyde resin, bisphenol S epoxy resin, and 1,4-butene glycol to the powder raw materials in step (3), and stirring until uniform; (5) pressurizing the fiberboard substrate material in step (4) in a mold for molding. However, the strength and impact resistance of the composite fiberboard material prepared by the invention are poor. Summary of the invention

[0006] In view of the deficiencies in the prior art, the technical problem to be solved by the present invention is to provide a high-strength composite fiber material with high strength and impact resistance and application thereof.

[0007] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:

[0008] A method for preparing a high-strength composite fiber material is as follows, in parts by weight:

[0009] Step 1, add 1 to 3 parts of fluoride to 30 to 50 parts of 5 to 10 mol / L hydrochloric acid, stir for 8 to 12 minutes, then add 1 to 3 parts of titanium aluminum carbide, stir the reaction mixture at 200 to 500 rpm at 30 to 40 ° C for 20 to 30 hours, collect the suspension and wash with water until the pH value of the supernatant is 5.5 to 6.5, then centrifuge at 3000 to 5000 rpm for 1 to 5 minutes, collect the sediment, and treat the sediment with ultrasound for 1 to 3 hours under nitrogen protection in an ice bath, the ultrasound treatment power is 100 to 300 W, the ultrasound treatment frequency is 20 to 60 kHz, and then centrifuge at 4000 to 6000 rpm for 10 to 40 minutes to obtain a solid, and add water to prepare a 2 to 8 mg / mL modified solution;

[0010] Step 2, ultrasonically treat the coconut shell fiber in water containing ozone at a concentration of 6-10 ppm for 5-15 minutes, then take out the coconut shell fiber, wash it with water for 20-40 minutes, and dry it at 50-70°C for 20-30 hours to obtain pretreated fiber, put 4-8 parts of the pretreated fiber into 500-700 parts of the modified solution prepared in step 1, stir it for 1-3 hours under nitrogen protection at room temperature, wash it with water 1-3 times, and then soak it in 400-600 parts of silane compound aqueous solution for 8-12 minutes, finally take out the fiber, and vacuum dry it at 50-70°C for 8-15 hours to obtain a high-strength composite fiber material.

[0011] The fluoride is at least one of sodium fluoride and lithium fluoride.

[0012] The concentration of the silane compound aqueous solution is 1-5 wt %.

[0013] The silane compound is at least one of N-aminoethyl-3-aminopropylmethyldimethoxysilane, 3-(dimethylethoxysilyl)-propane, 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, and γ-aminopropylmethyldiethoxysilane.

[0014] An application of a high-strength composite fiber material, the application is to use the high-strength composite fiber material to manufacture a composite fiber board.

[0015] The composite fiber board comprises the following ingredients in parts by weight: 30-40 parts of wood cellulose, 5-15 parts of bamboo fiber, 1-3 parts of hydroxypropyl starch, 6-10 parts of wheat bran, 10-20 parts of high-strength composite fiber material, 1-3 parts of reinforcing agent, 4-6 parts of plasticizer, and 20-30 parts of water-based bonding glue.

[0016] The preparation method of the composite fiber board is as follows:

[0017] S1. Weigh each raw material according to weight, crush wood cellulose, bamboo fiber and wheat bran, and pass through a 200-400 mesh sieve; then dry at 35-45° C. for 3-8 hours to obtain a powder;

[0018] S2. Add the high-strength composite fiber material and reinforcing agent to the powder prepared in step S1, tumble the mixture for 20 to 40 minutes under the action of airflow, and discharge the mixture to obtain a composite material; evenly mix the composite material with hydroxypropyl starch, plasticizer, and water-based bonding glue, and then inject the mixed material into a mold and hot-press it into a plate. After the material is injected into the mold, heat it to 60 to 70° C. and keep it warm for 10 to 20 minutes; then heat it to 70 to 80° C. and pressurize it for 5 to 10 minutes at a pressure of 60 to 90 MPa, and open the mold to obtain a composite fiber plate.

[0019] The reinforcing agent is at least one of silicon dioxide nanoparticles and carbon fibers.

