A high discharge capacity lithium nickel manganese oxide positive electrode material and preparation method thereof
By adding aluminum and ruthenium doping to the positive electrode material of lithium-ion battery and coating it with polypyrrole, combined with carbon-coated aluminum foil and composite adhesive, the transition metal dissolution and electrolyte corrosion problems of spinel nickel manganate are solved. , improves the discharge specific capacity and cycle stability of lithium-ion batteries.
Patent Information
- Application Number
- CN202411135070.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-19
AI Technical Summary
The existing lithium-ion battery positive electrode material spinel type lithium nickel manganese oxide has limited its application in lithium-ion batteries due to problems such as transition metal dissolution, ginger Taylor effect and electrolyte corrosion.
Ni-manganese carbonate precursor is prepared by co-precipitating manganese sulfate, nickel sulfate and precipitant solution, followed by step calcination and annealing under an oxygen atmosphere, doping aluminum and ruthenium, and finally coated with polypyrrole and combined coating. Carbon aluminum foil and composite adhesive are assembled to produce a high discharge specific capacity nickel-manganate lithium coelite.
It improves the specific surface area, conductivity and structural stability of the material, reduces the interface impedance and lithium ion diffusion path, enhances the room temperature cycle stability and rate performance, and reduces the decline in battery performance.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion battery materials, and in particular to a high discharge specific capacity lithium nickel manganese oxide positive electrode material and a preparation method thereof. Background Art
[0002] With the development of society, clean energy such as solar energy, wind energy and tidal energy have been widely developed and utilized. However, their intermittent and uncertain characteristics hinder their promotion and application. Therefore, people hope to promote the use of clean energy by developing new energy storage devices. Lithium-ion batteries are a new type of green and environmentally friendly batteries developed at the end of the 20th century. Because of their high energy density, long service life, no memory effect and no heavy metals such as cadmium and lead, they have quickly occupied the application fields of mobile phones, laptops, small cameras, digital cameras, power tools, electric vehicles, etc.
[0003] But at the same time, the capacity of lithium-ion batteries can no longer meet the development needs. An effective way to increase the energy density of batteries is to increase the working voltage and specific capacity of the positive electrode material. Spinel nickel manganese oxide has a high working voltage of 4.7V and a discharge specific capacity of 146.7mAh / g, and an energy density of 650Wh / kg. In addition, its low cost, high safety, and environmental friendliness make it one of the most promising positive electrode materials. However, spinel nickel manganese oxide has its own shortcomings such as transition metal dissolution, Jan-Taylor effect, and corrosion of electrolyte, which limits it from becoming the mainstream positive electrode material for lithium-ion batteries. Summary of the invention
[0004] The object of the present invention is to provide a lithium nickel manganese oxide positive electrode material with high discharge specific capacity and a preparation method thereof, so as to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A high discharge capacity lithium nickel manganese oxide positive electrode material is prepared by first mixing manganese sulfate, nickel sulfate and a precipitant solution for co-precipitation to obtain a nickel manganese carbonate precursor; step-calcining lithium carbonate, a nickel manganese carbonate precursor, aluminum hydroxide and ruthenium oxide in an oxygen atmosphere and then annealing to obtain aluminum / ruthenium doped lithium nickel manganese oxide; coating aluminum / ruthenium doped lithium nickel manganese oxide with polypyrrole to obtain lithium nickel manganese oxide with high discharge capacity; and assembling lithium nickel manganese oxide with high discharge capacity, carbon-coated aluminum foil, a composite binder and a conductive agent to obtain the high discharge capacity lithium nickel manganese oxide positive electrode material.
[0007] As an optimization, the precipitant solution is prepared by uniformly mixing sodium carbonate, ammonia monohydrate and pure water in a mass ratio of 1:12:60, and stirring at room temperature at 150-250 r / min until dissolved.
[0008] As an optimization, the carbon-coated aluminum foil was purchased from Guangzhou Nano New Materials Technology Co., Ltd.
