A welding deformation correction and stress elimination method, device and numerical simulation method
Through the welding deformation correction and stress removal method of segmented pressurization and heating, combined with numerical simulation optimization process, the challenges in the orthopedic stress and heat treatment process in the welding deformation correction and stress removal process of austenitic stainless steel are solved, and efficient welding is achieved Part correction and stress relief improve the mechanical properties and process efficiency of the material.
Patent Information
- Application Number
- CN202411140612.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-20
AI Technical Summary
In the process of deformation correction and stress removal of austenitic stainless steel welding, the prior art has challenges in the introduction of orthopedic stress, newly introduced stress and heat treatment, and the cost and efficiency are low.
Using a welding deformation correction and stress removal method, the welded parts are subjected to six-step gradient section pressurization and heating through loading devices, upper and lower molds and heating blocks, stress relaxation is performed in combination with the creep effect, and the process is optimized through numerical simulation method. parameter.
It effectively reduces the requirements of orthopedic loads, reduces carbide precipitation, improves the hardness and tensile strength of the material, ensures the shape accuracy and mechanical properties of the welded parts, simplifies the process flow, and reduces costs.
Smart Images

Figure CN118650030B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of welding technology, and in particular to a welding deformation correction and stress elimination method, device and numerical simulation method. Background Art
[0002] When welding butt joint weldments of austenitic stainless steel, welding deformation may cause large or high-precision parts to deviate from the expected geometric tolerance requirements, or even cause gaps, misalignments or overlaps during subsequent assembly. Tensile residual stresses near the weld area increase the possibility of fatigue damage, stress corrosion cracking and brittle fracture. Local deformation correction and residual stress relief of weldments are important parts of the post-welding process. Common correction processes include mechanical hammering, flame correction and induction heating correction, but deformation and stress are symbiotic. If the correction force and temperature are not properly controlled, new internal stresses and harmful phases will be generated, and even the mechanical properties of the material will be reduced. Residual stress is usually eliminated by heat treatment and vibration, which requires multiple different process steps for welding deformation correction and residual stress relief, and the implementation process is relatively cumbersome. Heat treatment stress relief is the simplest and most effective method. In order to completely eliminate the residual stress of austenitic stainless steel after welding, a solid solution treatment of 950℃~1150℃ is generally selected, and water quenching is required to cool down, otherwise carbides will precipitate during slow cooling, but water quenching will also introduce new cooling stress. The cost of overall post-weld heat treatment of large welded parts is extremely high, and there are few engineering applications. In addition, the precipitation temperature of σ phase and carbide of austenitic stainless steel is about 600℃~950℃. When stress relief treatment is performed at this temperature, there will be risks of sensitization and intergranular corrosion. When stress relief treatment is performed at 400℃~600℃, if the holding time is too long, carbides will also precipitate between grains, but if the holding time is too short, the welding residual stress cannot be fully eliminated. When the temperature is lower than 400℃, the effect of eliminating welding residual stress is not obvious. In summary, when correcting the welding deformation of austenitic stainless steel, it is necessary to consider the newly introduced corrective stress, and when eliminating residual stress, it is necessary to pay attention to the dimensional stability during heat treatment and the mechanical properties of austenitic stainless steel. In addition, the implementation efficiency and cost requirements of engineering applications must also be taken into account. Summary of the invention
[0003] Based on this, it is necessary to provide a welding deformation correction and stress elimination method, device and numerical simulation method for the correction and stress elimination of austenitic stainless steel welding deformation, which may introduce new corrective stress or reduce mechanical properties when eliminating residual stress.
[0004] A welding deformation correction and stress relief method is used to correct deformation and relieve stress of a welded part with a maximum deformation range of 12 to 15 mm and made of austenitic stainless steel; the deformation correction and stress relief method comprises the following steps:
[0005] Provided is a welding deformation correction and stress relief device; the welding deformation correction and stress relief device comprises a loading device, an upper mold, a lower mold and at least two heating blocks;
[0006] The welded part is installed between the upper mold and the lower mold that cooperate with each other; a plurality of the heating blocks are connected to the upper and lower surfaces of the welded part, and are used to uniformly heat the welded part to a preset temperature; the loading device applies pressure on the upper mold to perform six-level gradient segmented pressurization on the welded part, and the displacements of the six levels of gradient are 2.4mm, 2.2mm, 2mm, 2mm, 2mm, and 1mm respectively, and the time for the upper mold to pressurize to each level of gradient displacement is 1 to 5min; after each level of gradient pressurization, the pressure and preset temperature of the gradient pressurization are maintained within 0.5 to 1h for pressure and heat preservation, so as to correct the deformation of the welded part and relax the stress of the welded part through the creep effect;
[0007] After the sixth level of gradient pressure and temperature preservation, the heating block stops heating the weldment and maintains the sixth level of gradient pressure until the weldment cools to room temperature.
[0008] As a preferred example, the preset temperature is 400-550° C.; the heating rate of the preset temperature is 100-300° C. / h.
