Well wall strengthening agent composition and water-based drilling fluid and preparation method thereof

By using multi-stage sealing technology of cationic emulsified asphalt, ceramic powder and nanomaterials in water-based drilling fluid, the problems of well wall collapse and liquid phase invasion in deep coalbed methane horizontal wells are solved, and coal rock cleavage and The effective sealing and suppression of micro-slits improves the stability of the well wall and the sealing ability of drilling fluid.

CN118652671BActive Publication Date: 2024-11-12SHAANXI YANCHANG PETROLEUM GRP
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411103196.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-12
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

In deep coalbed methane horizontal well drilling, existing water-based drilling fluid is difficult to effectively block coal rock cleavage and micro-chambers, resulting in liquid phase invasion and wellbore collapse, and insufficient inhibitory and stability on coal gangue-containing coal.

Method used

A well wall reinforcement composition is prepared by using multi-stage sealing technology of cationic emulsified asphalt + film-forming anti-collapse, ceramic powder microparticles + cationically modified nanorigid particles + nanoemulsion flexible particles + chopped fibers, combined with pre-stage Hydrating bentonite slurry, potassium salt inhibitors and lubricants to form a water-based drilling fluid with moderate inhibition and strengthening sealing capabilities.

Benefits of technology

This water-based drilling fluid can effectively block micro-nano pores and cracks, inhibit the hydration of coal gangue, maintain the stability of the well wall, and significantly improve the drilling safety and stability of deep coalbed methane horizontal wells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention discloses a well wall strengthener composition and a water-based drilling fluid and a preparation method thereof, and relates to the technical field of coal bed methane drilling. The well wall strengthener composition is composed of the following components in parts by weight: 1-3 parts of cationic modified nano plugging agent, 1-3 parts of nanoemulsion, 2-6 parts of ceramic powder, and 1-3 parts of chopped fibers; the cationic modified nano plugging agent is composed of the following components in parts by weight: 20-30 parts of nano silicon dioxide, 20-30 parts of silane coupling agent, 8-12 parts of substituent, 10-15 parts of catalyst A, 5-10 parts of initiator, 30-40 parts of ionic liquid, 1-3 parts of catalyst B, and 15-20 parts of non-ionic monomer; the present invention also discloses a drilling fluid prepared by the well wall strengthener composition and a preparation method thereof. The well wall strengthener composition provided by the present invention has certain plugging properties, and the drilling fluid provided has excellent anti-collapse and plugging capabilities for coal rock cleats and micro-cracks, and is suitable for the long horizontal section drilling needs of deep coal bed methane horizontal wells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coalbed methane drilling, and in particular relates to a well wall strengthening agent composition and a water-based drilling fluid and a preparation method thereof. Background Art

[0002] How to improve the ability of water-based drilling fluid to plug coal-rock cleats and micro-cracks, prevent liquid intrusion, and prevent wellbore collapse in coalbed methane horizontal well drilling is the prerequisite for the successful use of water-based drilling fluid and ensuring safe drilling. At present, for deep coalbed methane horizontal well drilling operations, the water-based drilling fluid systems developed include strong plugging hydrophobic high-performance water-based drilling fluid, solid-free brine drilling fluid, and clean polyfilm drilling fluid. The patent "A Strong Plug Hydrophobic High-Performance Water-Based Drilling Fluid" (ZL202010633201.0) uses polymer-coated inhibitors prepared from alkyl carbonate, acrylamide, acrylic acid, and alkylamino acrylate monomers, anti-collapse agents prepared from hydrophobic functional monomers, acrylamide, and nano-silica, and lubricants prepared from nano-ferric oxide, hydrophobic monomers, acrylamide, and acrylic acid as the main components to prepare a strong plugging hydrophobic high-performance water-based drilling fluid with strong inhibition and plugging properties. The patent "A clean polyfilm drilling fluid for coalbed methane and its preparation method" (ZL201610828822.8) mainly uses polyacrylic polyurethane film former, methacrylate copolymer solidifying agent, and polyacrylic polymer emulsion strong film agent as the core to establish a clean polyfilm drilling fluid, which forms a consolidation and plugging film on the surface of the coal seam to prevent the coal seam from collapsing. However, the patents do not explain the inhibitory, plugging and well wall stabilization capabilities of coal seams containing coal gangue, and the application effect in deep coalbed methane horizontal wells needs further verification. Summary of the invention

[0003] The present invention provides a well wall strengthening agent composition and a water-based drilling fluid and a preparation method thereof. The provided drilling fluid has the ability of "moderate inhibition and enhanced plugging". Through multi-stage plugging of cationic emulsified asphalt + film-forming anti-collapse, ceramic powder micron particles + cationic modified nano rigid particles + nano emulsion flexible particles + chopped fibers, the drilling fluid can effectively plug micro-nano pores to prevent liquid phase from invading coal rock formations, and has certain inhibitory properties to inhibit the hydration of coal gangue in coal rock. It can be applied to coalbed methane horizontal well drilling to effectively plug micro-nano pores and cracks and keep the well wall stable.

[0004] A well wall strengthening agent composition, composed of the following components in parts by weight: 1-3 parts of cationic modified nano plugging agent, 1-3 parts of nanoemulsion, 2-6 parts of ceramic powder, and 1-3 parts of chopped fibers;

[0005] The cationic modified nano plugging agent is composed of the following components in parts by weight: 20-30 parts of nano silicon dioxide, 20-30 parts of silane coupling agent, 8-12 parts of substituent, 10-15 parts of catalyst A, 5-10 parts of initiator, 30-40 parts of ionic liquid, 1-3 parts of catalyst B, and 15-20 parts of non-ionic monomer; the catalyst A is triethylamine; the catalyst B is C-94;

[0006] The ionic liquid is one or two of N-ethylpyridinium hexafluorophosphate, 1-butyl-3-methylimidazolium bromide, 1-octyl-3-methylimidazolium trifluoromethanesulfonate, and 1-butyl-3-methylimidazolium methyl sulfate.

