Antibacterial diaper breathable bottom film

By passing corn stalk fibers through silver nitrate and ultrasonic treatment to form silver-carrying fibers, combined with 3-chloropropylmethyldimethoxysilane and chitosan, the problem of poor breathability of diaper sole cloth is solved, and the problem of poor breathability of diaper sole cloth is significantly improved. Improves antibacterial and breathable properties, is suitable for diapers, and improves user experience.

CN118649270BActive Publication Date: 2024-11-05FUJIAN MANSHANHONG NEW MATERIAL TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411143614.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-05
Estimated Expiration
2044-08-20

AI Technical Summary

Technical Problem

The existing diaper soles are poorly breathable and prone to bacterial growth, leading to skin sensitivity, and the domestic market generally uses more expensive non-woven fabrics, which affects the user experience.

Method used

Corn stalk fibers were soaked in silver nitrate solution and sonicated to form silver-carrying fibers, followed by nanosilver modification, and the combination of 3-chloropropylmethyldimethoxysilane and chitosan was used to form antibacterial fibers as diapers The material of the breathable base film improves antibacterial and breathable.

Benefits of technology

It significantly improves the antibacterial and breathable properties of the fiber, reduces the occurrence of allergies, and is suitable for children and adults, improving user comfort and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses an antibacterial diaper breathable bottom film, and relates to the technical field of sanitary products. The invention first uses corn straw fiber as a bottom film reinforcement material, first performs a pulping treatment with a silver nitrate solution, forms a silver ion layer on the fiber surface and inside, and preliminarily improves the antibacterial property of the fiber. On this basis, reduction forms nanosilver, and compared with the traditional single addition form, the combination of nanosilver and fiber is more firm, making the antibacterial property more durable, and then performs secondary impregnation modification, so that 3-chloropropylmethyldimethoxysilane is attached to the fiber surface, and chitosan is further introduced and grafted on the fiber surface to improve the antibacterial property of the fiber. The invention uses natural, low-sensitivity antibacterial substances such as straw fiber, nanosilver, and chitosan, while achieving high-efficiency antibacterial, can greatly reduce the occurrence of allergic phenomena, which is conducive to the use of children and adult diapers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sanitary products, in particular to an antibacterial diaper breathable bottom film. Background Art

[0002] Diapers are a commonly used sanitary product. Generally speaking, diapers are composed of three main parts: surface coating layer, absorbent core layer and base fabric. The base fabrics of many diapers abroad have been made of non-woven fabrics, which feel more comfortable, but due to the high price, the base fabrics of diapers in the domestic market are still mainly composed of membrane materials. According to market research, breathability, water absorption, comfort, dryness, safety and other factors are the five main factors people consider when buying diapers. Because urine is produced, the inside of the diaper is in a hot and humid environment for a long time. While the breathability is poor, it is easy to breed bacteria and cause skin sensitivity. Summary of the invention

[0003] The object of the present invention is to provide an antibacterial diaper breathable bottom film to solve the problems existing in the prior art.

[0004] In order to solve the above technical problems, the present invention provides the following technical solution: an antibacterial diaper breathable bottom film, comprising the following preparation steps:

[0005] (1) Soak corn straw fiber in silver nitrate solution for 6-8 hours, take it out, dry it at 60°C until the moisture content of the fiber is 50-70%, cut it into short pieces with a length of 0.5-2 cm, put it into a blade beater, and beat it vigorously for 3-5 minutes. Then add the composite solution with a mass of 0.1-0.3 times of the corn straw fiber, and continue beating it for 3-5 minutes. After ultrasonic treatment at 20-30kHz for 10-60 minutes, separate the solid and liquid, and dry it at 60°C for 24 hours to obtain silver-loaded fiber.