[0009] As a preferred example, the mold stops heating the weldment and then cools it down at a rate of 100 to 300° C. / h until it is cooled to room temperature.
[0010] A welding deformation correction and stress relief device, which uses the welding deformation correction and stress relief method as described above to correct deformation and relieve stress on a welded part, the welding deformation correction and stress relief device comprising a loading device, an upper die, a lower die and at least two heating blocks;
[0011] The loading device is used to drive the upper mold and the lower mold to close the mold and pressurize;
[0012] The pressurizing surface of the upper mold and the pressurizing surface of the lower mold are arranged in parallel, and the pressurizing surfaces of the upper mold and the lower mold are both provided with a space-avoiding groove for accommodating the heating block;
[0013] The heating block is connected to the welding part and corresponds to the air avoidance groove; when the welding part is in the first to fourth stage segmented pressurization process, the heating block gradually enters the air avoidance groove and there is a gap with the inner bottom of the air avoidance groove; when the welding part is in the fifth and sixth stage segmented pressurization process, one side of the heating block contacts the inner bottom of the air avoidance groove, and the other side is flush with the notch of the air avoidance groove to expand the area of the pressurization surface of the upper mold and the lower mold.
[0014] As a preferred example, the heating block includes a heat-conducting block and a heating rod; the heat-conducting block is connected to the welding piece, and a hole is opened on the heat-conducting block, and the heating rod is installed in the hole.
[0015] As a preferred example, there are four heat-conducting blocks, two of which are located on the upper surface of the welding piece, and the other two are located on the lower surface of the welding piece, and the heat-conducting blocks located on the upper and lower sides of the welding piece are arranged one by one.
[0016] As a preferred example, a spring is commonly connected between the heat conductive blocks on the upper and lower surfaces of the weldment, and the spring is used to tighten the heat conductive blocks on the upper and lower surfaces of the weldment to each other so that the heat conductive blocks fit tightly against the surface of the weldment.
[0017] As a preferred example, the welding deformation correction and stress elimination device also includes two fixing blocks, and the two fixing blocks are respectively connected to the two ends of the lower mold; the weldment is fixed between the two fixing blocks by bolts.
[0018] A numerical simulation method for the whole process from welding to creep is provided, which performs numerical simulation on the welding deformation correction and stress relief method as described above, and the numerical simulation method comprises the following steps:
[0019] Sequential coupling technology is used in the welding process, first thermal analysis and then mechanical analysis to obtain welding stress, strain and deformation results;
[0020] Using data transfer technology, the analysis results during welding are imported into the creep analysis model for creep analysis;
[0021] The changes of welding deformation correction and residual stress relaxation during multi-stage creep aging are simulated based on the creep analysis model.
[0022] As a preferred example, the analysis during welding includes the following steps:
[0023] Establish a welding finite element analysis model and divide the welds into different layers; set material parameters, including elastic modulus, Poisson's ratio, plasticity, thermal conductivity, specific heat capacity, density, thermal expansion coefficient and latent heat at different temperatures; define the weld as a birth and death unit, and activate the welds layer by layer in sequence; define the heat dissipation model and ambient temperature; define boundary constraints and mobile heat source model; divide the model into grids and solve the results;
[0024] The data transfer technology is used to use the stress, strain, temperature and deformation results of welding as the initial state of creep analysis to perform deformation correction and stress relaxation simulation in the next step;
[0025] The creep analysis includes the following steps:
[0026] A contact model between the weldment and the mold is established; corresponding simulation parameters are set according to each level of displacement, loading time, stress relaxation time, preset temperature, heating rate, and cooling rate during the welding deformation correction and stress relief process, and creep constitutive parameters of the weldment are assigned.
[0027] The beneficial effects of the present invention are:
[0028] 1. The present invention corrects welding deformation in multiple times, which reduces the requirement for the tonnage of the correction load. After correction, short-term stress relaxation is performed at a medium temperature of 400-550°C. The creep characteristics of the material can better eliminate residual stress and reduce the amount of correction rebound. The modular heating of the heating block is adopted without the need for a large heating furnace, making it easy to implement local deformation correction and stress elimination of austenitic stainless steel weldments, especially large austenitic stainless steel weldments.
[0029] 2. In the implementation process of the present invention, a relatively fast heating rate and cooling rate, as well as short-term stress relaxation at medium temperature are used to reduce the precipitation of carbides, and by selecting an aging temperature of 400-550°C, the toughness of the material is basically not affected, but the hardness, yield strength and tensile strength limit can be slightly improved. In addition, the constraints of the upper and lower molds can reduce the thermal deformation caused by the heating and cooling processes, and ensure the shape accuracy of the austenitic stainless steel after correction.
