A low on-resistance trench gate silicon carbide VDMOS and a preparation method thereof
By constructing the second P-type well region and the second N-type source region in silicon carbide VDMOS, and using the combination technology of Schottky contact and P-type shielding layer, the high on-resistance of silicon carbide power devices under high voltage resistance is solved. The problem is that lower on-resistance and faster reverse recovery speed are achieved.
Patent Information
- Application Number
- CN202411131885.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-19
AI Technical Summary
Existing silicon carbide power devices have high on-resistance under high voltage conditions, making it difficult to achieve the requirement of low on-resistance.
The second P-type well region and the second N-type source region are constructed in the silicon carbide VDMOS, and Schottky contact is formed through direct contact between the source metal layer and the N-type drift layer, reducing the body diode voltage drop of the device and improving the reverse Towards the recovery speed, while constructing a P-type shielding layer at the bottom of the gate dielectric layer to suppress the problem of electric field concentration at the gate corners.
It effectively reduces the on-resistance of the device, improves the reverse recovery speed and switching speed of the device, and enhances the reliability and voltage resistance of the device.
Smart Images

Figure CN118658883B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a low on-resistance trench gate silicon carbide VDMOS and a preparation method thereof. Background Art
[0002] Silicon carbide MOSFET is a typical representative of silicon carbide power devices, which is widely used in electric vehicles, aerospace, power conversion and other fields. The device has achieved good characteristics within 1200V, and has replaced silicon MOSFET and IGBT within 1200V. With the improvement of device withstand voltage and the reduction of on-resistance, achieving high reliability and low on-resistance under high withstand voltage conditions has become a new requirement for the development of device technology; it is urgent to provide a silicon carbide power device with low on-resistance. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a low on-resistance trench gate silicon carbide VDMOS and a preparation method thereof, wherein a second P-type well region and a second N-type source region are constructed on the basis of ensuring the voltage resistance of the device and the low on-resistance of the trench gate, thereby further reducing the on-resistance of the device.
[0004] In a first aspect, the present invention provides a method for preparing a low on-resistance trench gate silicon carbide VDMOS, comprising the following steps:
[0005] Step 1: depositing metal on the lower side of the silicon carbide substrate to form a drain metal layer; epitaxially growing on the side of the silicon carbide substrate to form a drift layer;
[0006] Step 2, forming a barrier layer on the upper part of the drift layer, etching the barrier layer to form a through hole, performing ion implantation on the drift layer, and forming a shielding layer in the drift layer;
[0007] Step 3, removing the barrier layer, re-forming the barrier layer, etching the barrier layer to form a through hole, and performing ion implantation on the drift layer to form a second P-type well region in the drift layer;
[0008] Step 4, removing the barrier layer, re-forming the barrier layer, etching the barrier layer to form a through hole, performing ion implantation on the drift layer, and forming a second N-type source region in the second P-type well region;
[0009] Step 5, removing the barrier layer, re-forming the barrier layer, etching the barrier layer to form a through hole, and performing ion implantation on the drift layer to form a first P-type well region in the drift layer;
[0010] Step 6: removing the barrier layer, re-forming the barrier layer, etching the barrier layer to form a through hole, and performing ion implantation on the drift layer to form a first N-type source region in the drift layer;
[0011] Step 7, removing the barrier layer, re-forming the barrier layer, etching the barrier layer to form a through hole, then etching the drift layer and the first P-type well region until the upper side of the shielding layer to form a groove, and performing dry oxygen oxidation on the groove to form a gate dielectric layer, wherein the gate dielectric layer is provided with a groove;
[0012] Step 8, removing the barrier layer, re-forming the barrier layer, etching the barrier layer to form a through hole, depositing metal, and forming a gate metal layer;
[0013] Step 9, removing the barrier layer, re-forming the barrier layer, etching the barrier layer to form a through hole, etching the drift layer, depositing metal, and forming a first source metal region;
[0014] Step 10, remove the barrier layer, reform the barrier layer, etch the barrier layer to form a through hole, etch the drift layer, deposit metal, form a second source metal region, the source metal layer includes the first source metal region and the second source metal region, remove the barrier layer, and complete the preparation.
[0015] In a second aspect, the present invention provides a low on-resistance trench gate silicon carbide VDMOS, wherein the silicon carbide VDMOS is prepared by the method for preparing a low on-resistance trench gate silicon carbide VDMOS according to the first aspect.
