A modification method of nano calcium carbonate for silicone sealant

By modifying and combining nano calcium carbonate, the problem of insufficient hardness, tensile strength and flame retardant performance of silicone sealant is solved, and silicone sealing with high hardness, high tensile strength and high flame retardant grade is achieved rubber meets application needs in the construction field.

CN118652566BActive Publication Date: 2024-11-08耒阳市百汇粉体有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411129769.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-08
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

The existing silicone sealant has low hardness and tensile strength and poor flame retardant performance, which cannot meet the application needs of some construction fields.

Method used

By selecting different forms of nano calcium carbonate for modification, nitrogen-containing nano calcium carbonate and phosphorus-containing nano calcium carbonate were obtained, and compounded to improve the hardness, tensile strength and flame retardant grade of silicone sealant.

Benefits of technology

The hardness and tensile strength of silicone sealant have been significantly improved, and its flame retardant grade has been improved to meet the performance requirements of V-0 grade.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118652566B_ABST
    Figure CN118652566B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of nano calcium carbonate, and in particular to a modification method of nano calcium carbonate for silicone sealant. The present invention selects nano calcium carbonate in different forms, and modifies them respectively to obtain nitrogen-containing nano calcium carbonate and phosphorus-containing nano calcium carbonate, and then compound the different modified nano calcium carbonates to obtain nano calcium carbonate for silicone sealant, and the prepared silicone sealant has high hardness and high tensile strength, and at the same time improves the flame retardant grade.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of nano calcium carbonate, and in particular to a modification method of nano calcium carbonate for silicone sealant. Background Art

[0002] The main ingredients of silicone sealant are polydimethylsiloxane, a paste made of terminal hydroxyl siloxane polymer and multifunctional siloxane crosslinker, with fillers, plasticizers, coupling agents and catalysts added. These raw materials are combined together and gradually cured to form elastic and adhesive silicone rubber. Nano calcium carbonate, as a new functional inorganic material with stable performance and easy processing, is widely used in rubber, silicone sealant, plastic, coating, ink and papermaking industries, so it is also the main filler of silicone sealant.

[0003] Silicone sealants that use nano-calcium carbonate as filler are widely used in the assembly of building components (such as aluminum doors and windows, glass curtain walls, stone curtain walls, etc.), bonding and caulking, but existing silicone sealants have poor mechanical properties, such as low hardness and tensile strength, which limit their application scenarios; at the same time, due to the high demand for fire protection of materials in the construction field, the flame retardant properties of silicone sealants are poor, and the flame retardant grade cannot meet the requirements of some scenarios.

[0004] Therefore, how to process nano-calcium carbonate to obtain modified nano-calcium carbonate, thereby improving the comprehensive performance of silicone sealants using modified nano-calcium carbonate as fillers, increasing the hardness and tensile strength of silicone sealants, and improving flame retardant properties has become a direction that needs to be focused on. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a modification method of nano-calcium carbonate for silicone sealant, aiming to solve the problems of low hardness and tensile strength and poor flame retardant performance of silicone sealant using nano-calcium carbonate as filler.

[0006] The invention selects nano calcium carbonate in different forms and modifies them respectively to obtain nitrogen-containing nano calcium carbonate and phosphorus-containing nano calcium carbonate, then compound the different modified nano calcium carbonates to obtain nano calcium carbonate for silicone sealant, and the prepared silicone sealant has high hardness and high tensile strength, while improving the flame retardant grade.

[0007] The technical solution of the present invention is as follows:

[0008] The first aspect of the present invention provides a method for modifying nano calcium carbonate for silicone sealant, comprising the following steps:

[0009] Step S1: adding 30-40 parts of a modifier to 1000 parts of deionized water, dissolving the modifier, stirring and adding 400-500 parts of nano calcium carbonate I, reacting for 1-2 hours, filtering to obtain a filter cake, drying the filter cake at 120° C., crushing the filter cake, and sieving to obtain nitrogen-containing nano calcium carbonate;

[0010] Step S2: adding 10-15 parts of nano calcium carbonate II and 5-10 parts of phosphate to 150 parts of deionized water, mixing evenly and then oscillating in a constant temperature water bath oscillator for constant temperature reaction, filtering and drying after the reaction, grinding and sieving to obtain phosphorus-containing nano calcium carbonate;

[0011] Step S3: Evenly mix the nitrogen-containing nano-calcium carbonate described in step S1 and the phosphorus-containing nano-calcium carbonate described in step S2, and obtain nano-calcium carbonate for silicone sealant after drying.