[0030] 3. The present invention has developed a numerical simulation method for the entire process from welding to creep, including thermal-elastic-viscoplastic coupling, which matches the experimental process. It can reveal the changing laws of the temperature, stress, strain and deformation of the workpiece during the process, and plays an important role in optimizing the creep aging process method, predicting deformation correction and residual stress relaxation results. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 A schematic diagram of the structure of a welding deformation correction and stress relief device proposed in an embodiment;
[0032] Figure 2 It is a flow chart of the numerical simulation method of the whole process from welding to creep in the embodiment;
[0033] Figure 3 A schematic diagram of the structure and geometric parameters of a butt joint of an embodiment;
[0034] Figure 4 A schematic diagram of a simulation result of a butt joint welding process according to an embodiment;
[0035] Figure 5 Temperature variation curve of butt joint welding and creep process for example
[0036] Figure 6The deformation simulation result of the creep process of the butt joint of the embodiment;
[0037] Figure 7 The residual stress simulation result of the creep process of the butt joint of the embodiment;
[0038] Figure 8 is a deformation correction curve of the creep process of the butt joint in the embodiment;
[0039] Fig. 9 The residual stress relaxation curve of the weld center point during the creep process of the butt joint in the embodiment;
[0040] Fig.10 is the equivalent creep strain curve of the weld center point during the creep process of the butt joint in the embodiment;
[0041] Fig.11 is a comparison of the longitudinal stress of the butt joint of the embodiment before and after creep;
[0042] Fig.12 Comparison of transverse stress before and after creep of butt joints of the embodiments;
[0043] Fig.13 Comparison of deformation of butt joints before and after creep in the embodiments;
[0044] Fig.14 This is a metallographic diagram of the butt joint of the embodiment before creep;
[0045] Fig.15 This is the metallographic image of the butt joint after creep of the embodiment.
[0046] In the figure: 1. welding part; 2. loading device; 3. upper mold; 4. lower mold; 5. heat conducting block; 6. heating rod; 7. fixing block. DETAILED DESCRIPTION
[0047] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0048] It should be noted that when a component is referred to as being "mounted on" another component, it may be directly on the other component or there may be a central component. When a component is considered to be "set on" another component, it may be directly set on the other component or there may be a central component at the same time. When a component is considered to be "fixed to" another component, it may be directly fixed on the other component or there may be a central component at the same time.
[0049] It should be understood that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0050] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "or / and" used herein includes any and all combinations of one or more of the related listed items.
[0051] Please refer to Figure 1, this embodiment provides a welding deformation correction and stress relief device, which is used to implement the proposed welding deformation correction and stress relief method for austenitic stainless steel. The welding deformation correction and stress relief device includes a loading device 2, an upper mold 3, a lower mold 4, a fixed block 7 and at least two heating blocks. The loading device 2 can adopt a high-precision hydraulic press, which includes some components such as a frame and a cylinder, which will not be described in detail here. The loading device 2 is used to drive the upper mold 3 and the lower mold 4 to open and close. The upper mold 3 and the lower mold 4 are respectively installed at the moving end and the fixed end of the loading device 2. It should be noted that the pressurizing surface of the upper mold 3 and the pressurizing surface of the lower mold 4 are arranged in parallel, which are used to pressurize the two side surfaces of the weldment so that the surface of the weldment tends to be flat. The fixed block 7 is connected to both ends of the lower mold 4, which is used to fix the weldment 1. In this embodiment, during the implementation process, the weldment 1 is fixed between the upper mold 3 and the lower mold 4 of the loading device 2. At the same time, the weld of the weldment 1 has corresponding support constraints on the lower mold 4. The heating method adopts a method of setting heating blocks on the upper and lower surfaces of the weldment 1. Specifically, the heating block includes a heat conductive block 5 and a heating rod 6. To match this, an air avoidance groove needs to be provided on the upper mold 3 and the lower mold 4 to avoid interference with the heat conductive block 5. And there is a specific setting relationship between the heating block and the air avoidance groove: when the weldment 1 is in the first to fourth stage segmented pressurization process, the heating block gradually enters the air avoidance groove, and there is a gap with the inner bottom of the air avoidance groove. When the weldment 1 is in the fifth and sixth stage segmented pressurization process, one side of the heating block contacts the inner bottom of the air avoidance groove, and the other side is flush with the notch of the air avoidance groove, so that one side of the heating block also serves as a pressurization surface to expand the area of the pressurization surface of the upper mold 3 and the lower mold 4, and reduce the additional deformation of the weldment 1 caused by uneven surface force. A heating rod 6 is installed in the hole of the heat conductive block 5. The heating rod 6 is connected to a temperature controller. The temperature controller is equipped with a thermocouple. The thermocouple is used to detect the temperature of the weldment 1 and feed it back to the temperature controller for dynamic control of heating and heat preservation. Furthermore, a spring is commonly connected between the heat-conducting blocks 5 on the upper and lower surfaces of the weldment 1. The spring makes the heat-conducting blocks 5 on the upper and lower surfaces of the weldment 1 tighten with each other, so that the heat-conducting blocks 5 are closely fitted with the surface of the weldment 1 to ensure the heat transfer effect. Heat insulation cotton is arranged around the weldment 1 for external heat insulation and internal heat preservation. Among them, the upper mold 3, the lower mold 4, the fixed block 7 and the heat-conducting block 5 are preferably made of the same material as the weldment 1 to avoid contamination of the chemical composition of the material. The rigidity of the upper mold 3 and the lower mold 4 is much greater than that of the weldment 1. The fixed blocks 7 at both ends of the lower mold 4 can be set as a threaded drive structure. Bolts are used to move and clamp the weldment 1. In another embodiment, the heat-conducting blocks 5 and the heating rods 6 can be provided with multiple groups, which are correspondingly distributed on the upper and lower surfaces of the weldment 1 and fixed on both sides of the weld on the weldment 1.
