Nano calcium carbonate for silane-modified polyether sealant and preparation method thereof

By wet modification, dry modification and plasma treatment of nano calcium carbonate, the mechanical properties and flame retardant problems of silane-modified polyether sealant are solved, and its tensile strength, elongation of break and Flame retardant performance achieves the effect of low water absorption.

CN118652567BActive Publication Date: 2024-11-26耒阳市百汇粉体有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411145674.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-26
Estimated Expiration
2044-08-20

AI Technical Summary

Technical Problem

The tensile strength and elongation of breaking of existing silane modified polyether sealants are insufficient, the water absorption rate is too high, and the flame retardant grade is insufficient, making it difficult to meet the needs of engineering structures.

Method used

Modified nano calcium carbonate for silane-modified polyether sealant was prepared by wet modification, dry modification and plasma treatment of nano calcium carbonate, which increased its tensile strength, elongation of break and resistance Fueling performance.

Benefits of technology

The tensile strength and elongation of break of silane modified polyether sealant are significantly improved, the water absorption rate is reduced, and the flame retardant performance is improved, achieving excellent mechanical properties and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118652567B_ABST
    Figure CN118652567B_ABST
Patent Text Reader

Abstract

The present invention provides a nano calcium carbonate for silane modified polyether sealant and a preparation method thereof, and relates to the field of nano calcium carbonate. The present invention sequentially performs wet modification, dry modification, and plasma treatment on nano calcium carbonate, obtains nano calcium carbonate for silane modified polyether sealant through multiple modification treatments, and the prepared silane modified polyether sealant has excellent tensile strength and elongation at break, low water absorption, and improved flame retardancy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of nano calcium carbonate, in particular to nano calcium carbonate used for silane-modified polyether sealant and a preparation method thereof. Background Art

[0002] Silane modified polyether (MS) sealant, as one of the modified silane sealants, is a high-performance environmentally friendly sealant prepared by mixing short silane polyether as prepolymer and plasticizer, filler, coupling agent, catalyst, dewatering agent and other additives. Silane modified polyether sealant has the characteristics of good storage stability, high elasticity, flexibility, excellent adhesion, paintability, green environmental protection and no substrate pollution. It is widely used in prefabricated buildings, transportation, home decoration, aviation and industry.

[0003] When existing silane-modified polyether sealants are used in engineering structures, their mechanical properties such as tensile strength and elongation at break are insufficient, and their water absorption rate is too high. They are easily penetrated by water, causing deformation of their structures and affecting their use. In addition, in the face of potential fire threats in life, it is also necessary to improve the flame retardant level of silane-modified polyether sealants.

[0004] Therefore, how to obtain modified nano-calcium carbonate by processing nano-calcium carbonate, thereby improving the comprehensive performance of silane-modified polyether sealant using modified nano-calcium carbonate as filler, improving the tensile strength and elongation at break of the sealant, reducing water absorption, and ensuring good flame retardant properties has become a direction that needs to be focused on. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a nano calcium carbonate for silane modified polyether sealant and a preparation method thereof, aiming to solve the problems of insufficient mechanical properties such as tensile strength and elongation at break, excessively high water absorption, and insufficient flame retardancy of silane modified polyether sealant using nano calcium carbonate as filler.

[0006] The invention sequentially performs wet modification, dry modification and plasma treatment on nano calcium carbonate to obtain nano calcium carbonate for silane-modified polyether sealant through multiple modification treatments, and the prepared silane-modified polyether sealant has excellent tensile strength and elongation at break, lower water absorption rate and improved flame retardancy.

[0007] The technical solution of the present invention is as follows:

[0008] The first aspect of the present invention provides a method for preparing nano calcium carbonate for silane-modified polyether sealant, comprising the following steps:

[0009] Step S1: wet-modifying nano-calcium carbonate to obtain modified nano-calcium carbonate I;

[0010] Step S2: dry-modifying the modified nano-calcium carbonate I described in step S1 to obtain modified nano-calcium carbonate II;

[0011] Step S3: Plasma treatment is performed on the modified nano-calcium carbonate II described in step S2 to obtain nano-calcium carbonate for silane-modified polyether sealant.