[0012] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the objectives and beneficial effects of the present invention can be better achieved and realized.

[0013] Preferably, the preparation method of the modifier in step S1 is: dissolving 0.1-0.3 parts of dimethylhexadecanamide in 30-50 parts of anhydrous methanol, adding 0.15-0.25 parts of propylene chloride to obtain a mixture, heating the mixture to reflux for 12-14 hours, recrystallizing the product with anhydrous ethanol, and obtaining the modifier after drying.

[0014] After adding quaternary ammonium salt modifier to nano-calcium carbonate, the positively charged end of the quaternary ammonium salt is adsorbed on the surface of the nano-calcium carbonate through electrostatic adsorption, and the other end is a long carbon chain hydrocarbon group and an allyl group with a double bond, which can cross-link with the polymer material of the silicone sealant, thereby improving the tensile strength of the silicone sealant; at the same time, the nitrogen element in the nitrogen-containing nano-calcium carbonate will produce flame-retardant nitrogen-containing compounds, diluting the concentration of the combustion gas near the flame to achieve a flame retardant effect.

[0015] As a preferred technical solution of the present invention, the nano-calcium carbonate I in step S1 is a spindle-shaped nano-calcium carbonate; the major diameter of the spindle-shaped nano-calcium carbonate is 200-250 nm, and the minor diameter is 60-80 nm.

[0016] Silicone sealant filled with spindle-shaped nano-calcium carbonate has many pores on the surface and inside, so the silicone sealant cures quickly and its hardness increases quickly. In addition, after being fully cured, the spindle-shaped nano-calcium carbonate plays a role similar to a "skeleton", intertwining with each other and attracting and entangled with the resin molecular chains of the silicone sealant, thereby improving the tensile strength of the sealant.

[0017] It should be noted that the source of spindle-shaped nano-calcium carbonate is not particularly limited in the present invention, and it can be purchased from the market or prepared by itself. The preparation method of spindle-shaped nano-calcium carbonate is not particularly limited in the present invention, and it can be prepared by referring to the method described in "CN107792872A" for example.

[0018] As a preferred technical solution of the present invention, the nano-calcium carbonate II in step S2 is needle-shaped nano-calcium carbonate; the long diameter of the needle-shaped nano-calcium carbonate is 100-120 nm, and the short diameter is 10-20 nm.

[0019] Needle-shaped nano-calcium carbonate has strong spatial orientation and tends to form a stacking structure with high porosity. In the silicone sealant system, it is easy to build a three-dimensional network structure by entangled with the silicone molecular chain, restricting the movement of the molecular chain, thereby increasing the hardness of the silicone sealant.

[0020] It should be noted that the present invention does not make any special restrictions on the source of needle-shaped nano calcium carbonate, which can be purchased from the market or prepared by itself. The present invention does not make any special restrictions on the preparation method of needle-shaped nano calcium carbonate, which can be prepared by referring to the method described in "CN101229926A" for example.

[0021] Preferably, in step S2, the phosphate ester is selected from any one of dodecyl phosphate, dihexadecyl phosphate, and octadecyl phosphate, or a combination of at least two thereof.

[0022] Phosphate esters mainly combine with calcium ions on the surface of nano-calcium carbonate to form phosphates, which produce a coating effect on the surface of calcium carbonate, thereby improving the hardness of the silicone sealant filled with modified nano-calcium carbonate; in addition, phosphorus-based groups will produce phosphaphenanthrene groups in the gas phase, which can capture free radicals of gas-phase cracking gases, form a stable structure, and exert a free radical quenching effect, thereby improving the flame retardant effect of silicone sealants.

[0023] Preferably, the constant temperature of the constant temperature oscillation in step S2 is 80-90° C., the oscillation time is 0.5-1 h, the drying temperature is 50-60° C., and the drying time is 24-48 h.

[0024] Preferably, the water content of the nano-calcium carbonate for silicone sealant after the drying treatment in step S3 is less than 0.3%.