[0007] Preferably, the well wall strengthener composition is composed of the following components in parts by weight: 1 part of cationic modified nano plugging agent, 1 part of nanoemulsion, 2 parts of ceramic powder, and 1 part of chopped fiber; wherein the cationic modified nano plugging agent is composed of the following components in parts by weight: 23 parts of nano silicon dioxide, 25 parts of silane coupling agent, 12 parts of substituent, 10 parts of catalyst A, 7 parts of initiator, 40 parts of ionic liquid, 3 parts of catalyst B, and 20 parts of non-ionic monomer; wherein the ionic liquid is 1-butyl-3-methylimidazolium bromide and 1-octyl-3-methylimidazolium trifluoromethane sulfonate, and the weight ratio thereof is 4:6.

[0008] Preferably, the preparation method of the cationic modified nano plugging agent is:

[0009] (1) Dispersing nano-silicon dioxide to obtain a uniform suspension;

[0010] (2) adding a silane coupling agent dropwise into the uniform suspension to obtain amino-modified nano-silica particles;

[0011] (3) adding the amino-modified nano-silica particles into toluene for dispersion, adding a substituent and a catalyst A for condensation reaction and purification, thereby obtaining purified modified nano-silica particles;

[0012] (4) The purified and modified nano-silica particles and the initiator are dissolved in deionized water to prepare a solution with a mass concentration of 30%. After deoxygenation, non-ionic monomers are added under nitrogen protection to cause free radical polymerization. Ionic liquid and catalyst B are then added in sequence to prepare a cationic modified nano-plugging agent after a condensation reaction.

[0013] Preferably, the ceramic powder is a ceramic powder with a particle size of 2.0-6.8 μm and a core-shell structure, which is specifically obtained by subjecting ceramic powder to nitridation treatment at 800-1200° C.; the chopped fibers are polyester fibers, mineral fibers or cotton fibers with a length of 0.1-0.5 mm.

[0014] Preferably, the nanoemulsion is prepared by mixing solid paraffin, white oil, emulsifier and water in a weight ratio of 2:2:1:5; the emulsifier is composed of Tween 80:Span 80 in a weight ratio of 56:44.

[0015] A method for preparing a well wall strengthening agent composition comprises mixing a cationic modified nano plugging agent, a nano emulsion, a ceramic powder and chopped fibers, stirring the mixture at a stirring speed of 2000 rpm for 2 hours to obtain the well wall strengthening agent composition.

[0016] A water-based drilling fluid comprises the following components in parts by weight: 80-100 parts of prehydrated bentonite slurry, 7-12 parts of potassium salt inhibitor, 2-5 parts of fluid loss reducer, 2-5 parts of anti-collapse agent composition, 5-10 parts of the above-mentioned well wall strengthening agent composition, 2-3 parts of lubricant, and 10-50 parts of weighting agent.

[0017] Preferably, the prehydrated bentonite slurry is prepared by adding 3 parts of bentonite and 0.2 parts of Na2CO3 to 100 parts of water and standing for 24 hours; the potassium salt inhibitor is KCl or KCOOH; the filtration loss reducer is polyanionic cellulose, carboxymethyl cellulose, carboxymethyl starch or hydroxyethyl starch; the anti-collapse agent composition is obtained by uniformly mixing cationic emulsified asphalt and a film-forming agent in a weight ratio of 1:1; the lubricant is an extreme pressure lubricant; and the weighting agent is limestone powder with a particle size of 38 μm.

[0018] A method for preparing a water-based drilling fluid comprises the following steps: sequentially adding a fluid loss reducer, a potassium salt inhibitor, an anti-collapse agent composition, a well wall strengthening agent composition and a lubricant to a prehydrated bentonite slurry, mixing them uniformly, adjusting the pH value to 8-9, adding a weighting agent, and mixing them uniformly to obtain a water-based drilling fluid.

[0019] Preferably, the method for preparing the cationic emulsified asphalt is as follows: 1) heating and melting 100 parts of base asphalt, adding 5 parts of nano-SiO2-lignin complex for ultrasonic dispersion; 2) mixing 1.5 parts of stabilizer calcium chloride and 100 parts of water, adding 5 parts of cationic emulsifier octadecyltrimethylammonium chloride at 70°C, mixing evenly, and adjusting the pH to 3; 3) simultaneously passing the obtained products of step 1) and step 2) through a colloid mill for emulsification to obtain cationic emulsified asphalt;

[0020] The preparation method of the film-forming agent is as follows: 25 parts of polycaprolactone are added into a reaction kettle, vacuum dehydrated at 120° C. for 2 hours, 25 parts of isophorone diisocyanate are added after the temperature is reduced to 80° C., reacted for 3 hours, cooled to 70° C., 8 parts of dimethylolpropionic acid are added, reacted for 2 hours, cooled to 60° C., reacted for 1.5 hours, cooled to 40° C., 25 parts of methyl methacrylate and 15 parts of 2-acrylamido-2-methylpropanesulfonic acid are added, stirred for 0.5 hours, 30 parts of deionized water are added for high-speed emulsification and dispersion, 4 parts of initiator potassium persulfate are added, free radical polymerization is carried out at 80° C. for 3.5 hours, and the material is cooled and discharged to obtain the film-forming agent.