[0012] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the objectives and beneficial effects of the present invention can be better achieved and realized.

[0013] As a preferred technical solution of the present invention, the wet modification process in step S1 is as follows: weigh 80-100 parts of nano-calcium carbonate, add them to 400-500 parts of anhydrous ethanol, and ultrasonically disperse them for 2 hours to obtain a nano-calcium carbonate suspension; add 10-20 parts of alanine modifier to the nano-calcium carbonate suspension, heat it to 70-80°C, stir it for 0.5 hours, and obtain modified nano-calcium carbonate I after suction filtration, washing and drying.

[0014] Preferably, the alanine modifier is selected from any one of DL-alanine, D-alanine, and L-alanine, or a combination of at least two of them.

[0015] Small molecular amino acid organic matter is grafted on the surface of wet-modified nano-calcium carbonate, which changes the hydrophilicity of the nano-calcium carbonate filler into lipophilicity, reduces the surface energy of the nano-calcium carbonate, and thus leads to a decrease in the water absorption rate of the sealant; at the same time, the wet-modified nano-calcium carbonate improves the dispersibility of the nano-filler in the sealant, and grafts amino groups on the surface of the nano-calcium carbonate, which can react with the silanol groups generated by the hydrolysis of the sealant siloxane to form a cross-linked network structure, thereby improving the tensile strength and elongation at break; in addition, the wet-modified nano-calcium carbonate contains nitrogen, which can form a hindered amine structure with a quenching effect, thereby obtaining a non-flammable gas, exerting a gas phase dilution effect, and improving the flame retardant efficiency.

[0016] As a preferred technical solution of the present invention, the dry modification process in step S2 is as follows: 150-200 parts of modified nano-calcium carbonate I are added to a stirrer and stirred and heated; when the temperature reaches 80-90°C, 20-30 parts of a borate modifier are added, the temperature is raised to 110-130°C and stirred for 2 hours, and modified nano-calcium carbonate II is obtained after sieving.

[0017] Preferably, the borate modifier is selected from any one of triethanolamine borate, diethanolamine borate, triphenyl borate, or a combination of at least two thereof.

[0018] The surface of the dry-modified nano-calcium carbonate is coated with the hydrophobic carbon chain of borate, which itself exhibits extremely strong hydrophobicity. When used as a sealant filler, it can significantly reduce the water absorption rate of the sealant after being immersed in water. In addition, the dry-modified nano-calcium carbonate contains boron element, which decomposes when heated to produce boric anhydride or boric acid to form a glassy melt that covers the surface of the material, isolating the propagation of oxygen and heat, inhibiting the generation of thick smoke, and improving the flame retardant properties of the sealant.

[0019] As a preferred technical solution of the present invention, the process of plasma treatment in step S3 is: placing the modified nano-calcium carbonate II in a low-temperature plasma treatment instrument for treatment for 10 to 15 minutes; preferably, the atmosphere of the low-temperature plasma treatment instrument is argon; preferably, the frequency of the low-temperature plasma treatment instrument is 40 to 70KHz, the power is 35 to 80W, and the pressure is 30 to 80Pa.

[0020] The plasma-treated nano-calcium carbonate has good dispersibility and improved compatibility with the organic polymer of the silane-modified polyether sealant. The evenly dispersed modified nano-calcium carbonate can hinder and passivate the crack propagation of the polymer matrix, thereby avoiding destructive cracking and enabling the composite material to withstand higher loads. When subjected to external forces, stress concentration points are formed, generating stress crazing to absorb external energy, which is manifested macroscopically as a significant increase in the tensile strength and elongation at break of the sealant.

[0021] In a second aspect, the present invention provides nano calcium carbonate for silane-modified polyether sealant prepared by the method described in the first aspect.