[0006] (2) Soaking the silver-loaded fiber in a 0.01 mol / L NaBH4 aqueous solution for 20-30 min, separating the solid from the liquid, and drying at 60°C for 8 h to obtain the nanosilver-modified fiber;

[0007] (3) Soak the nanosilver modified fiber in 1~5wt% 3-chloropropylmethyldimethoxysilane ethanol solution at 1g:5mL, let it stand for 2~4h, add chitosan solution, stir at 60rpm for 12h, filter, take the solid, rinse it with distilled water for 3 times, place it in a refrigerator, and freeze-dry it for 12h to obtain the antibacterial fiber;

[0008] (4) According to the weight percentage, 20-30 parts of antibacterial fiber, 50-60 parts of polylactic acid, 30-45 parts of terminal hydroxyl polystyrene and 0.1-1 part of antioxidant are extruded and granulated at 160-175°C by a twin-screw machine, hot-pressed into film by a flat vulcanizer, and then kept at 120°C for 30 minutes to obtain an antibacterial diaper breathable bottom film.

[0009] Furthermore, the silver nitrate solution in step (1) is a 0.01 mol / L silver nitrate aqueous solution.

[0010] Furthermore, the composite solution in step (1) comprises 0.01 mol / L sodium citrate aqueous solution and 0.1 mol / L hydrogen peroxide aqueous solution.

[0011] Furthermore, the ethanol in the 3-chloropropylmethyldimethoxysilane ethanol solution in step (3) is a 50 wt% ethanol aqueous solution.

[0012] Furthermore, in step (3), the mass ratio of 3-chloropropylmethyldimethoxysilane to chitosan is 0.5-5:1.

[0013] Furthermore, the preparation method of the chitosan solution in step (3) is: dispersing chitosan in a 10% by mass NaOH solution at a solid-liquid ratio of 1 g:30 mL, and stirring at 80 rpm for 8 h.

[0014] Furthermore, the relative molecular weight of the hydroxy-terminated polystyrene in step (4) is 20,000 to 70,000, and the molecular weight distribution index is 1.18.

[0015] Furthermore, the antioxidant in step (4) is catechol.

[0016] Furthermore, the working parameters of the flat vulcanizing press in step (4) are: temperature 190-240° C., pressure 5-10 MPa, and time 1-10 min.

[0017] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0018] The invention adopts corn stalk fiber as a base film reinforcement material, and firstly performs a pulping treatment with a silver nitrate solution. During the pulping process, the primary wall and the secondary wall are broken, silver ions enter, combine with hydroxyl groups, and are adsorbed on the surface of the fiber to form a silver ion layer, which preliminarily improves the antibacterial property of the fiber. Then, impregnation modification is performed to reduce the silver ions on the surface and inside to form nanosilver. Compared with the traditional single addition form, the combination of nanosilver and the fiber is more firm, making the antibacterial property more durable. Then, secondary impregnation modification is performed to attach 3-chloropropylmethyldimethoxysilane to the fiber surface, and on this basis, chitosan is introduced and grafted on the fiber surface by relying on the chlorine group of 3-chloropropylmethyldimethoxysilane, so as to further improve the antibacterial property of the fiber. The invention adopts natural, low-sensitivity antibacterial substances such as straw fiber, nanosilver, chitosan, etc., which can greatly reduce the occurrence of allergies while achieving high-efficiency antibacterial, and is conducive to the use of diapers for children and adults. DETAILED DESCRIPTION

[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] Example 1; (1) Soak corn stalk fiber in a 0.01 mol / L silver nitrate aqueous solution for 6 hours, take it out, dry it at 60°C until the fiber moisture content is 50%, cut it into a length of 0.5 cm, put it into a blade beater, and beat it vigorously for 4 minutes. Then add a composite solution 0.1 times the mass of the corn stalk fiber, the composite solution includes a 0.01 mol / L sodium citrate aqueous solution and a 0.1 mol / L hydrogen peroxide aqueous solution, continue to beat for 4 minutes, ultrasonically treat it at 25 kHz for 30 minutes, separate the solid and liquid, and dry it at 60°C for 24 hours to obtain silver-loaded fiber;