[0025] Preferably, the use of the nano-calcium carbonate prepared by the modification method in silicone sealant comprises the following steps: 45-50 parts of hydroxypolydimethylsiloxane, 45-50 parts of nano-calcium carbonate and 4-5 parts of dimethyl silicone oil are put into a stirrer, and the temperature is controlled to be 110-130°C for dehydration for 3-4 hours under a vacuum environment, and then cooled to 35-40°C, and then 3.5-4 parts of ethyl orthosilicate, 0.4-0.5 parts of 3-aminopropyltrimethoxysilane and 1.0-1.2 parts of dibutyltin dilaurate are added, and the mixture is uniformly mixed for 1 hour under a vacuum state, and then the material is discharged and canned to obtain a silicone sealant.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] (1) The present invention selects nano-calcium carbonate in different forms for compounding. The spindle-shaped nano-calcium carbonate attracts and entangles with the silicone sealant molecular chains; the needle-shaped nano-calcium carbonate can fill and entangle with the silicone molecular chains to easily build a three-dimensional network structure, thereby comprehensively improving the mechanical properties of the sealant.

[0028] (2) The silicone sealant used in the present invention contains silicon, and the modified nano calcium carbonate contains nitrogen and phosphorus. The silicon and nitrogen elements synergistically generate a flame retardant gas that exerts a flame retardant effect in the condensed phase and the gas phase. The phosphorus and silicon elements synergistically form a phosphorus-containing carbon layer and a silicon-containing protective layer to avoid oxidation of the carbon layer on the surface of the material, thereby achieving synergistic flame retardancy of silicon, nitrogen and phosphorus. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a performance test data table of the embodiments of the present invention and the comparative examples. DETAILED DESCRIPTION

[0030] To facilitate understanding of the present invention, the present invention lists application examples as follows. Those skilled in the art should understand that the application examples are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0031] The sources of some components in the application examples and comparative examples are as follows:

[0032] Preparation of nitrogen-containing nano-calcium carbonate: 0.3 parts of dimethylhexadecanamide (CAS No. 3886-91-7) are dissolved in 30 parts of anhydrous methanol (CAS No. 170082-17-4), and 0.25 parts of allyl chloride (CAS No. 107-05-1) are added to obtain a mixture. The mixture is heated to reflux for 14 hours, and the product is recrystallized with anhydrous ethanol (CAS No. 64-17-5). After drying, a modifier is obtained; 30 parts of the modifier are added to 1000 parts of deionized water, and after dissolution, 500 parts of spindle-shaped nano-calcium carbonate (long diameter of 200 nm, short diameter of 60 nm) are added with stirring, and after reacting for 2 hours, a filter cake is obtained by suction filtration. The filter cake is dried at 120°C and then crushed, and the nitrogen-containing nano-calcium carbonate is obtained after sieving.

[0033] Preparation of phosphorus-containing nano-calcium carbonate: Add 10 parts of needle-shaped nano-calcium carbonate (long diameter of 100 nm, short diameter of 10 nm) and 5 parts of dodecyl phosphate (CAS No. 12751-23-4) to 150 parts of deionized water, mix well and oscillate on a constant temperature water bath oscillator for constant temperature reaction. The constant temperature is 80°C and the oscillation time is 1 hour. After the reaction is completed, filter and dry (drying temperature is 60°C, drying time is 48 hours), grind and sieve to obtain phosphorus-containing nano-calcium carbonate.

[0034] Preparation of nano calcium carbonate for silicone sealant: 200 parts of nitrogen-containing nano calcium carbonate and 100 parts of phosphorus-containing nano calcium carbonate are mixed evenly, and dried to make the water content 0.2% to obtain nano calcium carbonate for silicone sealant.

[0035] Hydroxypolydimethylsiloxane: brand XHG-107, purchased from Zhejiang Xin'an Chemical Group Co., Ltd.;

[0036] Nano calcium carbonate: CAS No. 471-34-1;

[0037] Dimethyl silicone oil: CAS No. 9006-65-9;

[0038] Ethyl orthosilicate: CAS No. 78-10-4;

[0039] 3-Aminopropyltrimethoxysilane: CAS No. 13822-56-5;

[0040] Dibutyltin dilaurate: CAS No. 77-58-7.

[0041] Application Example 1

[0042] The present application embodiment provides a silicone sealant, the preparation of which includes the following steps: 45 parts of hydroxypolydimethylsiloxane, 45 parts of nano-calcium carbonate for silicone sealant, and 5 parts of dimethyl silicone oil are put into a stirrer, and under a vacuum environment, the temperature is controlled to be 130° C. for dehydration for 4 hours, and then cooled to 40° C., and then 3.5 parts of ethyl orthosilicate, 0.45 parts of 3-aminopropyltrimethoxysilane and 1.05 parts of dibutyltin dilaurate are added, and the mixture is uniformly mixed under a vacuum state for 1 hour, and then the material is discharged and canned to obtain the silicone sealant.