[0022] Preferably, the use of the nano-calcium carbonate in a silane-modified polyether sealant comprises the following steps: mixing 80 to 100 parts of a silane-modified polyether polymer, 40 to 50 parts of diisononyl phthalate, and 150 to 200 parts of nano-calcium carbonate, blending at a temperature of 70° C. to 130° C. for 1 to 3 hours, cooling to room temperature, adding 3 to 5 parts of a coupling agent and 1 to 3 parts of a catalyst, and reacting under vacuum conditions for 0.5 to 1.5 hours to obtain a silane-modified polyether sealant.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The present invention sequentially performs wet modification, dry modification, and plasma treatment on nano-calcium carbonate, wherein the wet modification introduces amino groups, the dry modification introduces boric acid esters, and the plasma treatment improves the dispersibility. The combined effect improves the tensile strength and elongation at break of the sealant and effectively reduces the water absorption rate.

[0025] (2) The silane-modified polyether sealant of the present invention contains three elements: silicon, nitrogen and boron. Silicon can form a dense and stable silicon-carbon layer on the surface of the substrate to prevent the escape of combustible substances. Nitrogen can combine with free radicals generated by combustion to block the chain reaction and thus slow down the combustion process. Boron can form a protective layer to isolate the propagation of oxygen and heat and inhibit the generation of thick smoke. The flame retardant level of the sealant is improved through the synergistic effect of silicon-nitrogen-boron. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a performance test data chart. DETAILED DESCRIPTION

[0027] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0028] The sources of some components in the application examples and comparative examples are as follows:

[0029] Preparation of modified nano-calcium carbonate I: Weigh 100 parts of nano-calcium carbonate (CAS No. 471-34-1), add it to 500 parts of anhydrous ethanol (CAS No. 364-17-5), and ultrasonically disperse it for 2 hours to obtain a nano-calcium carbonate suspension; add 20 parts of DL-alanine (CAS No. 302-72-7) modifier to the nano-calcium carbonate suspension, heat it to 80°C and stir it for 0.5 hours, and obtain modified nano-calcium carbonate I after filtration, washing and drying.

[0030] Preparation of modified nano-calcium carbonate II: Add 200 parts of modified nano-calcium carbonate I into a mixer, stir and heat up. When the temperature reaches 80°C, add 20 parts of triethanolamine borate (CAS No. 283-56-7), heat to 130°C and stir for 2 hours. After sieving, obtain modified nano-calcium carbonate II.

[0031] Preparation of nano-calcium carbonate for silane-modified polyether sealant: The modified nano-calcium carbonate II is placed in a low-temperature plasma treatment instrument for 10 to 15 minutes. The frequency of the low-temperature plasma treatment instrument is 70KHz, the power is 80W, the pressure is 30Pa, and the atmosphere is argon to obtain nano-calcium carbonate for silane-modified polyether sealant.

[0032] Preparation of dry modified nano calcium carbonate: 200 parts of nano calcium carbonate (CAS No. 471-34-1) are put into a mixer and stirred and heated. When the temperature reaches 80°C, 20 parts of triethanolamine borate (CAS No. 283-56-7) are added, the temperature is raised to 130°C and stirred for 2 hours. After sieving, dry modified nano calcium carbonate is obtained.

[0033] Preparation of plasma-modified nano-calcium carbonate: Nano-calcium carbonate (CAS No. 471-34-1) is placed in a low-temperature plasma treatment apparatus for 10 to 15 minutes. The frequency of the low-temperature plasma treatment apparatus is 70KHz, the power is 80W, the pressure is 30Pa, and the atmosphere is argon to obtain plasma-modified nano-calcium carbonate.

[0034] Silane-modified polyether polymer: brand S303H, purchased from Kaneka Chemical Industry Co., Ltd., Japan;

[0035] Diisononyl phthalate: CAS number is 28553-12-0;

[0036] Nano calcium carbonate: CAS number is 471-34-1;

[0037] Coupling agent: silane coupling agent KH-792, CAS number is 1760-24-3;

[0038] Catalyst: Catalyst chelated tin U-220H was purchased from Nitto Kasei Sangyo Co., Ltd., Japan.