[0052] Using the above-mentioned welding deformation correction and stress relief device, the welding deformation correction and stress relief method based on gradient creep proposed in this embodiment includes the following steps:
[0053] The weldment 1 with a maximum deformation range of 12 to 15 mm (the weldment 1 may still produce a deformation of several mm to more than ten mm under the constraint. According to the dimensional accuracy requirements of the weldment 1, too low a deformation may directly meet the requirements. Therefore, the present invention mainly proposes a correction method for this deformation range for deformation exceeding the allowable standard) and a weldment 1 made of austenitic stainless steel is placed between the upper mold 3 and the lower mold 4; after the heating block heats the weldment 1 to a preset temperature, the welding deformation correction and stress relief device performs six-level gradient segmented pressurization on the weldment 1. The displacement of the six-level gradient is 2.4 mm, 2.2 mm, 2 mm, 2 mm, 1 mm, respectively, and the time for the mold to pressurize to each level of gradient displacement is 1 to 5 minutes. It should be noted that after the six-level gradient displacement pressurization, the weldment 1 may still have a small deformation. At this time, the deformation is within the allowable range, and the purpose of deformation correction and stress relief has been achieved. If higher precision is required, the mold can continue to pressurize and displace to the deformation amount, or even the over-correction amount. After unloading and rebounding, the deformation amount can be close to 0. After each level of gradient pressurization, the pressure and preset temperature of the gradient pressurization level are maintained within 0.5 to 1 hour for pressure maintenance and heat preservation, which is used to correct the deformation of the weldment 1 and relax the stress of the weldment through the creep effect. Generally, when the deformation degree is small, the lattice distortion of the metal is small and is not enough to cause recrystallization, so the grain size will not change significantly. Since the grains obtained after recrystallization become coarse as the holding time increases, which significantly reduces the mechanical properties, it is necessary to use a relatively small correction amount and a slower loading rate to reduce the deformation degree of the lattice and reduce the risk of coarse grains. In addition, due to the work hardening phenomenon, as the degree of deformation increases, the resistance to plastic deformation increases, so that a larger correction amount can be used in the first few levels, a smaller correction amount in the next few levels, and the smallest correction amount in the last level, thereby reducing the amount of rebound after unloading.
[0054] In the specific implementation process, the weldment 1 is first fixed, the temperature controller is turned on to heat up to the preset temperature and then kept warm. The loading device 2 is pressed down to correct the welding deformation of the first level gradient, and then kept still for the first level stress relaxation. Then the loading device 2 is pressed down to correct the welding deformation of the second level gradient, and then kept still for the second stress relaxation. Repeat the implementation until the deformation of the weldment 1 is within the permitted range. After the weldment 1 is cooled to room temperature, the mold is unloaded and the weldment 1 is taken out. During the correction process of the first to fourth levels of the weldment 1, there is a gap between the heating block and the mold at this time, and the correction load is mainly transmitted through the contact surface between the upper mold and the weldment on both sides. In the correction process of the fifth and sixth levels, as the gap is reduced to disappear, the heating block is pressed between the mold and the weldment 1, and the correction load can also be transmitted to the weldment 1 through the heating block, which increases the contact area between the correction load and the weldment 1, reduces the additional deformation of the weldment 1 caused by uneven surface force, and makes it easier for the correction method of the present invention to ensure the flatness of the surface of the weldment 1. Since stress relaxation is performed after each level of gradient correction, the residual stress generated by welding and correction is fully eliminated. In the above implementation process, the preset temperature can be set to 400-550°C, and the heating rate can be set to 100-300°C / h. The cooling rate during cooling can be set to 100-300°C / h. The stress relaxation time can be set to 0.5-1h. Generally, the recovery temperature of pure metal is 0.25-0.3 times the melting point temperature, and the minimum recrystallization temperature is 0.4 times the melting point temperature. If alloy elements and trace impurities are doped in the metal, atomic diffusion and grain boundary migration will be hindered, and the recrystallization temperature will be significantly increased. Therefore, aging treatment at a temperature above the recovery temperature and below the recrystallization temperature can eliminate part of the work hardening, lattice distortion and residual stress without significantly affecting the mechanical properties.