[0021] (2) Soaking the silver-loaded fiber in a 0.01 mol / L NaBH4 aqueous solution for 20 min, separating the solid from the liquid, and drying at 60 °C for 8 h to obtain the nano-silver modified fiber;

[0022] (3) Soaking the nanosilver modified fiber in a 1wt% 3-chloropropylmethyldimethoxysilane ethanol solution at a ratio of 1g:5mL, wherein the ethanol in the 3-chloropropylmethyldimethoxysilane ethanol solution is a 50wt% ethanol aqueous solution, and after standing for 2h, adding chitosan solution, wherein the mass ratio of 3-chloropropylmethyldimethoxysilane to chitosan is 1.2:1, stirring at 60rpm for 12h, filtering, taking the solid, rinsing it with distilled water for 3 times, placing it in a refrigerator, and freeze-drying it for 12h to obtain the antibacterial fiber; the preparation method of the chitosan solution is: dispersing chitosan in a 10wt% NaOH solution at a solid-liquid ratio of 1g:30mL, and stirring at 80rpm for 8h;

[0023] (4) According to the mass percentage, 20 parts of antibacterial fiber, 50 parts of polylactic acid, 30 parts of terminal hydroxyl polystyrene and 0.1 parts of catechol are extruded and granulated at 175°C by a twin-screw machine, and then hot-pressed into a film by a flat-plate vulcanizer, and then kept at 120°C for 30 minutes to obtain an antibacterial diaper breathable bottom film; the working parameters of the flat-plate vulcanizer are: temperature 200°C, pressure 10MPa, time 5 minutes.

[0024] Example 2; (1) Soak corn stalk fiber in a 0.01 mol / L silver nitrate aqueous solution for 7 hours, take it out, dry it at 60°C until the fiber moisture content is 60%, cut it into 1 cm in length, put it into a blade beater, and beat it vigorously for 4 minutes. Then add a composite solution 0.2 times the mass of the corn stalk fiber, the composite solution includes a 0.01 mol / L sodium citrate aqueous solution and a 0.1 mol / L hydrogen peroxide aqueous solution, continue to beat for 4 minutes, ultrasonically treat it at 25 kHz for 30 minutes, separate the solid and liquid, and dry it at 60°C for 24 hours to obtain silver-loaded fiber;

[0025] (2) Soaking the silver-loaded fiber in a 0.01 mol / L NaBH4 aqueous solution for 25 min, separating the solid from the liquid, and drying at 60°C for 8 h to obtain the nanosilver-modified fiber;

[0026] (3) Soaking the nanosilver modified fiber in a 3wt% 3-chloropropylmethyldimethoxysilane ethanol solution at a ratio of 1g:5mL, wherein the ethanol in the 3-chloropropylmethyldimethoxysilane ethanol solution is a 50wt% ethanol aqueous solution, and after standing for 3 hours, adding chitosan solution, wherein the mass ratio of 3-chloropropylmethyldimethoxysilane to chitosan is 1.2:1, stirring at 60rpm for 12 hours, filtering, taking the solid, rinsing it with distilled water for 3 times, placing it in a refrigerator, and freeze-drying it for 12 hours to obtain the antibacterial fiber; the preparation method of the chitosan solution is: dispersing chitosan in a 10% NaOH solution at a solid-liquid ratio of 1g:30mL, and stirring at 80rpm for 8 hours;

[0027] (4) According to the mass percentage, 25 parts of antibacterial fiber, 55 parts of polylactic acid, 40 parts of terminal hydroxyl polystyrene and 0.5 parts of catechol are extruded and granulated at 175°C by a twin-screw machine, and then hot-pressed into a film by a flat-plate vulcanizer, and then kept at 120°C for 30 minutes to obtain an antibacterial diaper breathable bottom film; the working parameters of the flat-plate vulcanizer are: temperature 200°C, pressure 10MPa, time 5 minutes.