[0016] The advantages of the present invention are:
[0017] 1. Based on the trench gate VDMOS device structure, a second N-type source region and a second P-type well region structure are constructed to provide a large number of electrons in the drift region, thereby reducing the device on-resistance;
[0018] Second, direct contact between the source metal layer and the N-type drift layer is constructed on the left and right sides of the device, thereby forming a Schottky contact and constructing a parasitic Schottky diode, which can reduce the body diode voltage drop of the device and improve the reverse recovery speed of the device;
[0019] 3. The gate metal layer of the device is 170nm deeper than the first P-type well region, so that the second P-type well region and the second N-type source region structure are controlled by the gate;
[0020] Fourth, a P-type shielding layer is constructed at the bottom of the device gate dielectric layer, which can effectively suppress the gate reliability problem caused by electric field concentration at the gate corner, while shielding the gate-drain capacitance and improving the device switching speed. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The present invention will be further described below in conjunction with embodiments with reference to the accompanying drawings.
[0022] Figure 1 The present invention is a flow chart of a method for preparing a low on-resistance trench gate silicon carbide VDMOS.
[0023] Figure 2 A cross-sectional view of the process of manufacturing a low on-resistance trench gate silicon carbide VDMOS according to the present invention Figure 1 .
[0024] Figure 3 A cross-sectional view of the process of manufacturing a low on-resistance trench gate silicon carbide VDMOS according to the present invention Figure 2 .
[0025] Figure 4 A cross-sectional view of the process of manufacturing a low on-resistance trench gate silicon carbide VDMOS according to the present invention Figure 3 .
[0026] Figure 5 A cross-sectional view of the process of manufacturing a low on-resistance trench gate silicon carbide VDMOS according to the present invention Figure 4 .
[0027] Figure 6 A cross-sectional view of the process of manufacturing a low on-resistance trench gate silicon carbide VDMOS according to the present invention Figure 5 .
[0028] Figure 7 A cross-sectional view of the process of manufacturing a low on-resistance trench gate silicon carbide VDMOS according to the present invention Figure 6 .
[0029] Figure 8 A cross-sectional view of the process of manufacturing a low on-resistance trench gate silicon carbide VDMOS according to the present invention Figure 7 .
[0030] Fig. 9 A cross-sectional view of the process of manufacturing a low on-resistance trench gate silicon carbide VDMOS according to the present invention Figure 8 .
[0031] Fig.10 A cross-sectional view of the process of manufacturing a low on-resistance trench gate silicon carbide VDMOS according to the present invention Figure 9 .
[0032] Fig.11 A cross-sectional view of the process of manufacturing a low on-resistance trench gate silicon carbide VDMOS according to the present invention Figure 10 .
[0033] Fig.12 A cross-sectional view of the process of manufacturing a low on-resistance trench gate silicon carbide VDMOS according to the present invention Figure 10 one.
[0034] Fig.13 A cross-sectional view of the process of manufacturing a low on-resistance trench gate silicon carbide VDMOS according to the present invention Figure 10 two.
[0035] Fig.14 A cross-sectional view of the process of manufacturing a low on-resistance trench gate silicon carbide VDMOS according to the present invention Figure 10 three.
[0036] Fig.15 The schematic diagram of a low on-resistance trench gate silicon carbide VDMOS of the present invention is shown. DETAILED DESCRIPTION
[0037] In order to facilitate understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. Embodiments of the present application are provided in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thorough and comprehensive.
[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0039] It should be understood that when an element or layer is referred to as "on ...", "adjacent to ...", "connected to" or "coupled to" other elements or layers, it can be directly on, adjacent to, connected to or coupled to other elements or layers, or there can be intervening elements or layers. On the contrary, when an element is referred to as "directly on ...", "in contact with ...", "directly connected to" or "directly coupled to" other elements or layers, there is no intervening element or layer. It should be understood that although the terms first, second, third, etc. can be used to describe various elements, components, regions, layers, doping types and / or parts, these elements, components, regions, layers, doping types and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer, doping type or part from another element, component, region, layer, doping type or part. Therefore, without departing from the teachings of the present invention, the first element, component, region, layer, doping type or part discussed below can be represented as a second element, component, region, layer or part.