[0021] Advantages of the present invention:

[0022] In order to solve the problem of wellbore collapse during the drilling of deep coalbed methane horizontal wells, the wellbore strengthening agent composition provided by the present invention has strong adsorption with coal rock, and adopts the multi-stage plugging effect of ceramic powder micron particles + cationic modified nano rigid particles + nanoemulsion flexible particles + chopped fibers to strengthen the plugging ability of coal rock cleats and micro cracks. The water-based drilling fluid prepared on this basis has the ability of "cation moderate inhibition, multi-stage particle enhanced plugging". On the basis of inhibiting the hydration of clay minerals in coal gangue, the cementation of coal rock and coal gangue cleats and micro cracks is improved through cationic emulsified asphalt + film-forming agent. The water-based drilling fluid strengthens the stabilizing effect of coalbed methane horizontal wellbore wall under multiple effects, which can be applied to the drilling needs of long horizontal sections of deep coalbed methane horizontal wells. DETAILED DESCRIPTION

[0023] Example 1

[0024] 1. A well wall strengthening agent composition, composed of the following components in parts by weight: 2 parts of cationic modified nano plugging agent, 3 parts of nanoemulsion, 4 parts of ceramic powder, and 3 parts of chopped fibers;

[0025] The cationic modified nano plugging agent is composed of the following components in parts by weight: 20 parts of nano silicon dioxide, 20 parts of silane coupling agent, 10 parts of substituent, 10 parts of catalyst A, 5 parts of initiator, 35 parts of ionic liquid, 3 parts of catalyst B, and 15 parts of non-ionic monomer;

[0026] The ionic liquid is 1-butyl-3-methylimidazolium bromide; the silane coupling agent is γ-aminopropyltriethoxysilane coupling agent; the nonionic monomer is p-styrene; the substituent is 2-bromoisobutyryl; the catalyst A is triethylamine; the catalyst B is C-94, C-94 is a titanium / silicon oxide copolymer, wherein the molar mass ratio of Ti / Si is 9:1; the initiator is cuprous bromide;

[0027] The preparation method of the cationic modified nano plugging agent comprises the following steps:

[0028] (1) 70 nanometers of silica was dispersed in toluene to obtain a uniform suspension;

[0029] (2) adding the silane coupling agent dropwise into the uniform suspension and reacting at 85°C for 2 h to obtain amino-modified nano-silica particles;

[0030] (3) Add the amino-modified nano-silica particles into toluene for dispersion, add the substituent and catalyst A thereto for condensation reaction, add sufficient acetone for precipitation, filter, and dry in a vacuum environment at 80°C for 8 hours to obtain purified modified nano-silica particles;

[0031] (4) The purified and modified nano-silica particles and the initiator were dissolved in deionized water to prepare a solution with a mass concentration of 30%. After deoxygenation, non-ionic monomers were added under nitrogen protection, and free radical polymerization was carried out at a stirring speed of 1500 rpm for 5 hours. Then, ionic liquid and catalyst B were added in sequence, and a cationic modified nano-plugging agent was prepared after a condensation reaction for 2 hours.

[0032] The ceramic powder is a ceramic powder with a particle size of 5 μm, hard outside and tough inside, and has a core-shell structure, and is specifically obtained by subjecting ceramic powder to nitridation treatment at 800° C.; the chopped fibers are cotton fibers with a length of 0.2 mm;

[0033] The nanoemulsion is prepared by mixing solid paraffin, white oil, emulsifier and water in a weight ratio of 2:2:1:5; the emulsifier is composed of Tween 80 and Span 80 in a weight ratio of 56:44.

[0034] 2. The preparation method of the well wall strengthening agent composition is as follows: the cationic modified nano plugging agent, nanoemulsion, ceramic powder and chopped fibers are mixed and stirred at a stirring speed of 2000 rpm for 2 hours to obtain the well wall strengthening agent composition.

[0035] Example 2

[0036] 1. A well wall strengthening agent composition, composed of the following components in parts by weight: 3 parts of cationic modified nano plugging agent, 1 part of nanoemulsion, 4 parts of ceramic powder, and 2 parts of chopped fibers;

[0037] The cationic modified nano plugging agent is composed of the following components in parts by weight: 30 parts of nano silicon dioxide, 30 parts of silane coupling agent, 8 parts of substituent, 15 parts of catalyst A, 7 parts of initiator, 35 parts of ionic liquid, 2 parts of catalyst B, and 20 parts of non-ionic monomer;

[0038] The ionic liquid is N-ethylpyridinium hexafluorophosphate; the silane coupling agent is aniline methyl trimethoxy silane;

[0039] The nonionic monomer, substituent, catalyst A, catalyst B, and initiator are the same as those in Example 1;

[0040] The preparation method of the cationic modified nano plugging agent is the same as that of Example 1;

[0041] The ceramic powder is a ceramic powder with a particle size of 3.4 μm, hard outside and tough inside, and has a core-shell structure, and is specifically obtained by subjecting ceramic powder to a nitriding treatment at 1200° C.; the chopped fibers are mineral fibers with a length of 0.1 mm;

[0042] The nanoemulsion is prepared by mixing solid paraffin, white oil, emulsifier and water in a weight ratio of 2:2:1:5; the emulsifier is composed of Tween 80 and Span 80 in a weight ratio of 56:44.

[0043] 2. The preparation method of the well wall strengthening agent composition is the same as that in Example 1.