[0055] According to the above welding deformation correction and stress relief methods and related process, a numerical simulation method of the whole process from welding to creep with thermo-elastic-viscoplastic coupling is established. Figure 2, the numerical simulation method includes S1 welding analysis, S2 data transfer and S3 creep analysis in sequence. In this step, the sequential coupling technology is used in the welding process, that is, the heat transfer analysis is first performed, and then imported into the mechanical analysis model to obtain the welding stress, strain and deformation results. Secondly, the data transfer technology is used to import the results of the welding calculation into the creep analysis model for analysis. Finally, the welding deformation correction and residual stress relaxation simulation of multi-stage creep aging are carried out. Specifically, the welding analysis steps in the welding process include: establishing a welding finite element analysis model and dividing the welds of different layers. Setting material parameters, including elastic modulus, Poisson's ratio, plasticity, thermal conductivity, specific heat capacity, density, thermal expansion coefficient, latent heat and other material parameters at different temperatures. Define the weld as a life and death unit, and activate the welds layer by layer in sequence. Define the heat dissipation model and ambient temperature. Define boundary constraints and mobile heat source model. Divide the model into grids and solve the results. Using data transfer technology, the stress, strain, temperature and deformation results of welding are used as the initial state of creep analysis, and the deformation correction and stress relaxation simulation of the next link are carried out. Creep analysis includes the following steps: establishing a contact model between the weldment 1 and the upper mold 3 and the lower mold 4. According to the displacement of each level, loading time, stress relaxation time, preset temperature, heating rate, cooling rate, etc. in the process of welding deformation correction and stress elimination, the corresponding simulation parameters are set to assign creep constitutive parameters to the material. It should be noted that the creep analysis model mentioned above includes multiple operation steps such as heating, loading, heat preservation and loading, cooling, and unloading, and different constitutive models are used in different steps. Specifically, the creep analysis model includes two types of ideal elastic-plastic constitutive model and elastic-viscoplastic constitutive model. The ideal elastic-plastic constitutive model is used in the steps of loading and unloading related to deformation, and the elastic-viscoplastic constitutive model is used in the steps of heating, cooling, and heat preservation related to stress. The coupling of multiple models constitutes the creep analysis model. In order to facilitate the description of the process, the models used in the creep analysis process are collectively referred to as creep analysis models.
[0056] The welding deformation correction and stress elimination method based on gradient creep provided in this embodiment is further described in combination with experiments. Figure 3As shown, this embodiment uses a butt joint weldment 1 made of austenitic stainless steel for welding. The joint is set to 7 layers of welds, 60° butt groove, 14mm plate thickness, 2mm root assembly gap, manual argon arc welding, control the interlayer temperature below 100°C, and the welding wire is ER316LMnG. The weldment 1 is welded in a free state to obtain a larger welding deformation. After welding, the maximum deformation of the edge measured by a three-coordinate measuring machine is 12.5mm, and the residual stress on the weld surface detected by XRD is 488MPa. The above-mentioned deformation correction and stress relaxation experiments are then carried out. The heat conductive block 5 is fixed on the surface of the weldment 1. The upper and lower heat conductive blocks 5 are tightened by springs to ensure heat transfer with the surface. The weldment 1 is fixed between the upper mold 3 and the lower mold 4. The temperature controller is used to control the heating rod 6 to heat up, the preset temperature is 550°C, the heating time is 2h, and then the temperature is kept warm. The amount of correction allocated to each level is shown in Table 1.
[0057] Table 1 shows the distribution of each level of correction amount in the embodiment:
[0058]
[0059] Excessive correction may cause additional deformation and stress. This embodiment helps to achieve sufficient stress relaxation and reduce the rebound after unloading by reasonably allocating the correction amount. Since plastic deformation and new stress will be generated after each level of correction, stress relaxation is required after each level of correction, and the time is 0.5h. After the correction and stress relaxation are completed, natural cooling is carried out for 2h. During the heating and cooling stages, the upper mold 3 and the lower mold 4 will limit its thermal deformation. After unloading, the weldment 1 is taken out and the deformation and residual stress are measured again. According to the experimental results, the welding deformation is reduced from 12.5mm to 0.9mm, and the residual stress is reduced from 488MPa to 55MPa. And by sampling the welded joint for tensile testing, the yield strength of the original weldment is 445MPa, the tensile strength is 585MPa, the yield strength after creep aging treatment is 496MPa, the tensile strength is 684MPa, and the elongation is only reduced by 3%. This is attributed to the combined effects of work hardening, creep aging strengthening and heat treatment during the correction process, which also proves that the gradient creep aging process of the present invention has a certain improvement in mechanical properties.
[0060] Please refer to Figure 4, a numerical simulation of the entire welding and creep process matching the above experiments was carried out. The sequentially coupled thermal-elastic-plastic finite element method was used, that is, thermal analysis was performed first and then mechanical analysis. The heat source model was defined according to the process parameters such as welding voltage and current, a double ellipsoid was used to move the heat source, and the DFLUX program was written to define the parameters related to the heat source. The convection and radiation heat transfer coefficients were considered in the finite element software, and the ambient temperature was assumed to be 20°C. The cloud maps of the welding temperature field, stress field, strain field, and displacement field were obtained, and the simulation results were reasonable by comparing them with the stress and deformation states of the experimental results. Figure 5 As shown, the temperature change curve of a node next to the weld of the simulation model is extracted, which is divided into the temperature cycle curve of the welding process and the creep temperature curve of the post-processing. The simulation results are consistent with the actual process. In welding and creep analysis, data transfer technology is used to realize multi-field transfer of the two analyses. This makes it unnecessary to calculate the welding results from scratch when modifying the parameters of the creep analysis, thereby improving the calculation efficiency. This embodiment uses the restart technology to realize the data transfer function, which requires setting the corresponding restart frequency parameters and generating the .RES file for reading the calculation results of the previous stage.