[0009] As an optimization, the composite binder is prepared by uniformly mixing guar gum, O-carboxymethyl chitosan and pure water in a mass ratio of 1:4:30, stirring at 70-80°C and 200-300 r / min until dissolved, and naturally cooling to room temperature.
[0010] As an optimization, the guar gum was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.
[0011] As an optimization, the O-carboxymethyl chitosan was purchased from Shanghai Dibai Chemical Technology Co., Ltd., with a substitution degree of 60% to 70% and a deacetylation degree of greater than 85%.
[0012] As an optimization, the conductive agent is acetylene black with a median diameter of 1~3μm.
[0013] A method for preparing a lithium nickel manganese oxide positive electrode material with high discharge specific capacity comprises the following preparation steps:
[0014] (1) Manganese sulfate and nickel sulfate were added to pure water at a molar ratio of 3:1 to prepare a 2 mol / L solution, and the solution was input into a liquid phase stirred reactor using a peristaltic pump under a nitrogen atmosphere. The precipitant solution was then input into the liquid phase stirred reactor using a peristaltic pump at a volume ratio of 1:1.2. The precipitant solution was added at 50-55°C and 50-60 r / min. The speed of adding the precipitant solution was controlled to maintain the pH at 8.1. After the precipitant solution was completely added, the solution was reacted for 18-20 hours, filtered, and vacuum dried at 80-90°C for 8-10 hours to obtain a nickel manganese carbonate precursor.
[0015] (2) lithium carbonate, nickel manganese carbonate precursor, aluminum hydroxide, and ruthenium oxide are fully mixed in a mass ratio of 1:(5.73-5.75):(0.09-0.11):(0.1-0.11), poured into a mortar and ground for 1-1.5 hours, and step-calcined in an oxygen atmosphere to obtain aluminum / ruthenium-doped lithium nickel manganese oxide;
[0016] (3) Aluminum / ruthenium doped lithium nickel manganese oxide, pyrrole, sodium dodecylbenzene sulfonate and pure water are mixed evenly according to the formula, ultrasonically dispersed for 10-12 minutes, and a 20 g / L ferric chloride solution equal to the mass of pure water is added dropwise in an ice water bath at 100-150 r / min, 5-6 drops per second. After the addition is completed, the reaction is carried out for 12-15 hours, filtered, washed with pure water 3-5 times, and vacuum dried at 60-70°C for 10-12 hours to obtain lithium nickel manganese oxide with high discharge specific capacity;
[0017] (4) Pour high discharge capacity lithium nickel manganese oxide and a conductive agent into a mortar and grind them for 30 to 40 minutes respectively. Mix high discharge capacity lithium nickel manganese oxide, the conductive agent and the composite binder in a mass ratio of 8:1:1, pour them into a ball mill, stir them for 10 to 15 minutes using a high-speed swing ball mill, evenly spread them on a carbon-coated aluminum foil, and vacuum dry them at 60°C for 3 to 4 hours, and then vacuum dry them at 120°C for 10 to 12 hours to obtain a high discharge capacity lithium nickel manganese oxide positive electrode material.
[0018] As an optimization, the step calcination in step (2) is calcination at 180-200°C for 1-1.5 h, calcination at 350-370°C for 1.5-2 h, calcination at 550-570°C for 1-1.5 h, calcination at 900°C for 20 h, cooling to 700°C for annealing for 10-12 h, and the heating rate during the calcination process is 10°C / min.
[0019] As an optimization, the formula of step (3) is aluminum / ruthenium doped lithium nickel manganese oxide, pyrrole, sodium dodecylbenzene sulfonate, and pure water in a mass ratio of 1:(0.045~0.055):(0.0005~0.0006):(50~60).
[0020] The invention discloses an application of a high discharge specific capacity lithium nickel manganese oxide positive electrode material in a lithium ion battery.