[0044] Example 3

[0045] 1. A well wall strengthening agent composition, composed of the following components in parts by weight: 2 parts of cationic modified nano plugging agent, 2 parts of nanoemulsion, 6 parts of ceramic powder, and 1 part of chopped fiber;

[0046] The cationic modified nano plugging agent is composed of the following components in parts by weight: 27 parts of nano silicon dioxide, 24 parts of silane coupling agent, 12 parts of substituent, 13 parts of catalyst A, 10 parts of initiator, 30 parts of ionic liquid, 1 part of catalyst B, and 20 parts of non-ionic monomer;

[0047] The ionic liquid is 1-octyl-3-methylimidazole trifluoromethanesulfonate; the silane coupling agent is γ-aminopropyltrimethoxysilane; the nonionic monomer is styrene; the substituent is 2-bromoisobutyryl; the catalyst A is triethylamine; the catalyst B is C-94, which is a titanium / silicon oxide copolymer, wherein the molar mass ratio of Ti / Si is 9:1; and the initiator is cuprous bromide;

[0048] The preparation method of the cationic modified nano plugging agent comprises the following steps:

[0049] (1) 100 nanometers of silica was dispersed in toluene to obtain a uniform suspension;

[0050] (2) adding the silane coupling agent dropwise into the uniform suspension and reacting at 85°C for 2 h to obtain amino-modified nano-silica particles;

[0051] (3) Add the amino-modified nano-silica particles into toluene for dispersion, add the substituent and catalyst A thereto for condensation reaction, add sufficient acetone for precipitation, filter, and dry in a vacuum environment at 80°C for 8 hours to obtain purified modified nano-silica particles;

[0052] (4) The purified and modified nano-silica particles and the initiator were dissolved in deionized water to prepare a solution with a mass concentration of 30%. After deoxygenation, non-ionic monomers were added under nitrogen protection, and free radical polymerization was carried out at a stirring speed of 2000 rpm for 4 hours. Then, ionic liquid and catalyst B were added in sequence, and a cationic modified nano-plugging agent was prepared after a condensation reaction for 2 hours.

[0053] The ceramic powder is a ceramic powder with a particle size of 6.8 μm, hard outside and tough inside, and has a core-shell structure, and is specifically obtained by subjecting ceramic powder to nitridation treatment at 800° C.; the chopped fibers are mineral fibers with a length of 0.2 mm;

[0054] The nanoemulsion is prepared by mixing solid paraffin, white oil, emulsifier and water in a weight ratio of 2:2:1:5; the emulsifier is composed of Tween 80 and Span 80 in a weight ratio of 56:44.

[0055] 2. The preparation method of the well wall strengthening agent composition is the same as that in Example 1.

[0056] Example 4

[0057] 1. A well wall strengthening agent composition, composed of the following components in parts by weight: 1 part of cationic modified nano plugging agent, 1 part of nanoemulsion, 2 parts of ceramic powder, and 3 parts of chopped fibers;

[0058] The cationic modified nano plugging agent is composed of the following components in parts by weight: 27 parts of nano silicon dioxide, 25 parts of silane coupling agent, 10 parts of substituent, 12 parts of catalyst A, 7 parts of initiator, 38 parts of ionic liquid, 2 parts of catalyst B, and 17 parts of non-ionic monomer;

[0059] The ionic liquid is 1-butyl-3-methylimidazole methyl sulfate; the silane coupling agent is aniline methyl trimethoxy silane;

[0060] The nonionic monomer, substituent, catalyst A, catalyst B, and initiator are the same as those in Example 3;

[0061] The preparation method of the cationic modified nano plugging agent is the same as that of Example 3;

[0062] The ceramic powder is a ceramic powder with a particle size of 2 μm, hard outside and tough inside, and has a core-shell structure, and is specifically obtained by subjecting ceramic powder to nitridation treatment at 1000° C.; the chopped fibers are polyester fibers with a length of 0.5 mm;

[0063] The nanoemulsion is prepared by mixing solid paraffin, white oil, emulsifier and water in a weight ratio of 2:2:1:5; the emulsifier is composed of Tween 80 and Span 80 in a weight ratio of 56:44.

[0064] 2. The preparation method of the well wall strengthening agent composition is the same as that in Example 1.

[0065] Example 5

[0066] 1. A well wall strengthening agent composition, composed of the following components in parts by weight: 1 part of cationic modified nano plugging agent, 1 part of nanoemulsion, 2 parts of ceramic powder, and 1 part of chopped fiber;

[0067] A cationic modified nano plugging agent, composed of the following components in parts by weight: 23 parts of nano silicon dioxide, 25 parts of silane coupling agent, 12 parts of substituent, 10 parts of catalyst A, 7 parts of initiator, 40 parts of ionic liquid, 3 parts of catalyst B, and 20 parts of non-ionic monomer;

[0068] The ionic liquid is 1-butyl-3-methylimidazolium bromide and 1-octyl-3-methylimidazolium trifluoromethanesulfonate, with a weight ratio of 4:6;

[0069] The silane coupling agent, substituent, catalyst A, initiator, catalyst B, and nonionic monomer are the same as those in Example 3;

[0070] The preparation method of the cationic modified nano plugging agent is the same as that of Example 3;

[0071] The ceramic powder, chopped fibers and nanoemulsion are the same as those in Example 3.

[0072] 2. The preparation method of the well wall strengthening agent composition is the same as that in Example 1.

[0073] Comparative Example 1

[0074] No cationic modified nano plugging agent is added to the well wall strengthening agent composition, and the rest is the same as in Example 5.

[0075] Comparative Example 2

[0076] The cationic modified nano plugging agent was replaced with amino-modified nano silica particles, and the rest was the same as in Example 5.

[0077] Comparative Example 3

[0078] The well wall strengthening agent composition does not include cationic modified nano plugging agent, ceramic powder, and chopped fibers, and the rest is the same as in Example 5, specifically:

[0079] A well wall strengthening agent composition, comprising the following components in parts by weight: 1 part of nanoemulsion;

[0080] The nanoemulsion is prepared by mixing solid paraffin, white oil, emulsifier and water in a weight ratio of 2:2:1:5; the emulsifier is composed of Tween 80 and Span 80 in a weight ratio of 56:44.