[0061] During the creep process, it is necessary to consider the contact problem between weldment 1 and the mold, set the tangential friction coefficient to 0.1, and the normal contact to the hard contact law. In the loading process, the general analysis step of statics is used, and the viscous analysis step considering creep is used in the stress relaxation-related stage. The time for heating to 550°C is set to 2h, the loading time for each level is 60s, the stress relaxation time for each level is 0.5h, and the cooling time is 2h. Obtaining the creep constitutive equation of the material is an existing means and will not be repeated. The creep constitutive parameters at different temperatures are defined by the hyperbolic sine law, and the parameters are as follows:
[0062]
[0063] In the formula, is the creep rate, σ is stress, R is the gas constant, which is 8.31 J / mol / K, and T is the temperature.
[0064] like Figure 6 As shown, the change of deformation in the creep analysis process is extracted. The first step is data transmission, the second step is to establish contact relationship, and the subsequent process is to correct multiple levels of deformation, and after each level of correction, stress relaxation is performed. The simulation results can truly reflect the deformation process of the actual weldment 1. Please refer to Figure 6To explain in detail, U in the figure, magnitude represents the total displacement. In Step 1, the result obtained from the welding analysis is used as the initial state of the creep analysis process. In this state, the weldment 1 is in a deformed state with a maximum deformation of 12.46 mm, while the upper and lower molds are in the initial state with a displacement of 0 mm. In Step 2, the weldment 1 is kept stationary, the upper mold 3 is pressed down and the upper mold 4 is moved up, and contact properties are gradually established with the weldment 1. Step 3 is the result after the first level of correction is completed. In this process, the lower mold 4 does not move, and only the upper mold 3 needs to be pressed down, and the displacement increment generated by the upper mold 3 at the end of Step 2 is the preset first level correction amount. Looking at Step 4 again, it can be seen that the total displacement of the upper mold 3 is 18.5 mm, and the total displacement of the upper mold 3 of the previous level is 16.3 mm. Their difference increment is the second level correction amount of 2.2 mm. In Step 5, the total displacement of the upper mold 3 is 20.5 mm, and the difference between it and the previous level is the third level correction amount of 2 mm. In Step 6, the total displacement of the upper mold 3 is 22.5 mm, and the difference between it and the previous level is the correction amount of 2 mm in the fourth level. So far, during the correction process of the first four levels, the force conditions of the weldment 1 are as follows: the bottom of the weldment 1 is supported and constrained, and the upper surface of the weldment 1 is subjected to the load of the upper mold 3 on both sides, so that the weldment 1 produces a slight bending effect to reduce the deformation angle. In Step 7, the total displacement of the upper mold 3 is 24.5 mm, and the displacement increment from the previous level is the correction amount of 2 mm in the fifth level. In Step 8, the total displacement of the upper mold 3 is 25.5 mm, and the displacement increment from the previous level is the correction amount of 1 mm in the sixth level. The correction process of the latter two levels is different from the first four levels. At this time, the heating block comes into contact with the mold and begins to transfer the load, so that the mold is subjected to the load on the entire surface of the weldment 1. Such a uniform load can ensure that the surface of the weldment 1 is smoother in the final stage of correction without wave deformation, thereby ensuring the shape accuracy. Finally, in Step 9, the upper mold 3 needs to be moved up and the lower mold 4 needs to be moved down, gradually breaking away from the weldment 1. The unloading process causes a certain amount of deformation and springback of the weldment 1. It can be seen that after the step-by-step correction, the deformation of the weldment is gradually reduced and tends to be flat.
[0065] like Figure 7 As shown in Figure 2, the variation of residual stress during creep analysis is extracted. Figure 7In the first figure, it shows that the stress generated is the residual stress after the welding is completed, and then pressurized heating is performed. As shown in the second figure, during the heating stage, the overall stress of weldment 1 decreases, but the overall stress distribution trend is similar, and the maximum stress still exists in the weld and its vicinity. Then, as shown in the third figure, the amplitude of the residual stress of weldment 1 is increased due to the elastic-plastic deformation caused by the corrective load. At this time, the residual stress is the superposition and coupling of the residual welding stress and the corrective stress, and the stress distribution pattern is changed. High stress areas are generated on the upper and lower surfaces of the weld, while the stress in the center area of the weld is lower. These areas may be near the neutral plane of the weldment bending process, and are therefore less affected by the corrective load. Then refer to Figure 7 In the fourth figure, the residual stress is released by the stress relaxation process, and the overall stress is reduced. The repeated process of multi-level correction and stress relaxation makes the stress distribution law the same, forming a periodic stress change. Figure 6 The stress relaxation process has been described in the description of the stress relief method mentioned above, and will not be repeated here. Figure 7 As shown in the fifth and sixth figures, the stress of weldment 1 increases slightly during the cooling stage, and the stress in the central area increases. The overall stress state of weldment 1 is significantly reduced after unloading, and the maximum stress is in the cross section of the middle thickness of the weldment. The above simulation results can truly reflect the stress change process of the actual weldment 1. The above method simulates the changes in welding deformation correction and residual stress relaxation of multi-stage creep aging.