[0040] Spatially relative terms such as "under," "beneath," "below," "under," "above," "above," and the like may be used herein to describe the relationship of one element or feature described in the figures to other elements or features. It should be understood that, in addition to the orientations described in the figures, spatially relative terms also include different orientations of the device in use and operation. For example, if the device in the accompanying drawings is flipped, an element or feature described as "under other elements" or "under it" or "under it" will be oriented as being "above" the other elements or features. Thus, the exemplary terms "under" and "under" may include both upper and lower orientations. In addition, the device may also include additional orientations (e.g., rotated 90 degrees or other orientations), and the spatial descriptors used herein are interpreted accordingly.
[0041] When used herein, the singular forms "a", "an", and "said / the" may also include plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "include / comprise" or "have" and the like specify the presence of stated features, wholes, steps, operations, components, parts, or combinations thereof, but do not exclude the possibility of the presence or addition of one or more other features, wholes, steps, operations, components, parts, or combinations thereof. At the same time, in this specification, the term "and / or" includes any and all combinations of the relevant listed items.
[0042] like Figures 1 to 14 As shown, the embodiment of the present application provides a method for preparing a low on-resistance trench gate silicon carbide VDMOS, comprising the following steps:
[0043] Step 1: depositing metal on the lower side of the silicon carbide substrate 1 to form a drain metal layer 8; epitaxially growing on the side of the silicon carbide substrate 1 to form a drift layer 2;
[0044] Step 2, forming a barrier layer a on the upper part of the drift layer 2, etching the barrier layer a to form a through hole, performing ion implantation on the drift layer 2, forming a shielding layer 23 in the drift layer 2, the ion implantation energy is 370-440kev, 1100nm-1300nm;
[0045] Step 3, removing the barrier layer a, re-forming the barrier layer a, etching the barrier layer a to form a through hole, performing ion implantation on the drift layer 2, forming a second P-type well region 21 in the drift layer 2, and the ion implantation energy is 300-400kev;
[0046] Step 4, removing the barrier layer a, re-forming the barrier layer a, etching the barrier layer a to form a through hole, performing ion implantation on the drift layer 2, forming a second N-type source region 211 in the second P-type well region 21, and the ion implantation energy is 300-370kev;
[0047] Step 5, removing the barrier layer a, re-forming the barrier layer a, etching the barrier layer a to form a through hole, and performing ion implantation on the drift layer 2 to form a first P-type well region 3 in the drift layer 2, wherein the ion implantation energy is 200-300kev;
[0048] Step 6, removing the barrier layer a, re-forming the barrier layer a, etching the barrier layer a to form a through hole, performing ion implantation on the drift layer 2, forming a first N-type source region 4 in the drift layer 2, and the ion implantation energy is 100-200kev;
[0049] Step 7, removing the barrier layer a, re-forming the barrier layer a, etching the barrier layer a to form a through hole, then etching the drift layer 2 and the first P-type well region 3 until the upper side of the shielding layer 23 to form a groove 22, and performing dry oxygen oxidation on the groove 22 to form a gate dielectric layer 5, wherein the gate dielectric layer 5 is provided with a groove 51;
[0050] Step 8, removing the barrier layer a, re-forming the barrier layer a, etching the barrier layer a to form a through hole, depositing metal, and forming a gate metal layer 7;
[0051] Step 9, removing the barrier layer a, re-forming the barrier layer a, etching the barrier layer a to form a through hole, etching the drift layer 2 to a depth of 900 nm, depositing metal to form a first source metal region 61;
[0052] Step 10, remove the barrier layer a, reform the barrier layer a, etch the barrier layer a to form a through hole, etch the drift layer 2, the etching depth is 300nm, deposit metal to form a second source metal region 62, the source metal layer 6 includes a first source metal region 61 and a second source metal region 62, remove the barrier layer a, and complete the preparation.
[0053] The depth of the groove 22 is 200 nm; the distance L1 from the inner wall of the second N-type source region 211 to the inner wall of the second P-type well region 21 is 10 nm; the distance L2 from the outer wall of the second N-type source region 211 to the outer wall of the second P-type well region 21 is 60 nm.
[0054] The silicon carbide substrate 1 and the drift layer 2 are both N-type, and the shielding layer 23 is P-type; the doping concentration of the silicon carbide substrate 1 is 5e18cm -3 The doping concentration of the drift layer 2 is 2e17cm -3 The doping concentration of the shielding layer 23 is 1e18 cm -3 The doping concentration of the second P-type well region 21 is 5e17 cm -3 The doping concentration of the second N-type source region 211 is 8e18cm -3 The doping concentration of the first P-type well region 21 is 5e17 cm -3The doping concentration of the first N-type source region 211 is 8e18cm -3 The gate metal layer 7 is an alloy of Ni and Al in a ratio of 2:8; the source metal layer 6 is an alloy of Ni and Al in a ratio of 2:8.