[0081] Comparative Example 4

[0082] The ceramic powder was not subjected to the 800° C. nitridation process, and the rest was the same as in Example 5.

[0083] Comparative Example 5

[0084] The chopped fibers were replaced with mineral fibers having a length of 1 mm, and the rest were the same as in Example 5.

[0085] Performance testing:

[0086] The well wall strengthening agent compositions of Examples 1-5 and Comparative Examples 1-5 were evaluated as follows: plugging rate test and uniaxial compressive strength test.

[0087] 1. Blockage rate test

[0088] The plugging rate was evaluated using a low permeability sand disk plugging instrument, and the test conditions were 120°C and a pressure difference of 3.5 MPa for 30 minutes. Take 5 parts of the well wall strengthening agent composition prepared in Examples 1-5 and Comparative Examples 1-5, place it in 90 parts of deionized water, and prepare it into a solution. After hot rolling aging at 105°C / 16h, take it out and place it in the plugging instrument kettle. The plugging rate calculation method is to test the original permeability P0 of the simulated core, and the permeability of the core after the plugging agent solution acts is P1, then the plugging rate R0=(P0-P1) / P0×100%, and the experimental results are shown in Table 1.

[0089] 2. Rock uniaxial compressive strength test

[0090] Coal rock was taken to make square coal rock cores of 35 mm × 35 mm × 15 mm in size, and the uniaxial compressive strength of the original rock, original rock + clean water, and original rock + well wall strengthening agent combination after immersion for 16 hours was tested. The results are shown in Table 1;

[0091] Table 1 The plugging rate of the wellbore strengthening agent composition and the image evaluation results of the coal rock compressive strength

[0092]

[0093] It can be seen from the results in Table 1 that the wellbore strengthening agent compositions prepared in Examples 1-5 all have a certain plugging effect, among which Example 5 has the best plugging rate. The ability to strengthen the rock strength of coal rock was evaluated by soaking coal rock in different liquids. Compared with the original rock, the compressive strength of coal rock after water immersion was greatly reduced, and the uniaxial compressive strength of coal rock increased after soaking in the wellbore strengthening agent composition. Example 5 has the best effect. In the comparative example, the plugging rate and the compressive strength of coal rock were significantly reduced by removing or replacing the cationic modified nano plugging agent and changing the components of the wellbore strengthening agent composition.

[0094] Example 6

[0095] 1. A water-based drilling fluid comprising the following components in parts by weight: 90 parts of prehydrated bentonite slurry, 7 parts of potassium salt inhibitor, 2 parts of fluid loss reducer, 5 parts of anti-collapse agent composition, 5 parts of wellbore strengthening agent composition, 2 parts of lubricant, and 10 parts of weighting agent;

[0096] The well wall strengthening agent composition is the well wall strengthening agent composition described in Example 1;

[0097] The potassium salt inhibitor is KCl; the fluid loss reducer is polyanionic cellulose; the prehydrated bentonite slurry is prepared by adding 3 parts of bentonite and 0.2 parts of Na2CO3 to 100 parts of water and standing for 24 hours; the anti-collapse agent composition is prepared by mixing cationic emulsified asphalt and film-forming agent in a weight ratio of 1:1; the lubricant is an extreme pressure lubricant; the weighting agent is limestone powder with a particle size of 38 μm;

[0098] The preparation method of the cationic emulsified asphalt is as follows: 1) heating and melting 100 parts of base asphalt, adding 5 parts of nano-SiO2-lignin composite to perform ultrasonic dispersion; 2) mixing 1.5 parts of stabilizer calcium chloride and 100 parts of water, adding 5 parts of cationic emulsifier octadecyltrimethylammonium chloride at 70° C., mixing evenly, and adjusting the pH to 3; 3) simultaneously passing the obtained products of step 1) and step 2) through a colloid mill for emulsification to obtain cationic emulsified asphalt;

[0099] The preparation method of the film-forming agent is as follows: 25 parts of polycaprolactone are added into a reaction kettle, vacuum dehydrated at 120° C. for 2 hours, 25 parts of isophorone diisocyanate are added after the temperature is reduced to 80° C., reacted for 3 hours, cooled to 70° C., 8 parts of dimethylolpropionic acid are added, reacted for 2 hours, cooled to 60° C., reacted for 1.5 hours, cooled to 40° C., 25 parts of methyl methacrylate and 15 parts of 2-acrylamido-2-methylpropanesulfonic acid are added, stirred for 0.5 hours, 30 parts of deionized water are added for high-speed emulsification and dispersion, 4 parts of initiator potassium persulfate are added, free radical polymerization is carried out at 80° C. for 3.5 hours, and the material is cooled and discharged to obtain the film-forming agent.

[0100] 2. The preparation method of the water-based drilling fluid comprises the following steps: adding a filtrate reducer, a potassium salt inhibitor, an anti-collapse agent composition, a well wall strengthening agent composition and a lubricant to a prehydrated bentonite slurry in sequence, mixing them evenly at a stirring speed of 200 rpm, adding NaOH to adjust the pH value to 8, then adding a weighting agent, and stirring for 2 hours to obtain a water-based drilling fluid.