[0043] Application Example 2

[0044] The present application embodiment provides a silicone sealant, the preparation of which includes the following steps: 50 parts of hydroxypolydimethylsiloxane, 50 parts of nano-calcium carbonate for silicone sealant, and 4 parts of dimethyl silicone oil are put into a stirrer, and the temperature is controlled to be 110° C. for dehydration for 3 hours under a vacuum environment, and then cooled to 35° C., and then 4 parts of ethyl orthosilicate, 0.5 parts of 3-aminopropyltrimethoxysilane and 1.2 parts of dibutyltin dilaurate are added, and the mixture is uniformly mixed under a vacuum state for 1 hour, and then the mixture is discharged and canned to obtain the silicone sealant.

[0045] Application Example 3

[0046] The present application embodiment provides a silicone sealant, the preparation of which includes the following steps: 48 parts of hydroxypolydimethylsiloxane, 47 parts of nano-calcium carbonate, and 4.6 parts of dimethyl silicone oil are put into a stirrer, and under a vacuum environment, the temperature is controlled to be 120° C. for dehydration for 3.5 hours, and then cooled to 38° C., and then 3.8 parts of ethyl orthosilicate, 0.4 parts of 3-aminopropyltrimethoxysilane, and 1.0 parts of dibutyltin dilaurate are added, and the mixture is uniformly mixed under a vacuum state for 1 hour, and then the material is discharged and canned to obtain the silicone sealant.

[0047] Application Example 4

[0048] This application example provides a silicone sealant, which is different from application example 1 only in that the nano-calcium carbonate in the silicone sealant is replaced by nitrogen-containing nano-calcium carbonate.

[0049] Application Example 5

[0050] This application example provides a silicone sealant, which is different from application example 1 only in that the nano-calcium carbonate in the silicone sealant is replaced by phosphorus-containing nano-calcium carbonate.

[0051] Application Comparative Example 1

[0052] This application comparison example provides a silicone sealant, and the preparation of the silicone sealant includes the following steps: 45 parts of hydroxypolydimethylsiloxane, 45 parts of nano calcium carbonate (CAS No. 471-34-1), and 5 parts of dimethyl silicone oil are put into a stirrer, and under a vacuum environment, the temperature is controlled to be 130°C for dehydration for 4 hours, and then cooled to 40°C, and then 3.5 parts of ethyl orthosilicate, 0.45 parts of 3-aminopropyltrimethoxysilane and 1.05 parts of dibutyltin dilaurate are added, and the mixture is uniformly mixed under a vacuum state for 1 hour, and then the material is discharged and canned to obtain a silicone sealant.

[0053] Application Comparative Example 2

[0054] This application comparison example provides a silicone sealant, which is different from application comparison example 1 only in that the nano calcium carbonate (CAS No. 471-34-1) is replaced by spindle-shaped nano calcium carbonate (long diameter of 200 nm, short diameter of 60 nm) in this application comparison example.

[0055] Application Comparative Example 3

[0056] This application comparison example provides a silicone sealant, which is different from application comparison example 1 only in that the nano calcium carbonate (CAS No. 471-34-1) is replaced by needle-shaped nano calcium carbonate (long diameter of 100 nm and short diameter of 10 nm) in this application comparison example.

[0057] The performance of the silicone sealant provided in the above application examples and application comparison examples was tested, and the testing method was as follows:

[0058] Tensile strength: Tested in accordance with the requirements of GB 16776-2005 Silicone Structural Sealant for Buildings.

[0059] Shore hardness: Tested in accordance with the requirements of GB 16776-2005 Silicone Structural Sealant for Buildings.

[0060] Flame retardant grade: Tested in accordance with the requirements of GB / T 24267-2009 Flame retardant sealants for building.

[0061] The above performance test data is as follows Figure 1 shown.

[0062] From the above content, it can be seen that in the present invention, nano-calcium carbonate in different forms is selected and modified to obtain nitrogen-containing nano-calcium carbonate and phosphorus-containing nano-calcium carbonate, and then the different modified nano-calcium carbonates are compounded to obtain nano-calcium carbonate for silicone sealant, and the prepared silicone sealant has a tensile strength of 1.74~1.76MPa, a Shore hardness of 48~50, and a flame retardant grade of V-0.