[0021] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0022] When preparing a high-discharge-specific-capacity lithium nickel manganese oxide positive electrode material, the present invention comprises the following steps: firstly, manganese sulfate, nickel sulfate and a precipitant solution are mixed for co-precipitation to obtain a nickel manganese carbonate precursor; lithium carbonate, a nickel manganese carbonate precursor, aluminum hydroxide and ruthenium oxide are step-calcined in an oxygen atmosphere and then annealed to obtain aluminum / ruthenium-doped lithium nickel manganese oxide; aluminum / ruthenium-doped lithium nickel manganese oxide is coated with polypyrrole to obtain a high-discharge-specific-capacity lithium nickel manganese oxide; and lithium nickel manganese oxide with a high-discharge-specific-capacity, a carbon-coated aluminum foil, a composite binder and a conductive agent are assembled to obtain a high-discharge-specific-capacity lithium nickel manganese oxide positive electrode material.
[0023] First, manganese sulfate, nickel sulfate and a precipitant solution are mixed for co-precipitation to obtain a nickel-manganese carbonate precursor, and the nickel-manganese is co-precipitated with a carbonate precipitant. The precipitation rates of the two are similar, ensuring that the nickel and manganese in the formed precursor are evenly dispersed. At the same time, the carbonate precursor releases carbon dioxide gas due to the thermal decomposition of the carbonate during subsequent calcination, thereby forming a porous spherical morphology of lithium nickel manganese oxide. The porous spherical morphology increases the specific surface area, improves the contact with the conductive agent, reduces the interface impedance, and reduces the diffusion path of lithium ions and electrons. At the same time, it has a higher phase transition rate, showing better room temperature cycle stability and rate performance.
[0024] Secondly, lithium carbonate, nickel manganese carbonate precursor, aluminum hydroxide, and ruthenium oxide are step-calcined in an oxygen atmosphere and then annealed to obtain aluminum / ruthenium-doped nickel manganese oxide. During the conventional calcination process of nickel manganese oxide, Li x Ni 1-x O impurity phase is generated, which affects the electrochemical performance of lithium nickel manganese oxide as a positive electrode material, while ruthenium doping inhibits Li x Ni 1-x The formation of O impurity phase stabilizes the cubic spinel crystal structure. 4+ The addition of ions makes some Mn 4+ Reduction to Mn 3+ To balance the charge, Mn 3+ Ions can improve the conductivity of the material; aluminum doping can improve the structural stability of the material, inhibit and weaken the influence of the Jan-Taylor effect, and improve the discharge capacity and rate cycle performance at high rates. At the same time, the bond energy of Ru-O and Al-O bonds is higher than that of Mn-O bonds, and its stability is significantly stronger than that of undoped lithium nickel manganese oxide; high-temperature calcination in an oxygen atmosphere causes the material to generate a P4332 space group structure, and the high-temperature stability is improved. At the same time, the incorporation of aluminum and ruthenium ions increases the phase transition rate of the P4332 space group structure during the charge and discharge process, which is beneficial to the extraction and embedding of lithium ions; by mixing the nickel manganese carbonate precursor and lithium carbonate powder It can be seen from the TG-DSC thermal analysis curve that there are three obvious weight loss points during the calcination process, one at 80~200℃, one at 220~380℃, and one at 400~600℃. The weight loss at 80~200℃ is the removal of a small amount of free water, interlayer water and adsorbed water, 220~380℃ is the decomposition of nickel carbonate and manganese carbonate to generate manganese oxide and nickel oxide required for subsequent production, and the weight loss at 400~600℃ is the decomposition of lithium carbonate. In response to this situation, a step-by-step calcination system was developed, and the three weight loss temperatures were kept warm and calcined for a period of time to allow the reaction at each stage to fully occur and reduce the impact of incomplete reaction on the subsequent reactions.