[0101] Example 7

[0102] 1. A water-based drilling fluid comprising the following components in parts by weight: 80 parts of prehydrated bentonite slurry, 7 parts of potassium salt inhibitor, 3 parts of fluid loss reducer, 2 parts of anti-collapse agent composition, 8 parts of wellbore strengthening agent composition, 3 parts of lubricant, and 50 parts of weighting agent;

[0103] The well wall strengthening agent composition is the well wall strengthening agent composition described in Example 5;

[0104] The potassium salt inhibitor is KCOOH; the fluid loss reducer is carboxymethyl cellulose;

[0105] The prehydrated bentonite slurry, anti-collapse agent composition, lubricant, weighting agent, and the preparation method of the cationic emulsified asphalt and the preparation method of the film-forming agent are the same as those in Example 6.

[0106] 2. The preparation method of the water-based drilling fluid comprises the following steps: adding a filtrate reducer, a potassium salt inhibitor, an anti-collapse agent composition, a well wall strengthening agent composition and a lubricant to a prehydrated bentonite slurry in sequence, mixing them evenly at a stirring speed of 200 rpm, adding NaOH to adjust the pH value to 8.5, adding a weighting agent, and stirring for 2 hours to obtain a water-based drilling fluid.

[0107] Example 8

[0108] 1. A water-based drilling fluid, comprising the following components in parts by weight: 100 parts of prehydrated bentonite slurry, 10 parts of potassium salt inhibitor, 5 parts of fluid loss reducer, 5 parts of anti-collapse agent composition, 10 parts of wellbore strengthening agent composition, 3 parts of lubricant, and 10 parts of weighting agent;

[0109] The well wall strengthening agent composition is the well wall strengthening agent composition described in Example 5;

[0110] The potassium salt inhibitor is KCOOH; the fluid loss reducer is carboxymethyl starch;

[0111] The prehydrated bentonite slurry, anti-collapse agent composition, lubricant, weighting agent, and the preparation method of the cationic emulsified asphalt and the preparation method of the film-forming agent are the same as those in Example 6.

[0112] 2. The preparation method of the water-based drilling fluid comprises the following steps: adding a filtrate reducer, a potassium salt inhibitor, an anti-collapse agent composition, a well wall strengthening agent composition and a lubricant to a prehydrated bentonite slurry in sequence, mixing them evenly at a stirring speed of 200 rpm, adding KOH to adjust the pH value to 9, then adding a weighting agent, and stirring for 2 hours to obtain a water-based drilling fluid.

[0113] Example 9

[0114] 1. A water-based drilling fluid, comprising the following components in parts by weight: 100 parts of prehydrated bentonite slurry, 12 parts of potassium salt inhibitor, 3 parts of fluid loss reducer, 3 parts of anti-collapse agent composition, 8 parts of wellbore strengthening agent composition, 2 parts of lubricant, and 30 parts of weighting agent;

[0115] The well wall strengthening agent composition is the well wall strengthening agent composition described in Example 2;

[0116] The potassium salt inhibitor is KCl; the fluid loss reducer is hydroxyethyl starch;

[0117] The prehydrated bentonite slurry, anti-collapse agent composition, lubricant, weighting agent, and the preparation method of the cationic emulsified asphalt and the preparation method of the film-forming agent are the same as those in Example 6.

[0118] 2. The preparation method of the water-based drilling fluid is the same as that in Example 8.

[0119] Comparative Example 6

[0120] The well wall strengthening agent composition of Comparative Example 1 was used, and the rest was the same as in Example 8.

[0121] Comparative Example 7

[0122] The well wall strengthening agent composition of Comparative Example 2 was used, and the rest was the same as in Example 8.

[0123] Comparative Example 8

[0124] The well wall strengthening agent composition of Comparative Example 3 was used, and the rest was the same as in Example 8.

[0125] Comparative Example 9

[0126] The well wall strengthening agent composition of Comparative Example 4 was used, and the rest was the same as in Example 8.

[0127] Comparative Example 10

[0128] The well wall strengthening agent composition of Comparative Example 5 was used, and the rest was the same as in Example 8.

[0129] Comparative Example 11

[0130] No cationic emulsified asphalt is added to the anti-collapse agent composition, and the rest is the same as in Example 8, specifically:

[0131] 1. A water-based drilling fluid, comprising the following components in parts by weight: 100 parts of prehydrated bentonite slurry, 10 parts of potassium salt inhibitor, 5 parts of fluid loss reducer, 5 parts of anti-collapse agent composition, 10 parts of wellbore strengthening agent composition, 3 parts of lubricant, and 10 parts of weighting agent;

[0132] The well wall strengthening agent composition is the well wall strengthening agent composition described in Example 5;

[0133] The potassium salt inhibitor is KCOOH; the fluid loss reducer is carboxymethyl starch;

[0134] The anti-collapse agent composition component is a film-forming agent;

[0135] The preparation method of the prehydrated bentonite slurry, lubricant, weighting agent and film-forming agent is the same as that of Example 6.

[0136] 2. The preparation method of the water-based drilling fluid comprises the following steps: adding a filtrate reducer, a potassium salt inhibitor, an anti-collapse agent composition, a well wall strengthening agent composition and a lubricant to a prehydrated bentonite slurry in sequence, mixing them evenly at a stirring speed of 200 rpm, adding KOH to adjust the pH value to 9, then adding a weighting agent, and stirring for 2 hours to obtain a water-based drilling fluid.

[0137] Performance testing:

[0138] The water-based drilling fluids of Examples 6-9 and Comparative Examples 6-11 were evaluated as follows: rolling recovery test, linear expansion test, rheological test, normal pressure filtration loss test, and plugging rate test. The test methods were based on the standards SY / T 5613-2016 Drilling fluid test - Test method for physical and chemical properties of shale, and GB / T 16783.1-2014 Field test of drilling fluids in the petroleum and natural gas industry - Part 1: Water-based drilling fluids.