[0063] Compared with Example 1, if only nitrogen-containing nano-calcium carbonate is used, the hardness decreases and the flame retardant performance deteriorates (Example 4); compared with Example 1, if only phosphorus-containing nano-calcium carbonate is used, the tensile strength decreases and the flame retardant performance deteriorates (Example 5).

[0064] Comparative Example 1 does not adopt the technical innovation of the present invention, so the performance is poor, with a tensile strength of 1.51 MPa, a Shore hardness of 33, and a flame retardant grade of V-2; compared with Comparative Example 1, if spindle-shaped nano-calcium carbonate is used, the tensile strength is improved (Comparative Example 2); compared with Comparative Example 1, if needle-shaped nano-calcium carbonate is used, the hardness is improved (Comparative Example 3).

[0065] In summary, the present invention improves the mechanical properties of the sealant by compounding nano-calcium carbonate in different forms; at the same time, the silicone sealant contains silicon, and the modified nano-calcium carbonate contains nitrogen and phosphorus, which can achieve the synergistic flame retardancy of silicon, nitrogen and phosphorus.

[0066] The applicant declares that the present invention illustrates the detailed process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for modifying nano calcium carbonate for silicone sealant, characterized in that: The following steps are involved: Step S1: adding 30-40 parts of a modifier to 1000 parts of deionized water, dissolving the modifier, stirring and adding 400-500 parts of nano calcium carbonate I, reacting for 1-2 hours, filtering to obtain a filter cake, drying the filter cake at 120° C., crushing the filter cake, and sieving to obtain nitrogen-containing nano calcium carbonate; Step S2: adding 10-15 parts of nano calcium carbonate II and 5-10 parts of phosphate to 150 parts of deionized water, mixing evenly and then oscillating in a constant temperature water bath oscillator for constant temperature reaction, filtering and drying after the reaction, grinding and sieving to obtain phosphorus-containing nano calcium carbonate; Step S3: uniformly mixing the nitrogen-containing nano-calcium carbonate described in step S1 and the phosphorus-containing nano-calcium carbonate described in step S2, and drying the mixture to obtain nano-calcium carbonate for silicone sealant; The preparation method of the modifier in step S1 is as follows: dissolving 0.1-0.3 parts of dimethyl hexadecanoic acid amide in 30-50 parts of anhydrous methanol, adding 0.15-0.25 parts of propylene chloride to obtain a mixture, heating the mixture to reflux for 12-14 hours, and recrystallizing the product with anhydrous ethanol, and drying to obtain the modifier; In step S1, the nano calcium carbonate I is a spindle-shaped nano calcium carbonate; the spindle-shaped nano calcium carbonate has a long diameter of 200-250 nm and a short diameter of 60-80 nm; In step S2, the nano-calcium carbonate II is needle-shaped nano-calcium carbonate; the long diameter of the needle-shaped nano-calcium carbonate is 100-120 nm, and the short diameter is 10-20 nm.

2. The method for modifying nano calcium carbonate for silicone sealant according to claim 1, characterized in that: In step S2, the phosphate ester is selected from any one of dodecyl phosphate, dihexadecyl phosphate, and octadecyl phosphate, or a combination of at least two thereof.

3. The method for modifying nano calcium carbonate for silicone sealant according to claim 1, characterized in that: The constant temperature of the constant temperature oscillation in step S2 is 80-90° C., the oscillation time is 0.5-1 h, the drying temperature is 50-60° C., and the drying time is 24-48 h.

4. The method for modifying nano calcium carbonate for silicone sealant according to claim 1, characterized in that: The water content of the nano-calcium carbonate for silicone sealant after the drying treatment in step S3 is less than 0.3%.

5. The use of the nano calcium carbonate prepared by the modification method of nano calcium carbonate for silicone sealant according to claim 1 in silicone sealant comprises the following steps: 45-50 parts of hydroxy polydimethylsiloxane, 45-50 parts of The nano-calcium carbonate prepared by the modification method of nano-calcium carbonate for silicone sealant according to claim 1 and 4 to 5 parts of dimethyl silicone oil are put into a stirrer, and the temperature is controlled to be 110 to 130° C. for dehydration for 3 to 4 hours under a vacuum environment, and then cooled to 35 to 40° C., and then 3.5 to 4 parts of ethyl orthosilicate, 0.4 to 0.5 parts of 3-aminopropyltrimethoxysilane and 1.0 to 1.2 parts of dibutyltin dilaurate are added, and the mixture is uniformly mixed for 1 hour under a vacuum state, and then the material is discharged and canned to obtain a silicone sealant.