[0020] The plasticizer is at least one of dibutyl phthalate and epoxy resin.

[0021] The role of each substance in the preparation of high-strength composite fiber materials:

[0022] Sodium fluoride: The addition of sodium fluoride can promote the reaction in the subsequent steps and help prepare the modified solution.

[0023] Hydrochloric acid: Hydrochloric acid provides a reaction medium and reacts with sodium fluoride to form hydrogen fluoride, which may react with titanium aluminum carbide to form a surface modifier.

[0024] Titanium aluminum carbide: Titanium aluminum carbide is a carbide that may react with hydrogen fluoride when added to hydrochloric acid to form a surface modifier for improving the interfacial bonding strength between the fiber and the matrix material.

[0025] Water: used to wash the suspension and collect the precipitate.

[0026] Ultrasonic treatment: Ultrasonic treatment can promote better mixing and dispersion of modifier and precipitate, which is beneficial to improve the performance of fiber.

[0027] Coconut shell fiber: After ultrasonic treatment, washing and drying, coconut shell fiber becomes pre-treated fiber, providing basic fiber material for subsequent steps.

[0028] Modified solution: prepared from the precipitate in step S1, wherein the modifier reacts with the fiber surface to enhance the bonding strength between the fiber and the matrix material and the fiber strength.

[0029] N-aminoethyl-3-aminopropylmethyldimethoxysilane: It can react chemically with the fiber surface to enhance the interfacial bonding strength between the fiber and the matrix material and the fiber strength, and can also improve the hydrophilicity of the fiber.

[0030] In the application of high-strength composite fiber materials:

[0031] Lignocellulosic material, bamboo fiber and wheat bran: After being crushed and dried, these fiber materials become the matrix materials for preparing composite materials, providing structural support for the composite materials and increasing the strength of the materials.

[0032] Carbon fiber: used as an additive to enhance the strength and rigidity of composite materials.

[0033] Hydroxypropyl starch, epoxy resin and water-based laminating glue: These materials are used to mix and prepare adhesives, which help to bind fibers and additives and provide overall performance of the material.

[0034] Mould and hot press: Through the mould and hot press process, the mixed materials are shaped and cured to form composite fiber sheets.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] 1) The present invention soaks the coconut shell fiber in a modification solution after ultrasonic treatment and pretreatment, so that the fiber surface is better combined with the modifier, and the strength and tensile properties of the fiber are enhanced, so that the high-strength composite fiber material finally prepared has better strength characteristics.

[0037] 2) In the preparation process of the present invention, by fully mixing and soaking the fiber with the modified solution, N-aminoethyl-3-aminopropylmethyldimethoxysilane can chemically react with the fiber surface to form a reinforced interface bond, thereby improving the bonding strength between the fiber and the matrix material.

[0038] 3) The present invention uses common fiber materials, such as coconut shell fiber, wood cellulose, bamboo fiber, etc., and improves their performance through modification. These raw materials are relatively easy to obtain and relatively low in cost, making the preparation process more cost-effective.

[0039] 4) The high-strength composite fiber material prepared by the present invention can be widely used in the manufacture of composite products, such as plates, components, etc. By mixing with other additives (such as carbon fiber, epoxy resin, etc.), it can play a reinforcing role in the composite material, so that the composite fiber plate has higher strength and tensile properties. DETAILED DESCRIPTION

[0040] Main sources of substances:

[0041] Titanium aluminum carbide: Shanghai Yuanye Biotechnology Co., Ltd., product number: T27062.

[0042] Coconut shell fiber: Guangzhou Yousuda Trading Co., Ltd., item number: AL-631802263247.

[0043] Lignocellulose: Zhengzhou Xinke Chemical Products Co., Ltd., catalog number: 58796-23.

[0044] Bamboo fiber: Lu'an Xingzhu New Material Technology Co., Ltd., model: ZF200.

[0045] Wheat bran: Lingshou County Taizhen Mineral Products Processing Factory, item number: Q-4.

[0046] Carbon fiber: Hangzhou Gaoke Composite Materials Co., Ltd., item number: CF.