[0139] 1. Rolling recovery rate test

[0140] (1) Core preparation

[0141] Select the outcrop core of the 7th layer of mudstone in the Zhangjiatan Yanchang Formation in the Ordos Basin, crush the core on a clean plastic plate or steel plate, and sieve it with a double-layer sample sieve with apertures of 6 mesh (3.2mm) and 10 mesh (2.0mm), and collect the core that passes through the 3.2mm sieve but does not pass through the 2.0mm sieve. Place the core in an oven at 105℃±3℃ and dry it to constant weight. Take 1000g of the dried core and store it in a wide-mouth bottle for later use;

[0142] (2) Test methods

[0143] First, weigh 50g (accurate to 0.1g) of the core prepared in the previous step, put it into a high-temperature aging tank containing 350mL of the drilling fluid prepared in Example 6-9 and Comparative Example 6-11, and cover it tightly. Place the aging tank with the sample in a roller heating furnace at 80℃±3℃, and roll it at a constant temperature for 16 hours. Take out the aging tank and cool it to room temperature. Transfer the liquid and rock sample in the tank to a 40-mesh (0.42mm) screen cloth, and rinse with tap water until the water is clear. Transfer the rock sample to a dried and weighed evaporating dish, and place it in a blast constant-temperature drying oven at 105℃±3℃ to keep it constant in weight. Take it out and put it in a dryer to cool to room temperature. The mass after weighing is m 2.

[0144] The calculation formula for rolling recovery rate is:

[0145] R = m 2 / 50×100% (Formula 1)

[0146] The results are shown in Table 2.

[0147] 2. Linear expansion rate test

[0148] The bentonite was sieved on a sieve with an aperture of 100 mesh (0.149 mm), and the bentonite that passed was collected and placed in a constant temperature drying oven at 105°C ± 3°C to maintain constant weight. The shale expansion test method in the standard SY / T 5613-2016 Drilling fluid test method for shale physical and chemical properties was used to record the expansion amounts for 2h and 16h, respectively. The results are shown in Table 2.

[0149] Table 2 Evaluation results of drilling fluid rolling recovery rate and linear expansion rate

[0150]

[0151] From the experimental results in Table 2, it can be seen that the rolling recovery rates of the drilling fluids prepared in Examples 6-9 are all above 90%, and the 16h linear expansion rate is less than 8%. Among them, the drilling fluid prepared in Example 8 has the best effect, with a rolling recovery rate of 97.8% and a 16h linear expansion rate as low as 4.78%. The rolling recovery rates of the drilling fluids in Comparative Examples 6-11 are reduced and the linear expansion is increased, indicating that the ability of the water-based drilling fluid system to inhibit the hydration, dispersion and expansion of clay minerals is reduced after changing the well wall strengthening agent composition and the anti-collapse agent composition.

[0152] 3. Drilling fluid rheology and atmospheric pressure filtration loss test

[0153] The test method and steps are based on the standard GB / T 16783.1-2014 Field test of drilling fluids in the petroleum and natural gas industry Part 1: Drilling fluid density, viscosity and shear force, and filtration loss in water-based drilling fluids. The test results are shown in Table 3.

[0154] 4. Blockage rate test

[0155] The plugging rate evaluation adopts a low permeability sand disk plugging instrument, and the test conditions are 120℃, 3.5MPa pressure difference, and 30min. Take the drilling fluid prepared in Examples 6-9 and Comparative Examples 6-11, take it out after hot rolling aging at 105℃ / 16h, and place it in the plugging instrument kettle. The plugging rate calculation method is to test the original permeability P0 of the simulated core, and the permeability of the core after the plugging agent solution acts is P1, then the plugging rate R0=(P0-P1) / P0×100%, and the experimental results are shown in Table 3.

[0156] Table 3 Evaluation results of conventional properties and plugging performance of drilling fluid

[0157]

[0158] From the results in Table 3, it can be seen that the rheological properties of the drilling fluids in Examples 6-9 change little, the atmospheric filtration loss is ≤4.0mL, and the plugging rate is >92%. The prepared drilling fluids have good plugging and filtration loss reduction properties. The atmospheric filtration loss of Example 8 is as low as 2.4mL, and the plugging rate is as high as 96.8%, which has the best effect. After changing the well wall strengthening agent composition and removing the cationic emulsified asphalt, the filtration loss of Comparative Examples 6-11 increased significantly, and the plugging rate was greatly reduced. Among them, the plugging rate of the drilling fluid of Comparative Example 8, which does not contain cationic modified nano plugging agent, ceramic powder and chopped fiber, decreased the most, indicating that the well wall strengthening agent composition and anti-collapse agent composition of the present application have a significant effect on the plugging performance of the drilling fluid, and can effectively improve the water loss and wall-building properties of the drilling fluid. The comparative experimental results show that the drilling fluid prepared by this method has better anti-collapse and plugging capabilities for coal rock cleats and micro-cracks.

Claims

1. A well wall strengthening agent composition, characterized in that: The method is composed of the following components in parts by weight: 1-3 parts of cationic modified nano plugging agent, 1-3 parts of nano emulsion, 2-6 parts of ceramic powder, and 1-3 parts of chopped fibers; The cationic modified nano plugging agent is composed of the following components in parts by weight: 20-30 parts of nano silicon dioxide, 20-30 parts of silane coupling agent, 8-12 parts of substituent, 10-15 parts of catalyst A, 5-10 parts of initiator, 30-40 parts of ionic liquid, 1-3 parts of catalyst B, and 15-20 parts of non-ionic monomer; The catalyst A is triethylamine; the catalyst B is C-94; The ionic liquid is one or two of N-ethylpyridinium hexafluorophosphate, 1-butyl-3-methylimidazolium bromide, 1-octyl-3-methylimidazolium trifluoromethanesulfonate, and 1-butyl-3-methylimidazolium methyl sulfate; The ceramic powder is a ceramic powder with a particle size of 2.0-6.8 μm and a core-shell structure, obtained by subjecting ceramic powder to nitridation treatment at 800-1200° C.; the chopped fibers are polyester fibers, mineral fibers or cotton fibers with a length of 0.1-0.5 mm; The substituent is 2-bromoisobutyryl; The nonionic monomer is styrene; The nanoemulsion is prepared by mixing solid paraffin, white oil, emulsifier and water in a weight ratio of 2:2:1:5; the emulsifier is composed of Tween 80 and Span 80 in a weight ratio of 56:

44.