[0066] Please refer to Figure 8 , the deformation changes with time were extracted, and it can be seen that the overall trend is a step-down, and there will be a rebound phenomenon in the final unloading stage, and the rebound amount is small, so that the welding deformation is well corrected. Within 0.5h of each level of stress relaxation, due to the constraint of the mold, the deformation does not change, and the shape accuracy is well guaranteed.
[0067] Please refer to Fig. 9, the stress relaxation curve of the center point of the weld was extracted. The first stress drop is the heating stage, mainly for the following reasons: due to the increase in temperature, the yield strength of the material decreases. When the internal force is greater than the yield strength of the material, the stress will be converted into deformation. At the same time, the elastic modulus will also decrease during heating. Since stress is the product of elastic strain and elastic modulus, the stress will decrease. The last reason is the stress relaxation effect of material creep. Part of the elastic strain is converted into creep strain, which also reduces the stress. Subsequently, loading and correction are performed. Due to the plastic deformation, the stress will increase, and the maximum will only reach the yield strength at the current temperature. Then keep the mold still and perform stress relaxation under constant load. It can be seen that the stress decreases faster and gradually slows down in the early stage of creep. This is because stress is the internal driving force of creep. Large stress makes the creep effect strong. As the stress is eliminated, the creep effect weakens, which makes short-term stress relaxation sufficient to ensure the effect of stress elimination, thereby improving the time efficiency of the process. In the insulation stage, the yield strength and elastic modulus of the material remain unchanged, so the stress relaxation in this stage is mainly dominated by the creep effect. In the cooling stage, the elastic modulus and yield strength of the material increase, and the creep effect gradually weakens as the temperature decreases, causing the stress to increase to a certain extent. When unloading, the stress will further decrease because the orthopedic load introduces new stress. After the load is removed, the structure is released and rebounds, and the stress will also decrease.
[0068] Please refer to Fig.10 , extract the cumulative process curve of equivalent creep strain. Since each stress relaxation will produce creep strain, the cumulative creep strain will also show a continuous upward trend. During the creep process, part of the elastic strain is converted into creep strain, which reduces the stress. Fig.11 and Fig.12 , the stress curve of the upper surface of the vertical weld section was extracted. Before creep indicates the stress state when welding is completed, and after creep indicates the state after multiple stress relaxations. It can be clearly seen that the longitudinal stress and transverse stress are greatly reduced after creep, which shows that it has a significant effect on overall stress relief. Among them, the longitudinal direction indicates the direction along the weld, and the transverse direction indicates the direction perpendicular to the weld. Fig.13 , the deformation curve of the upper surface of the vertical weld section was extracted, and it can be seen that the welding deformation is significantly reduced before and after creep. Fig.14 , microscopic metallographic observation of the weld area before creep shows that the weld structure is mainly austenite, accompanied by high-temperature ferrite phase. The weld metal solidified into ferrite has a high resistance to the formation of hot cracks, which is consistent with the metallographic characteristics of the weld. Fig.15 , the thickness of ferrite increases after creep, accompanied by a small amount of carbide and σ phase precipitation, which leads to an increase in the hardness and strength of the material, while the plasticity and toughness decrease.
[0069] In summary, the gradient creep aging process disclosed in the present invention can better correct welding deformation, and achieve a significant elimination of welding residual stress and orthopedic stress in multiple stress relaxations, while improving the strength of the material, which has good application value and engineering significance. The numerical simulation method of the whole process from welding to creep of the thermo-elastic-viscoplastic coupling disclosed in the present invention can effectively predict and evaluate the orthopedic and stress relaxation effects, thereby optimizing the process parameters and guiding the practical process.