[0047] Epoxy resin: Shenzhen Yoshida Chemical Co., Ltd., item number: F0707.

[0048] Water-based laminating glue: Dongguan Mikai Waterproof Decoration New Materials Co., Ltd., item number: 1840.

[0049] Example 1

[0050] A method for preparing a high-strength composite fiber material is as follows:

[0051] Step 1, adding 2g of sodium fluoride to 40g of 8mol / L hydrochloric acid, stirring for 10min, then adding 2g of titanium aluminum carbide, stirring the reaction mixture at 400rpm at 35°C for 24h, collecting the suspension and washing with water until the pH value of the supernatant is 6, then centrifuging at 4000rpm for 3min, collecting the sediment, and treating the sediment with ultrasound for 2h under nitrogen protection in an ice bath, with an ultrasound power of 200W and an ultrasound frequency of 40kHz, and then centrifuging at 5000rpm for 30min to obtain a solid, and adding water to prepare a 5mg / mL modified solution;

[0052] Step 2, ultrasonically treating the coconut shell fiber in water containing ozone at a concentration of 8 ppm for 10 minutes, then taking out the coconut shell fiber, washing it with water for 30 minutes, and drying it at 60°C for 24 hours to obtain pretreated fiber, placing 6 g of the pretreated fiber into 600 g of the modified solution prepared in step 1, stirring it under nitrogen protection at room temperature for 2 hours, washing it with water three times, and then soaking it in 500 g of a 3 wt% aqueous solution of N-aminoethyl-3-aminopropylmethyldimethoxysilane for 10 minutes, and finally taking out the fiber, and vacuum drying it at 60°C for 12 hours to obtain a high-strength composite fiber material;

[0053] The applications of the high-strength composite fiber material are as follows:

[0054] S1, 35kg of wood cellulose, 10kg of bamboo fiber, and 8kg of wheat bran were crushed and passed through a 300-mesh sieve; then dried at 40°C for 5h to obtain a powder;

[0055] S2. Add 15 kg of the high-strength composite fiber material and 2 kg of carbon fiber to the powder prepared in step S1, tumble the mixture for 30 minutes under the action of airflow, and discharge the mixture to obtain a composite material; mix the composite material with 2 kg of hydroxypropyl starch, 5 kg of epoxy resin, and 25 kg of water-based bonding glue, and then inject the mixed material into a mold and hot-press it into a plate. After the material is injected into the mold, heat it to 65° C. and keep it warm for 15 minutes; then heat it to 75° C. and pressurize it for 8 minutes at a pressure of 80 MPa. Open the mold to obtain a composite fiber plate.

[0056] Example 2

[0057] A method for preparing a high-strength composite fiber material is as follows:

[0058] Step 1, add 2g of lithium fluoride to 40g of 8mol / L hydrochloric acid, stir for 10min, then add 2g of titanium aluminum carbide, stir the reaction mixture at 400rpm at 35°C for 24h, collect the suspension and wash with water until the pH value of the supernatant is 6, then centrifuge at 4000rpm for 3min, collect the sediment, and treat the sediment with ultrasound for 2h under nitrogen protection in an ice bath, the ultrasound treatment power is 200W, the ultrasound treatment frequency is 40kHz, and then centrifuge at 5000rpm for 30min to obtain a solid, and add water to prepare a 5mg / mL modified solution;

[0059] Step 2, ultrasonically treating the coconut shell fiber in water containing ozone at a concentration of 8 ppm for 10 minutes, then taking out the coconut shell fiber, washing it with water for 30 minutes, and drying it at 60°C for 24 hours to obtain pretreated fiber, placing 6 g of the pretreated fiber into 600 g of the modified solution prepared in step 1, stirring it under nitrogen protection at room temperature for 2 hours, washing it with water three times, and then soaking it in 500 g of a 3 wt% aqueous solution of N-aminoethyl-3-aminopropylmethyldimethoxysilane for 10 minutes, and finally taking out the fiber, and vacuum drying it at 60°C for 12 hours to obtain a high-strength composite fiber material;

[0060] Example 3

[0061] A method for preparing a high-strength composite fiber material is as follows:

[0062] Step 1, adding 2g of sodium fluoride to 40g of 8mol / L hydrochloric acid, stirring for 10min, then adding 2g of titanium aluminum carbide, stirring the reaction mixture at 400rpm at 35°C for 24h, collecting the suspension and washing with water until the pH value of the supernatant is 6, then centrifuging at 4000rpm for 3min, collecting the sediment, and treating the sediment with ultrasound for 2h under nitrogen protection in an ice bath, with an ultrasound power of 200W and an ultrasound frequency of 40kHz, and then centrifuging at 5000rpm for 30min to obtain a solid, and adding water to prepare a 5mg / mL modified solution;

[0063] Step 2, ultrasonically treating the coconut shell fiber in water containing ozone at a concentration of 8 ppm for 10 minutes, then taking out the coconut shell fiber, washing it with water for 30 minutes, and drying it at 60°C for 24 hours to obtain pretreated fiber, placing 6 g of the pretreated fiber into 600 g of the modified solution prepared in step 1, stirring it under nitrogen protection at room temperature for 2 hours, washing it with water three times, and then soaking it in 500 g of a 3 wt% 3-(dimethylethoxysilyl) n-propane aqueous solution for 10 minutes, and finally taking out the fiber, and vacuum drying it at 60°C for 12 hours to obtain a high-strength composite fiber material;

[0064] Example 4

[0065] A method for preparing a high-strength composite fiber material is as follows:

[0066] Step 1, adding 2g of sodium fluoride to 40g of 8mol / L hydrochloric acid, stirring for 10min, then adding 2g of titanium aluminum carbide, stirring the reaction mixture at 400rpm at 35°C for 24h, collecting the suspension and washing with water until the pH value of the supernatant is 6, then centrifuging at 4000rpm for 3min, collecting the sediment, and treating the sediment with ultrasound for 2h under nitrogen protection in an ice bath, with an ultrasound power of 200W and an ultrasound frequency of 40kHz, and then centrifuging at 5000rpm for 30min to obtain a solid, and adding water to prepare a 5mg / mL modified solution;

[0067] Step 2, ultrasonically treating the coconut shell fiber in water containing ozone at a concentration of 8 ppm for 10 minutes, then taking out the coconut shell fiber, washing it with water for 30 minutes, and drying it at 60°C for 24 hours to obtain pretreated fiber, putting 6 g of the pretreated fiber into 600 g of the modified solution prepared in step 1, stirring it under nitrogen protection at room temperature for 2 hours, washing it with water three times, and then soaking it in 500 g of a 3 wt% 3-aminopropyltriethoxysilane aqueous solution for 10 minutes, finally taking out the fiber, and vacuum drying it at 60°C for 12 hours to obtain a high-strength composite fiber material;

[0068] Example 5

[0069] A method for preparing a high-strength composite fiber material is as follows:

[0070] Step 1, adding 2g of sodium fluoride to 40g of 8mol / L hydrochloric acid, stirring for 10min, then adding 2g of titanium aluminum carbide, stirring the reaction mixture at 400rpm at 35°C for 24h, collecting the suspension and washing with water until the pH value of the supernatant is 6, then centrifuging at 4000rpm for 3min, collecting the sediment, and treating the sediment with ultrasound for 2h under nitrogen protection in an ice bath, with an ultrasound power of 200W and an ultrasound frequency of 40kHz, and then centrifuging at 5000rpm for 30min to obtain a solid, and adding water to prepare a 5mg / mL modified solution;

[0071] Step 2, ultrasonically treating the coconut shell fiber in water containing ozone at a concentration of 8 ppm for 10 minutes, then taking out the coconut shell fiber, washing it with water for 30 minutes, and drying it at 60°C for 24 hours to obtain pretreated fiber, putting 6 g of the pretreated fiber into 600 g of the modified solution prepared in step 1, stirring it under nitrogen protection at room temperature for 2 hours, washing it with water three times, and then soaking it in 500 g of a 3 wt% 3-aminopropyltrimethoxysilane aqueous solution for 10 minutes, finally taking out the fiber, and vacuum drying it at 60°C for 12 hours to obtain a high-strength composite fiber material;