[0055] The thickness of the N-type silicon carbide substrate 1 of the device is 1 μm, the thickness of the N-type drift layer 2 is 20-30 μm, the thickness of the P-type shield gate 23 is 200 nm, the thickness of the second P-type well region 21 is 300 nm, the thickness of the second N-type source region 211 is 200 nm, the distance L1 between the farthest end of the second P-type well region 21 close to the gate and the farthest end of the second N-type source region 211 close to the gate is 10 nm, and the distance L2 on the other side is 60 nm, and the bottom of the gate dielectric layer 5 is 200 nm. The thickness is 30nm, the side wall thickness is 20nm, the thickness of the first P-type well region 3 is 300nm, the thickness of the first N-type source region 4 is 300nm, the thickness from the top of the source metal layer 6 to the N-type drift layer 2 and the second P-type well region 21, the thickness of the second N-type source region 211 is 900nm, the thickness from the top of the source metal layer 6 to the top of the first N-type source region 4 is 300nm, the thickness of the gate metal layer 7 is 1100nm, and the device withstand voltage is 1200-3000V;
[0056] The concentration of the N-type silicon carbide substrate 1 is to form a low-resistance ohmic contact with the drain metal layer 8 to reduce the on-resistance of the device. Its thickness is to ensure support when doing device epitaxy and improve process stability. The thickness and doping concentration of the P-type shielding layer 23 are a compromise based on the realization of the gate protection capability. The best effect is that the lower the doping concentration, the better, and the thinner the thickness, the better. Because the protection capability is to be achieved, the two relationships affect each other and the compromise is taken; the thickness and doping capability of the second P-type well region 21 are related to the depth of the gate metal layer 7, which improves the gate's control capability over the second P-type well region 21 and the second N-type source region 211. The second P-type well region 21 and the second N-type source region 211 are horizontally connected. The relationship between the width and the gate width is that under this structural condition, the gate has weak control over the second P-type well region 21 and the second N-type source region 211, and the thin second P-type well region 211 close to the gate side can improve the gate control ability. The doping concentration and thickness of the first P-type well region 3 are designed to ensure the device's gate control ability over the first P-type well region 3. The doping concentration of the N-type drift layer 2 is a compromise between the device's withstand voltage and on-resistance. The first N-type source region 4 is to achieve ohmic contact with the source metal layer 6; the second P-type well region 21 and the second N-type source region 211 are under the control of the gate metal layer 7. When the device is turned on, they can provide a large number of electrons to the drift layer, thereby reducing the on-resistance of the device.
[0057] The device constructs direct contact between the source metal layer 6 and the N-type drift layer 2, thereby forming a Schottky contact and constructing a parasitic Schottky diode, which can reduce the body diode voltage drop of the device and improve the reverse recovery speed of the device.
[0058] like Fig.15 As shown, the silicon carbide VDMOS obtained by the above manufacturing method includes: a silicon carbide substrate 1, a drift layer 2, the lower side of the drift layer 2 is connected to the upper side of the silicon carbide substrate 1; a second P-type well region 21 is provided in the drift layer 2, a second N-type source region 211 is provided in the second P-type well region 21, a groove 22 is provided on the drift layer 2, a shielding layer 23 is provided in the drift layer 2, and the shielding layer 23 is located at the bottom of the groove 22;
[0059] A first P-type well region 3, wherein the lower side of the first P-type well region 3 is connected to the drift layer 2, the second P-type well region 21 and the second N-type source region 211;
[0060] A first N-type source region 4, wherein the lower side of the first N-type source region 4 is connected to the upper side of the first P-type well region 3;
[0061] A gate dielectric layer 5, wherein the lower portion of the gate dielectric layer 5 is disposed in the groove 22, the outer sidewalls of the gate dielectric layer 5 are respectively connected to the first N-type source region 4, the first P-type well region 3 and the drift layer 2, and a trench 51 is disposed in the gate dielectric layer 5;
[0062] A source metal layer 6, wherein the source metal layer 6 is respectively connected to the first N-type source region 4, the first P-type well region 3, the drift layer 2, the second P-type well region 21 and the second N-type source region 211;
[0063] A gate metal layer 7, wherein the gate metal layer 7 is disposed in the groove 51;
[0064] and a drain metal layer 8 , wherein the drain metal layer 8 is connected to the lower side of the silicon carbide substrate 1 .