2. The well wall strengthening agent composition according to claim 1, characterized in that: The invention is composed of the following components in parts by weight: 1 part of cationic modified nano plugging agent, 1 part of nanoemulsion, 2 parts of ceramic powder and 1 part of chopped fiber; wherein the cationic modified nano plugging agent is composed of the following components in parts by weight: 23 parts of nano silicon dioxide, 25 parts of silane coupling agent, 12 parts of substituent, 10 parts of catalyst A, 7 parts of initiator, 40 parts of ionic liquid, 3 parts of catalyst B and 20 parts of non-ionic monomer; wherein the ionic liquid is 1-butyl-3-methylimidazolium bromide and 1-octyl-3-methylimidazolium trifluoromethane sulfonate, and the weight ratio thereof is 4:

6.

3. The well wall strengthening agent composition according to claim 1 or 2, characterized in that: The preparation method of the cationic modified nano plugging agent is: (1) Dispersing nano-silicon dioxide to obtain a uniform suspension; (2) adding a silane coupling agent dropwise into the uniform suspension to obtain amino-modified nano-silica particles; (3) adding the amino-modified nano-silica particles into toluene for dispersion, adding a substituent and a catalyst A for condensation reaction and purification, thereby obtaining purified modified nano-silica particles; (4) The purified and modified nano-silica particles and the initiator are dissolved in deionized water to prepare a solution with a mass concentration of 30%. After deoxygenation, non-ionic monomers are added under nitrogen protection to cause free radical polymerization. Ionic liquid and catalyst B are then added in sequence to prepare a cationic modified nano-plugging agent after a condensation reaction.

4. The method for preparing the well wall strengthening agent composition according to claim 1 or 2, characterized in that: The cationic modified nano plugging agent, nanoemulsion, ceramic powder and chopped fibers are mixed and stirred at a stirring speed of 2000 rpm for 2 hours to obtain a well wall strengthening agent composition.

5. A water-based drilling fluid, characterized in that: The water-based drilling fluid comprises the following components in parts by weight: 80-100 parts of prehydrated bentonite slurry, 7-12 parts of potassium salt inhibitor, 2-5 parts of fluid loss reducer, 2-5 parts of anti-collapse agent composition, 5-10 parts of well wall strengthener composition, 2-3 parts of lubricant, and 10-50 parts of weighting agent; the well wall strengthener composition is the well wall strengthener composition according to claim 1 or 2.

6. The water-based drilling fluid according to claim 5, characterized in that: The prehydrated bentonite slurry is prepared by adding 3 parts of bentonite and 0.2 parts of Na2CO3 to 100 parts of water and standing for 24 hours; The potassium salt inhibitor is KCl or KCOOH; The fluid loss reducer is polyanionic cellulose, carboxymethyl starch or hydroxyethyl starch; The anti-collapse agent composition is obtained by uniformly mixing cationic emulsified asphalt and a film-forming agent in a weight ratio of 1:1; The lubricant is an extreme pressure lubricant; The weighting agent is limestone powder with a particle size of 38 μm.

7. The water-based drilling fluid according to claim 6, characterized in that: The preparation method of the cationic emulsified asphalt is as follows: 1) heating and melting 100 parts of base asphalt, adding 5 parts of nano-SiO2-lignin composite to perform ultrasonic dispersion; 2) mixing 1.5 parts of stabilizer calcium chloride and 100 parts of water, adding 5 parts of cationic emulsifier octadecyltrimethylammonium chloride at 70° C., mixing evenly, and adjusting the pH to 3; 3) simultaneously passing the obtained products of step 1) and step 2) through a colloid mill for emulsification to obtain cationic emulsified asphalt; The preparation method of the film-forming agent is as follows: 25 parts of polycaprolactone are added into a reaction kettle, vacuum dehydrated at 120° C. for 2 hours, 25 parts of isophorone diisocyanate are added after the temperature is reduced to 80° C., reacted for 3 hours, cooled to 70° C., 8 parts of dimethylolpropionic acid are added, reacted for 2 hours, cooled to 60° C., reacted for 1.5 hours, cooled to 40° C., 25 parts of methyl methacrylate and 15 parts of 2-acrylamido-2-methylpropanesulfonic acid are added, stirred for 0.5 hours, 30 parts of deionized water are added for high-speed emulsification and dispersion, 4 parts of initiator potassium persulfate are added, free radical polymerization is carried out at 80° C. for 3.5 hours, and the material is cooled and discharged to obtain the film-forming agent.

8. The method for preparing water-based drilling fluid according to claim 5, characterized in that: The following steps are involved: Add a fluid loss reducer, a potassium salt inhibitor, an anti-collapse agent composition, a well wall strengthening agent composition and a lubricant to the prehydrated bentonite slurry in sequence, mix them evenly, adjust the pH value to 8-9, add a weighting agent, and mix them evenly to obtain a water-based drilling fluid.

Citation Information

Cited By

  • Segmented copolymer well wall reinforcer rich in positive charge anchor points as well as preparation method and application of segmented copolymer well wall reinforcer

    CN121248944A