[0072] Comparative Example 1

[0073] A method for preparing a high-strength composite fiber material is as follows:

[0074] Step 1, adding 2g of sodium fluoride to 40g of 8mol / L hydrochloric acid, stirring for 10min, then adding 2g of titanium aluminum carbide, stirring the reaction mixture at 400rpm at 35°C for 24h, collecting the suspension and washing with water until the pH value of the supernatant is 6, then centrifuging at 4000rpm for 3min, collecting the sediment, and treating the sediment with ultrasound for 2h under nitrogen protection in an ice bath, with an ultrasound power of 200W and an ultrasound frequency of 40kHz, and then centrifuging at 5000rpm for 30min to obtain a solid, and adding water to prepare a 5mg / mL modified solution;

[0075] Step 2, ultrasonically treating the coconut shell fiber in water containing ozone at a concentration of 8 ppm for 10 minutes, then taking out the coconut shell fiber, washing it with water for 30 minutes, and drying it at 60°C for 24 hours to obtain pretreated fiber, placing 6 g of the pretreated fiber into 600 g of the modified solution prepared in step 1, stirring it under nitrogen protection at room temperature for 2 hours, washing it with water three times, and then soaking it in 500 g of a 3 wt% γ-aminopropylmethyldiethoxysilane aqueous solution for 10 minutes, and finally taking out the fiber, and vacuum drying it at 60°C for 12 hours to obtain a high-strength composite fiber material;

[0076] Comparative Example 2

[0077] A method for preparing a high-strength composite fiber material is as follows:

[0078] Step 1, adding 2g of sodium fluoride to 40g of 8mol / L hydrochloric acid, stirring for 10min, then adding 2g of titanium aluminum carbide, stirring the reaction mixture at 400rpm at 35°C for 24h, collecting the suspension and washing with water until the pH value of the supernatant is 6, then centrifuging at 4000rpm for 3min, collecting the sediment, and treating the sediment with ultrasound for 2h under nitrogen protection in an ice bath, with an ultrasound power of 200W and an ultrasound frequency of 40kHz, and then centrifuging at 5000rpm for 30min to obtain a solid, and adding water to prepare a 5mg / mL modified solution;

[0079] Step 2, ultrasonically treating the coconut shell fiber in water containing ozone at a concentration of 8 ppm for 10 minutes, then taking out the coconut shell fiber, washing it with water for 30 minutes, and drying it at 60°C for 24 hours to obtain pretreated fiber, putting 6 g of the pretreated fiber into 600 g of the modified solution prepared in step 1, stirring it under nitrogen protection at room temperature for 2 hours, washing it with water three times, and then soaking it in 500 g of a 1wt% aqueous solution of N-aminoethyl-3-aminopropylmethyldimethoxysilane for 10 minutes, and finally taking out the fiber, and vacuum drying it at 60°C for 12 hours to obtain a high-strength composite fiber material;

[0080] Comparative Example 3

[0081] A method for preparing a high-strength composite fiber material is as follows:

[0082] Step 1, adding 2g of sodium fluoride to 40g of 8mol / L hydrochloric acid, stirring for 10min, then adding 2g of titanium aluminum carbide, stirring the reaction mixture at 400rpm at 35°C for 24h, collecting the suspension and washing with water until the pH value of the supernatant is 6, then centrifuging at 4000rpm for 3min, collecting the sediment, and treating the sediment with ultrasound for 2h under nitrogen protection in an ice bath, with an ultrasound power of 200W and an ultrasound frequency of 40kHz, and then centrifuging at 5000rpm for 30min to obtain a solid, and adding water to prepare a 5mg / mL modified solution;

[0083] Step 2, ultrasonically treating the coconut shell fiber in water containing ozone at a concentration of 8 ppm for 10 minutes, then taking out the coconut shell fiber, washing it with water for 30 minutes, and drying it at 60°C for 24 hours to obtain pretreated fiber, putting 6 g of the pretreated fiber into 600 g of the modified solution prepared in step 1, stirring it under nitrogen protection at room temperature for 2 hours, washing it with water three times, and then soaking it in 500 g of a 5wt% aqueous solution of N-aminoethyl-3-aminopropylmethyldimethoxysilane for 10 minutes, finally taking out the fiber, and vacuum drying it at 60°C for 12 hours to obtain a high-strength composite fiber material;