[0070] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0071] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for welding deformation correction and stress relief, characterized in that: It is used to correct deformation and eliminate stress for welded parts with a maximum deformation range of 12 to 15 mm and made of austenitic stainless steel; the deformation correction and stress elimination method includes the following steps: Provided is a welding deformation correction and stress relief device; the welding deformation correction and stress relief device comprises a loading device (2), an upper mold (3), a lower mold (4) and at least two heating blocks; The weld is mounted between an upper mold (3) and a lower mold (4) that cooperate with each other; a plurality of heating blocks are connected to the upper and lower surfaces of the weld, and are used to uniformly heat the weld to a preset temperature; the loading device (2) applies pressure to the upper mold (3) to perform six-level gradient segmented pressurization on the weld, the six-level gradient displacements are 2.4 mm, 2.2 mm, 2 mm, 2 mm, 2 mm, and 1 mm, respectively, and the time for the upper mold (3) to pressurize to each level of gradient displacement is 1 to 5 minutes; after each level of gradient pressurization, the pressure and preset temperature of the gradient pressurization are maintained within 0.5 to 1 hour for pressure and heat preservation, so as to correct the deformation of the weld and relax the stress of the weld through the creep effect; wherein the preset temperature is 400 to 550°C; the heating rate of the preset temperature is 100 to 300°C / h; After the sixth level of gradient pressure and temperature preservation, the heating block stops heating the weldment and maintains the sixth level of gradient pressure until the weldment cools to room temperature.
2. The welding deformation correction and stress relief method according to claim 1, characterized in that: When the heating block stops heating the weldment and then cools it down, the cooling rate is 100-300°C / h until it cools down to room temperature.
3. A welding deformation correction and stress relief device, characterized in that: It uses the welding deformation correction and stress relief method as described in any one of claims 1 to 2 to correct deformation and relieve stress on welded parts, and the welding deformation correction and stress relief device comprises a loading device (2), an upper mold (3), a lower mold (4) and at least two heating blocks; The loading device (2) is used to drive the upper mold (3) and the lower mold (4) to close the mold and apply pressure; The pressurizing surface of the upper mold (3) and the pressurizing surface of the lower mold (4) are arranged in parallel, and the pressurizing surfaces of the upper mold (3) and the lower mold (4) are both provided with air-avoiding grooves for accommodating the heating block; The heating block is connected to the welded part and corresponds to the air avoidance groove; when the welded part is in the first to fourth stage of segmented pressurization, the heating block gradually enters the air avoidance groove and there is a gap between the heating block and the inner bottom of the air avoidance groove; when the welded part is in the fifth and sixth stage of segmented pressurization, one side of the heating block contacts the inner bottom of the air avoidance groove and the other side is flush with the notch of the air avoidance groove to expand the area of the pressurized surface of the upper mold (3) and the lower mold (4).
4. The welding deformation correction and stress relief device according to claim 3, characterized in that: The heating block comprises a heat conducting block (5) and a heating rod (6); the heat conducting block (5) is connected to a welding piece, and a hole is provided on the heat conducting block (5), and the heating rod (6) is installed in the hole.
5. The welding deformation correction and stress relief device according to claim 4, characterized in that: Four heat conducting blocks (5) are provided, of which two heat conducting blocks (5) are located on the upper surface of the welding piece, and the other two heat conducting blocks (5) are located on the lower surface of the welding piece, and the heat conducting blocks (5) located on the upper and lower sides of the welding piece are arranged in a one-to-one correspondence.
6. The welding deformation correction and stress relief device according to claim 5, characterized in that: A spring is commonly connected between the heat conducting blocks (5) on the upper and lower surfaces of the welded part, and the spring is used to pull the heat conducting blocks (5) on the upper and lower surfaces of the welded part together so that the heat conducting blocks (5) are closely fitted to the surface of the welded part.
7. The welding deformation correction and stress relief device according to claim 3, characterized in that: The welding deformation correction and stress relief device further comprises two fixing blocks (7), the two fixing blocks (7) being respectively connected to two ends of the lower mould (4); the weldment is fixed between the two fixing blocks (7) by bolts.
8. A numerical simulation method for the whole process from welding to creep, characterized in that: The method for correcting welding deformation and eliminating stress according to any one of claims 1 to 2 is numerically simulated, and the numerical simulation method comprises the following steps: Sequential coupling technology is used in the welding process, first thermal analysis and then mechanical analysis to obtain welding stress, strain and deformation results; Using data transfer technology, the analysis results during welding are imported into the creep analysis model for creep analysis; The changes of welding deformation correction and residual stress relaxation during multi-stage creep aging are simulated based on the creep analysis model.
9. The numerical simulation method for the whole process from welding to creep according to claim 8, characterized in that: Analysis during welding includes the following steps: Establish a welding finite element analysis model and divide the welds into different layers; set material parameters, including elastic modulus, Poisson's ratio, plasticity, thermal conductivity, specific heat capacity, density, thermal expansion coefficient and latent heat at different temperatures; define the weld as a birth and death unit, and activate the welds layer by layer in sequence; define the heat dissipation model and ambient temperature; define boundary constraints and mobile heat source model; divide the model into grids and solve the results; The data transfer technology is used to use the stress, strain, temperature and deformation results of welding as the initial state of creep analysis to perform deformation correction and stress relaxation simulation in the next step; The creep analysis includes the following steps: A contact model between the weldment and the mold is established; corresponding simulation parameters are set according to each level of displacement, loading time, stress relaxation time, preset temperature, heating rate, and cooling rate during the welding deformation correction and stress relief process, and creep constitutive parameters of the weldment are assigned.