[0039] Application Example 1

[0040] The present application embodiment provides a silane-modified polyether sealant. The preparation of the silane-modified polyether sealant includes the following steps: 100 parts of silane-modified polyether polymer, 50 parts of diisononyl phthalate, and 200 parts of nano-calcium carbonate for silane-modified polyether sealant are mixed, blended at a temperature of 130° C. for 3 hours, cooled to room temperature, and then 5 parts of silane coupling agent KH-792 and 3 parts of catalyst chelated tin U-220H are added, and the mixture is reacted under vacuum conditions for 1.5 hours to obtain the silane-modified polyether sealant.

[0041] Application Example 2

[0042] The present application embodiment provides a silane-modified polyether sealant. The preparation of the silane-modified polyether sealant includes the following steps: 80 parts of silane-modified polyether polymer, 40 parts of diisononyl phthalate, and 150 parts of nano-calcium carbonate for silane-modified polyether sealant are mixed, blended at a temperature of 70°C for 1 hour, cooled to room temperature, and then 3 parts of silane coupling agent KH-792 and 1 part of catalyst chelated tin U-220H are added, and the mixture is reacted under vacuum conditions for 0.5 hour to obtain the silane-modified polyether sealant.

[0043] Application Example 3

[0044] The present application embodiment provides a silane-modified polyether sealant. The preparation of the silane-modified polyether sealant includes the following steps: 85 parts of a silane-modified polyether polymer, 48 parts of diisononyl phthalate, and 170 parts of nano-calcium carbonate for silane-modified polyether sealant are mixed, blended at a temperature of 110° C. for 2 hours, cooled to room temperature, and then 4 parts of a silane coupling agent KH-792 and 2 parts of a catalyst chelated tin U-220H are added, and the mixture is reacted under vacuum conditions for 1.2 hours to obtain the silane-modified polyether sealant.

[0045] Application Example 4

[0046] This application example provides a silane-modified polyether sealant, which is different from application example 1 only in that the nano-calcium carbonate used in the silane-modified polyether sealant is replaced by modified nano-calcium carbonate II.

[0047] Application Example 5

[0048] This application example provides a silane-modified polyether sealant, which is different from application example 1 only in that the nano-calcium carbonate used in the silane-modified polyether sealant is replaced by modified nano-calcium carbonate I.

[0049] Application Comparative Example 1

[0050] This application comparison example provides a silane-modified polyether sealant. The preparation of the silane-modified polyether sealant includes the following steps: 100 parts of silane-modified polyether polymer, 50 parts of diisononyl phthalate, and 200 parts of nano calcium carbonate (CAS No. 471-34-1) are mixed, blended at a temperature of 130°C for 3 hours, cooled to room temperature, and then 5 parts of silane coupling agent KH-792 and 3 parts of catalyst chelated tin U-220H are added, and the mixture is reacted under vacuum conditions for 1.5 hours to obtain the silane-modified polyether sealant.

[0051] Application Comparative Example 2

[0052] This application comparison example provides a silane-modified polyether sealant, which is different from application comparison example 1 only in that nano calcium carbonate (CAS No. 471-34-1) is replaced by dry-modified nano calcium carbonate in this application comparison example, and the rest is the same as application comparison example 1.

[0053] Application Comparative Example 3

[0054] This application comparison example provides a silane-modified polyether sealant, which is different from application comparison example 1 only in that nano calcium carbonate (CAS No. 471-34-1) is replaced by plasma-modified nano calcium carbonate in this application comparison example, and the rest is the same as application comparison example 1.

[0055] The performance of the silane-modified polyether sealant provided in the above application examples and application comparison examples was tested, and the testing method was as follows:

[0056] Tensile strength and elongation at break: Tested in accordance with the requirements of GB / T 528-2009 Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber.

[0057] Water absorption: Test according to the requirements of ASTM D570 Standard Test Method for Water Absorption of Plastics.

[0058] Flame retardant performance: Tested in accordance with the requirements of GB / T 2408-2021 Horizontal and vertical methods for determination of combustion performance of plastics.

[0059] The above performance test data is as follows Figure 1 shown.