[0084] Comparative Example 4

[0085] A method for preparing a composite fiber board is as follows:

[0086] Step 1, 35kg of wood cellulose, 10kg of bamboo fiber, and 8kg of wheat bran are crushed and passed through a 300-mesh sieve; then dried at 40° C. for 5 hours to obtain a powder;

[0087] Step 2, add 15kg coconut shell fiber and 2kg carbon fiber to the powder prepared in step S1, tumble and mix for 30 minutes under the action of airflow, and discharge to obtain a composite material; mix the composite material with 2kg hydroxypropyl starch, 5kg epoxy resin, and 25kg water-based bonding glue, and then inject the mixed material into a mold and hot press it into a plate. After the material is injected into the mold, heat it to 65°C and keep it warm for 15 minutes; then heat it to 75°C, pressurize it for 8 minutes, and the pressure is 80MPa. The composite fiber plate is obtained by opening the mold.

[0088] Test Example 1

[0089] Mechanical properties test

[0090] The composite fiber board samples prepared in the embodiments and comparative examples were tested for mechanical properties with a thickness of 1.2 mm. The test method adopted GB / T1447-2005 "Test method for tensile properties of fiber reinforced plastics". The initial load was 50 N, the modulus rate was set to 2 mm / min, the strength rate was 5 mm / min, and 5 specimens were tested for each group of samples. The average value was then taken. The test results are shown in Table 1.

[0091] Table 1 Mechanical properties test results

[0092]

[0093] Test Example 2

[0094] Notched impact strength test

[0095] The composite fiber board samples prepared in the embodiments and comparative examples and having a thickness of 1.2 mm were subjected to a notched impact strength test using an cantilever beam impact test method. Five specimens were tested for each group of samples, and the average value was taken. The test results are shown in Table 2.

[0096] Table 2 Notched impact strength test results

[0097]

[0098] It can be seen from the test data in Table 1 and Table 2 that the composite fiber board prepared in Example 1 of the present invention has better effects in terms of mechanical properties and notched impact strength.

[0099] In the preparation method, sodium fluoride is used as a modifier for coconut shell fiber. Compared with the use of lithium fluoride, sodium fluoride can improve the interface bonding between coconut shell fiber and matrix, enhance the bonding force between fiber and matrix, thereby improving the strength and stiffness of the composite material. Sodium fluoride modification can improve the hydrophilicity of coconut shell fiber, making it easier to wet and bond well with the matrix. This helps to reduce the gap between fiber and matrix and improve the physical bonding ability between fiber and matrix. Sodium fluoride modification can promote the densification of microstructure at the fiber / matrix interface, increase the constraint pressure on the fiber, thereby improving the energy consumption and friction performance of the fiber during the stretching process. Compared with lithium fluoride, sodium fluoride is more competitive in cost, so it may be more economical in industrial applications.

[0100] The present invention uses N-aminoethyl-3-aminopropylmethyldimethoxysilane to modify the composite fiber. Compared with other silane modifiers, N-aminoethyl-3-aminopropylmethyldimethoxysilane modification can enhance the mechanical properties of the composite fiber board, including strength, stiffness and toughness. By forming a uniform and continuous film at the fiber / matrix interface, the interface bonding is enhanced, and the physical bonding between the fiber and the matrix is ​​improved, thereby effectively transferring the load, preventing interface peeling and fiber breakage, and improving the overall strength of the composite fiber board. The notched impact strength of the composite fiber board can also be improved. The introduction of the modifier can improve the interface bonding between the fiber and the matrix, enhance the bonding strength of the interface, thereby effectively preventing crack propagation and notch sensitivity, and improving the impact resistance of the material.