[0028] Example 3; (1) Soak corn stalk fiber in a 0.01 mol / L silver nitrate aqueous solution for 8 h, take it out, dry it at 60°C until the fiber moisture content is 70%, cut it into 2 cm in length, put it into a blade beater, and beat it vigorously for 4 min. Then add a composite solution 0.3 times the mass of the corn stalk fiber, the composite solution includes a 0.01 mol / L sodium citrate aqueous solution and a 0.1 mol / L hydrogen peroxide aqueous solution, continue to beat for 4 min, treat it ultrasonically at 25 kHz for 30 min, separate the solid and liquid, and dry it at 60°C for 24 h to obtain silver-loaded fiber;

[0029] (2) Soaking the silver-loaded fiber in a 0.01 mol / L NaBH4 aqueous solution for 30 min, separating the solid from the liquid, and drying at 60°C for 8 h to obtain the nanosilver-modified fiber;

[0030] (3) Soaking the nanosilver modified fiber in a 5wt% 3-chloropropylmethyldimethoxysilane ethanol solution at a ratio of 1g:5mL, wherein the ethanol in the 3-chloropropylmethyldimethoxysilane ethanol solution is a 50wt% ethanol aqueous solution, and after standing for 4 hours, adding chitosan solution, wherein the mass ratio of 3-chloropropylmethyldimethoxysilane to chitosan is 1.2:1, stirring at 60rpm for 12 hours, filtering, taking the solid, rinsing it with distilled water for 3 times, placing it in a refrigerator, and freeze-drying it for 12 hours to obtain the antibacterial fiber; the preparation method of the chitosan solution is: dispersing chitosan in a 10% NaOH solution at a solid-liquid ratio of 1g:30mL, and stirring at 80rpm for 8 hours;

[0031] (4) According to the mass percentage, 30 parts of antibacterial fiber, 60 parts of polylactic acid, 45 parts of terminal hydroxyl polystyrene and 1 part of catechol are extruded into granules by a twin-screw machine at 175°C, and then hot-pressed into films by a flat-plate vulcanizer, and then kept at 120°C for 30 minutes to obtain an antibacterial diaper breathable bottom film; the working parameters of the flat-plate vulcanizer are: temperature 200°C, pressure 10MPa, time 5 minutes.

[0032] Comparative Example 1: The difference between Comparative Example 1 and Example 2 is that no silver nitrate aqueous solution is added for pulping, and distilled water is used for pulping, and the remaining steps are the same as Example 2.

[0033] Comparative Example 2: The difference between Comparative Example 2 and Example 2 is that 3-chloropropylmethyldimethoxysilane ethanol solution is not added for modification treatment, and the remaining steps are the same as Example 2.

[0034] Comparative Example 3: The difference between Comparative Example 3 and Example 2 is that chitosan is not added, and the remaining steps are the same as Example 2.

[0035] Effect example

[0036] The films obtained in Examples 1 to 3 of the present invention and Comparative Examples 1 to 3 were subjected to performance tests, wherein the tensile strength and elongation at break were measured in accordance with GB / T1040-1992, the tensile speed was 50 mm / min, and the test results were averaged 5 times; the water vapor permeability was tested in accordance with GB / T1037, and the results are shown in Table 1 below:

[0037] Table 1

[0038]

[0039] From the comparison of the experimental data of the embodiment and the comparative example, it can be found that the present invention adopts corn straw fiber as the base film reinforcement material, and first performs a pulping treatment with a silver nitrate solution. During the pulping process, the primary wall and the secondary wall are broken, and silver ions enter, combine with hydroxyl groups, and are adsorbed to the surface of the fiber to form a silver ion layer, which preliminarily improves the antibacterial property of the fiber. Then, impregnation modification is performed to reduce the silver ions on the surface and inside to form nanosilver. Compared with the traditional single addition form, the combination of nanosilver and fiber is more firmly, making the antibacterial property more lasting. Then, a secondary impregnation modification is performed to attach 3-chloropropylmethyldimethoxysilane to the fiber surface, and on this basis, relying on the chlorine group of 3-chloropropylmethyldimethoxysilane, chitosan is introduced to be grafted on the fiber surface to further improve the antibacterial property of the fiber.