[0060] From the above content, it can be seen that in the present invention, nano calcium carbonate is subjected to wet modification, dry modification and plasma treatment in sequence, and nano calcium carbonate for silane-modified polyether sealant is obtained through multiple modification treatments, and the prepared silane-modified polyether sealant has a tensile strength of 1.51-1.53 ​​MPa, an elongation at break of 442-446%, a water absorption of 1.8-1.9%, and a flame retardant grade of V-0.

[0061] Compared with Example 1, if modified nano-calcium carbonate II is used, the tensile strength and elongation at break decrease (Example 4); compared with Example 1, if modified nano-calcium carbonate I is used, the tensile strength and elongation at break decrease, the water absorption rate increases, and the flame retardant performance decreases (Example 5).

[0062] Comparative Example 1 does not adopt the technical innovation of the present invention, so the performance is poor, the tensile strength is 1.24MPa, the elongation at break is 321%, the water absorption rate is 3.2%, and the flame retardant grade is V-2; compared with Comparative Example 1, if dry-modified nano-calcium carbonate is used, the water absorption rate is reduced and the flame retardant performance is improved (Comparative Example 2); compared with Comparative Example 1, if plasma-modified nano-calcium carbonate is used, the tensile strength and elongation at break are improved (Comparative Example 3).

[0063] In summary, the present invention sequentially performs wet modification, dry modification, and plasma treatment on nano-calcium carbonate to obtain nano-calcium carbonate for silane-modified polyether sealant through multiple modification treatments, and the prepared silane-modified polyether sealant has excellent tensile strength and elongation at break, lower water absorption, and improved flame retardant properties.

[0064] The applicant declares that the present invention illustrates the detailed process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing nano calcium carbonate for silane-modified polyether sealant, characterized in that: The following steps are involved: Step S1: wet-modifying nano-calcium carbonate to obtain modified nano-calcium carbonate I; Step S2: dry-modifying the modified nano-calcium carbonate I described in step S1 to obtain modified nano-calcium carbonate II; Step S3: performing plasma treatment on the modified nano-calcium carbonate II described in step S2 to obtain nano-calcium carbonate for silane-modified polyether sealant; The wet modification process in step S1 is as follows: weigh 80-100 parts of nano-calcium carbonate, add them to 400-500 parts of anhydrous ethanol, and disperse them by ultrasonic for 2 hours to obtain a nano-calcium carbonate suspension; add 10-20 parts of alanine modifier to the nano-calcium carbonate suspension, heat it to 70-80° C., stir it for 0.5 hours, and obtain modified nano-calcium carbonate I after suction filtration, washing and drying; The alanine modifier is selected from any one of DL-alanine, D-alanine, and L-alanine, or a combination of at least two thereof; The dry modification process in step S2 is as follows: 150-200 parts of modified nano-calcium carbonate I are added into a stirrer, stirred and heated; when the temperature reaches 80-90° C., 20-30 parts of a borate modifier are added, the temperature is raised to 110-130° C., stirred for 2 hours, and sieved to obtain modified nano-calcium carbonate II; The borate modifier is selected from any one of triethanolamine borate, diethanolamine borate, and triphenyl borate, or a combination of at least two thereof; The plasma treatment process in step S3 is as follows: placing the modified nano-calcium carbonate II in a low-temperature plasma treatment apparatus for 10 to 15 minutes; The atmosphere of the low-temperature plasma treatment instrument is argon; The low-temperature plasma treatment instrument has a frequency of 40 to 70 KHz, a power of 35 to 80 W, and a pressure of 30 to 80 Pa.

2. A nano calcium carbonate for silane-modified polyether sealant, characterized in that: Prepared according to the preparation method described in claim 1.

3. The nano calcium carbonate for silane-modified polyether sealant according to claim 2, characterized in that: The application of the nano-calcium carbonate in the silane-modified polyether sealant comprises the following steps: 80-100 parts of a silane-modified polyether polymer, 40-50 parts of diisononyl phthalate and 150-200 parts of nano-calcium carbonate are mixed, blended at a temperature of 70°C-130°C for 1-3 hours, cooled to room temperature, then 3-5 parts of a coupling agent and 1-3 parts of a catalyst are added, reacted under vacuum conditions for 0.5-1.5 hours, and the silane-modified polyether sealant is obtained.