Claims

1. A method for preparing a high-strength composite fiber material, characterized in that: The method is as follows, in parts by weight: Step 1, add 1 to 3 parts of fluoride to 30 to 50 parts of 5 to 10 mol / L hydrochloric acid, stir for 8 to 12 minutes, then add 1 to 3 parts of titanium aluminum carbide, stir the reaction mixture at 200 to 500 rpm at 30 to 40 ° C for 20 to 30 hours, collect the suspension and wash with water until the pH value of the supernatant is 5.5 to 6.5, then centrifuge at 3000 to 5000 rpm for 1 to 5 minutes, collect the sediment, and treat the sediment with ultrasound for 1 to 3 hours under nitrogen protection in an ice bath, the ultrasound treatment power is 100 to 300 W, the ultrasound treatment frequency is 20 to 60 kHz, and then centrifuge at 4000 to 6000 rpm for 10 to 40 minutes to obtain a solid, and add water to prepare a 2 to 8 mg / mL modified solution; Step 2, ultrasonically treating the coconut shell fiber in water containing ozone at a concentration of 6-10 ppm for 5-15 minutes, then taking out the coconut shell fiber, washing it with water for 20-40 minutes, and drying it at 50-70° C. for 20-30 hours to obtain pretreated fiber, placing 4-8 parts of the pretreated fiber into 500-700 parts of the modified solution prepared in step 1, stirring it under nitrogen protection at room temperature for 1-3 hours, washing it with water for 1-3 times, and then immersing it in 400-600 parts of an aqueous solution of a silane compound for 8-12 minutes, and finally taking out the fiber, and vacuum drying it at 50-70° C. for 8-15 hours to obtain a high-strength composite fiber material; The fluoride is sodium fluoride; The concentration of the silane compound aqueous solution is 3wt%; The silane compound is N-aminoethyl-3-aminopropylmethyldimethoxysilane.

2. A high-strength composite fiber material, characterized in that: Prepared by the method described in claim 1.

3. An application of a high-strength composite fiber material, characterized in that: The application is to use the high-strength composite fiber material as claimed in claim 2 to manufacture composite fiber boards.

4. The use according to claim 3, characterized in that The composite fiber board comprises the following ingredients in parts by weight: 30-40 parts of wood cellulose, 5-15 parts of bamboo fiber, 1-3 parts of hydroxypropyl starch, 6-10 parts of wheat bran, 10-20 parts of high-strength composite fiber material, 1-3 parts of reinforcing agent, 4-6 parts of plasticizer, and 20-30 parts of water-based bonding glue.

5. The use according to claim 4, characterized in that The preparation method of the composite fiber board is as follows: S1. Weigh each raw material according to weight, crush wood cellulose, bamboo fiber and wheat bran, and pass through a 200-400 mesh sieve; then dry at 35-45° C. for 3-8 hours to obtain a powder; S2. Add the high-strength composite fiber material and reinforcing agent to the powder prepared in step S1, tumble the mixture for 20 to 40 minutes under the action of airflow, and discharge the mixture to obtain a composite material; evenly mix the composite material with hydroxypropyl starch, plasticizer, and water-based bonding glue, and then inject the mixed material into a mold and hot-press it into a plate. After the material is injected into the mold, heat it to 60 to 70° C. and keep it warm for 10 to 20 minutes; then heat it to 70 to 80° C. and pressurize it for 5 to 10 minutes at a pressure of 60 to 90 MPa, and open the mold to obtain a composite fiber plate.

6. The use according to claim 4 or 5, characterized in that The reinforcing agent is at least one of silicon dioxide nanoparticles and carbon fibers.

7. The use according to claim 4 or 5, characterized in that The plasticizer is at least one of dibutyl phthalate and epoxy resin.

Citation Information

Patent Citations

  • A kind of composite fiberboard material and its preparation method and use

    CN104441190B

  • Novel composite fiberboard material and novel manufacturing method and application thereof

    CN104441190A

  • Heat insulation antiseptic composite floor tile and preparation method thereof

    CN108456415A

  • Building composite board with good impact resistance and preparation method thereof

    CN111499296A

  • Preparation method of carbon nanotube composite transparent conductive film

    CN112652424A