[0040] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. An antibacterial diaper breathable bottom film, characterized in that: The method comprises the following preparation steps: (1) Soak corn straw fiber in a 0.01 mol / L silver nitrate aqueous solution for 6-8 hours, take it out, dry it at 60°C until the moisture content of the fiber is 50-70%, cut it into short pieces to a length of 0.5-2 cm, put it into a blade beater, and vigorously beat it for 3-5 minutes, then add a composite solution of 0.1-0.3 times the mass of the corn straw fiber, continue to beat it for 3-5 minutes, treat it with ultrasound at 20-30 kHz for 10-60 minutes, separate the solid from the liquid, and dry it at 60°C for 24 hours to obtain silver-loaded fiber; the composite solution includes a 0.01 mol / L sodium citrate aqueous solution and a 0.1 mol / L hydrogen peroxide aqueous solution; (2) Soaking the silver-loaded fiber in a 0.01 mol / L NaBH4 aqueous solution for 20-30 min, separating the solid from the liquid, and drying at 60°C for 8 h to obtain the nanosilver-modified fiber; (3) Soaking the nanosilver modified fiber in a 1-5wt% 3-chloropropylmethyldimethoxysilane ethanol solution at a ratio of 1 g:5 mL, leaving it to stand for 2-4 hours, adding chitosan solution, stirring at 60 rpm for 12 hours, filtering, taking the solid, rinsing it with distilled water for 3 times, placing it in a refrigerator, and freeze-drying it for 12 hours to obtain the antibacterial fiber; the preparation method of the chitosan solution is as follows: dispersing chitosan in a 10% NaOH solution at a solid-liquid ratio of 1 g:30 mL, stirring at 80 rpm for 8 hours; (4) According to the weight percentage, 20-30 parts of antibacterial fiber, 50-60 parts of polylactic acid, 30-45 parts of terminal hydroxyl polystyrene and 0.1-1 part of antioxidant are extruded and granulated at 160-175°C by a twin-screw machine, hot-pressed into film by a flat vulcanizer, and then kept at 120°C for 30 minutes to obtain an antibacterial diaper breathable bottom film.

2. The antibacterial diaper breathable bottom film according to claim 1, characterized in that: The ethanol in the 3-chloropropylmethyldimethoxysilane ethanol solution in step (3) is a 50 wt % ethanol aqueous solution.

3. The antibacterial diaper breathable bottom film according to claim 1, characterized in that: The mass ratio of 3-chloropropylmethyldimethoxysilane to chitosan in step (3) is 0.5-5:

1.

4. The antibacterial diaper breathable bottom film according to claim 1, characterized in that: The relative molecular weight of the hydroxy-terminated polystyrene in step (4) is 20,000 to 70,000, and the molecular weight distribution index is 1.

18.

5. The antibacterial diaper breathable bottom film according to claim 1, characterized in that: The antioxidant in step (4) is catechol.

6. The antibacterial diaper breathable bottom film according to claim 1, characterized in that: The working parameters of the flat vulcanizing press in step (4) are: temperature 190-240° C., pressure 5-10 MPa, and time 1-10 min.

Citation Information

Patent Citations

  • Biological degradable gas-permeable membrane for paper diaper and preparation method of biological degradable gas-permeable membrane

    CN107083033A

  • Degradable antibacterial packaging film

    CN109401155A

  • Antibacterial breathable film capable of being composted and degraded as well as a preparation method and application of antibacterial breathable film

    CN113683872A

  • Antioxidant silver fiber fabric

    CN116556051A

  • Corn straw-based composite membrane material and preparation method thereof

    CN118085360A