[0065] Although the specific implementation modes of the present invention are described above, those skilled in the art should understand that the specific implementation modes described are only illustrative and are not intended to limit the scope of the present invention. Equivalent modifications and changes made by those skilled in the art in accordance with the spirit of the present invention should be included in the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a low on-resistance trench gate silicon carbide VDMOS, characterized in that: The steps include: Step 1: depositing metal on the lower side of the silicon carbide substrate to form a drain metal layer; epitaxially growing on the side of the silicon carbide substrate to form a drift layer; Step 2: forming a barrier layer on the upper part of the drift layer, etching the barrier layer to form a through hole, performing ion implantation on the drift layer, and forming a shielding layer in the drift layer; Step 3, removing the barrier layer, re-forming the barrier layer, etching the barrier layer to form a through hole, and performing ion implantation on the drift layer to form a second P-type well region in the drift layer; Step 4, removing the barrier layer, re-forming the barrier layer, etching the barrier layer to form a through hole, performing ion implantation on the drift layer, and forming a second N-type source region in the second P-type well region; Step 5, removing the barrier layer, re-forming the barrier layer, etching the barrier layer to form a through hole, and performing ion implantation on the drift layer to form a first P-type well region in the drift layer; Step 6: removing the barrier layer, re-forming the barrier layer, etching the barrier layer to form a through hole, and performing ion implantation on the drift layer to form a first N-type source region in the drift layer; Step 7, removing the barrier layer, re-forming the barrier layer, etching the barrier layer to form a through hole, then etching the drift layer and the first P-type well region until the upper side of the shielding layer to form a groove, and performing dry oxygen oxidation on the groove to form a gate dielectric layer, wherein the gate dielectric layer is provided with a groove; Step 8, removing the barrier layer, re-forming the barrier layer, etching the barrier layer to form a through hole, depositing metal, and forming a gate metal layer; Step 9, removing the barrier layer, re-forming the barrier layer, etching the barrier layer to form a through hole, etching the drift layer, depositing metal, and forming a first source metal region; Step 10, removing the barrier layer, re-forming the barrier layer, etching the barrier layer to form a through hole, etching the drift layer, depositing metal, forming a second source metal region, the source metal layer includes the first source metal region and the second source metal region, removing the barrier layer, and completing the preparation; The second P-type well region is arranged in the drift layer, the second N-type source region is arranged in the second P-type well region, the lower side of the first P-type well region is connected to the drift layer, the second P-type well region and the second N-type source region; the source metal layer is respectively connected to the first N-type source region, the first P-type well region, the drift layer, the second P-type well region and the second N-type source region.
2. The method for preparing a low on-resistance trench gate silicon carbide VDMOS according to claim 1, characterized in that: The bottom thickness of the gate dielectric layer is 30 nm, and the side wall thickness is 20 nm.
3. The method for preparing a low on-resistance trench gate silicon carbide VDMOS according to claim 1, characterized in that: The depth of the groove is 200 nm.
4. The method for preparing a low on-resistance trench gate silicon carbide VDMOS according to claim 1, characterized in that: The thickness of the shielding layer is 200 nm.
5. The method for preparing a low on-resistance trench gate silicon carbide VDMOS according to claim 1, characterized in that: The distance from the inner sidewall of the second N-type source region to the inner sidewall of the second P-type well region is 10 nm; the distance from the outer sidewall of the second N-type source region to the outer sidewall of the second P-type well region is 60 nm.
6. The method for preparing a low on-resistance trench gate silicon carbide VDMOS according to claim 1, characterized in that: The doping concentration of the silicon carbide substrate is 5e18cm -3 The doping concentration of the drift layer is 2e17cm -3 The doping concentration of the shielding layer is 1e18 cm -3 The doping concentration of the second P-type well region is 5e17 cm -3 , the doping concentration of the second N-type source region is 8e18cm -3 The doping concentration of the first P-type well region is 5e17 cm -3 , the doping concentration of the first N-type source region is 8e18cm -3 .
7. The method for preparing a low on-resistance trench gate silicon carbide VDMOS according to claim 1, characterized in that: The gate metal layer is an alloy of Ni and Al in a ratio of 2:8; the source metal layer is an alloy of Ni and Al in a ratio of 2:8.