[0025] Again, aluminum / ruthenium doped lithium nickel manganese oxide is coated with polypyrrole to obtain lithium nickel manganese oxide with high discharge specific capacity. The aluminum / ruthenium doped lithium nickel manganese oxide prepared above has a porous spherical structure and a larger specific surface area. While improving the contact efficiency and reducing the diffusion path of lithium ions and electrons, it also increases the effect of electrolyte corrosion. In order to reduce this effect, pyrrole is used for in-situ polymerization to coat the aluminum / ruthenium doped lithium nickel manganese oxide with a layer of polypyrrole for protection. The conductivity of polypyrrole itself provides a transmission channel for lithium ions. At the same time, polypyrrole can also protect the aluminum / ruthenium doped lithium nickel manganese oxide from corrosion by the electrolyte. At the same time, since it does not directly contact the electrolyte, the Mn 2+The dissolution of ions stabilizes the crystal structure. Although polypyrrole has conductivity, it is relatively low. Therefore, sodium dodecylbenzene sulfonate is doped in the polypyrrole polymerization process to improve its conductivity. At the same time, the effect of low emulsion diffusion can be achieved in the pyrrole aggregation process, which can prevent the agglomeration of polypyrrole and improve the uniformity of the surface coating thickness.
[0026] Finally, high discharge capacity lithium nickel manganese oxide, carbon-coated aluminum foil, composite binder, and conductive agent were assembled to obtain high discharge capacity lithium nickel manganese oxide positive electrode material. Since lithium nickel manganese oxide has a working voltage of up to 4.7V, the aluminum foil used as the current collector will inevitably be corroded under high voltage conditions, reducing the ion and electron transmission capacity, and the active material and the current collector will have contact failure, resulting in capacity decay, thereby reducing battery performance. Carbon coating on the surface of the aluminum foil can protect the aluminum foil from corrosion and reduce the battery performance degradation caused by current collector corrosion. The contact failure under high voltage may also be related to the fact that the polyvinylidene fluoride binder cannot exert normal viscosity under high voltage, and the viscosity between the polyvinylidene fluoride and the current collector interface is poor, and a layer of interface film with low lithium ion conductivity will be formed. In order to improve this situation, guar gum was selected. Used as a composite binder with O-carboxymethyl chitosan, guar gum is a water-soluble, non-toxic, abundant, renewable and environmentally friendly polysaccharide that can adapt to volume changes during charge and discharge by maintaining the structure and improving the mechanical strength of the electrode. Low-substituted O-carboxymethyl chitosan retains amino groups while introducing a large number of hydrophilic carboxymethyl groups. The amino groups on O-carboxymethyl chitosan can play a complexing role to fix the free nickel and manganese ions and reduce their loss in the electrolyte. At the same time, guar gum and O-carboxymethyl chitosan, as water-soluble binders, have a lower contact angle and good wettability, so that the electrolyte can better wet the electrode, improve the contact between the electrolyte and the active substance, and improve the lithium ion and electron transmission efficiency. At the same time, it avoids the use of toxic N-methylpyrrolidone and uses pure water, which is environmentally friendly. DETAILED DESCRIPTION
[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0028] The preparation process of the precipitant solution and the composite binder used in all subsequent examples and comparative examples is as follows:
[0029] A. Mix sodium carbonate, ammonia monohydrate and pure water in a mass ratio of 1:12:60, stir at room temperature at 200r / min until dissolved, and prepare a precipitant solution;
[0030] B. Mix guar gum, O-carboxymethyl chitosan and pure water in a mass ratio of 1:4:30, stir at 75°C and 250 r / min until dissolved, and cool naturally to room temperature to obtain a composite adhesive. Example 1
[0031] A method for preparing a lithium nickel manganese oxide positive electrode material with a high discharge specific capacity, the method for preparing a lithium nickel manganese oxide positive electrode material with a high discharge specific capacity comprising the following preparation steps:
[0032] (1) Manganese sulfate and nickel sulfate were added to pure water at a molar ratio of 3:1 to prepare a 2 mol / L solution, and the solution was input into a liquid-phase stirred reactor using a peristaltic pump under a nitrogen atmosphere. The precipitant solution was then input into the liquid-phase stirred reactor using a peristaltic pump at a volume ratio of 1:1.2. The precipitant solution was added at 50°C and 50 r / min, and the pH was maintained at 8.1. After the precipitant solution was completely added, the solution was reacted for 18 hours, filtered, and vacuum dried at 80°C for 10 hours to obtain a nickel manganese carbonate precursor;
[0033] (2) lithium carbonate, nickel manganese carbonate precursor, aluminum hydroxide, and ruthenium oxide were fully mixed in a mass ratio of 1:5.73:0.09:0.1, poured into a mortar and ground for 1 hour, calcined at 180°C for 1.5 hours, 350°C for 2 hours, 550°C for 1.5 hours, and 900°C for 20 hours in an oxygen atmosphere, cooled to 700°C and annealed for 12 hours. The heating rate during the calcination process was 10°C / min, and aluminum / ruthenium doped nickel manganese oxide was obtained;
[0034] (3) Aluminum / ruthenium doped lithium nickel manganese oxide, pyrrole, sodium dodecylbenzene sulfonate and pure water were mixed in a mass ratio of 1:0.045:0.0005:50, and ultrasonically dispersed for 10 minutes. A 20 g / L ferric chloride solution equal to the mass of pure water was added dropwise in an ice water bath at 100 r / min, 5 drops per second. After the addition was completed, the reaction was continued for 12 hours, filtered, washed with pure water 3 times, and vacuum dried at 60°C for 12 hours to obtain lithium nickel manganese oxide with high discharge specific capacity;
[0035] (4) Pour high discharge capacity lithium nickel manganese oxide and a conductive agent into a mortar and grind them for 30 minutes respectively. Mix high discharge capacity lithium nickel manganese oxide, the conductive agent and the composite binder in a mass ratio of 8:1:1, pour them into a ball mill, stir them for 10 minutes using a high-speed oscillating ball mill, evenly spread them on a carbon-coated aluminum foil, and vacuum dry them at 60°C for 3 hours, and then vacuum dry them at 120°C for 10 hours to obtain a high discharge capacity lithium nickel manganese oxide positive electrode material. Example 2
[0036] A method for preparing a lithium nickel manganese oxide positive electrode material with a high discharge specific capacity, the method for preparing a lithium nickel manganese oxide positive electrode material with a high discharge specific capacity comprising the following preparation steps:
[0037] (1) Manganese sulfate and nickel sulfate were added to pure water at a molar ratio of 3:1 to prepare a 2 mol / L solution, and the solution was input into a liquid-phase stirred reactor using a peristaltic pump under a nitrogen atmosphere. The precipitant solution was then input into the liquid-phase stirred reactor using a peristaltic pump at a volume ratio of 1:1.2. The precipitant solution was added at 55°C and 60 r / min, and the pH was maintained at 8.1. After the precipitant solution was completely added, the reaction was continued for 19 hours, filtered, and vacuum dried at 85°C for 9 hours to obtain a nickel manganese carbonate precursor;
[0038] (2) lithium carbonate, nickel manganese carbonate precursor, aluminum hydroxide, and ruthenium oxide were fully mixed in a mass ratio of 1:5.74:0.1:0.11, poured into a mortar and ground for 1.5 hours, calcined at 190°C for 1 hour, 360°C for 1.5 hours, 560°C for 1 hour, and 900°C for 20 hours in an oxygen atmosphere, cooled to 700°C and annealed for 11 hours. The heating rate during the calcination process was 10°C / min, and aluminum / ruthenium doped nickel manganese oxide was obtained;
[0039] (3) Aluminum / ruthenium doped lithium nickel manganese oxide, pyrrole, sodium dodecylbenzene sulfonate and pure water were mixed in a mass ratio of 1:0.05:0.0005:55, and ultrasonically dispersed for 11 minutes. A 20 g / L ferric chloride solution equal to the mass of pure water was added dropwise in an ice water bath at 150 r / min, 6 drops per second. After the addition was completed, the reaction was continued for 13 hours, filtered, washed with pure water 4 times, and vacuum dried at 65°C for 11 hours to obtain lithium nickel manganese oxide with high discharge specific capacity;
[0040] (4) Pour high discharge capacity lithium nickel manganese oxide and a conductive agent into a mortar and grind them for 35 minutes respectively. Mix high discharge capacity lithium nickel manganese oxide, the conductive agent and the composite binder in a mass ratio of 8:1:1, pour them into a ball mill, stir them for 12 minutes using a high-speed oscillating ball mill, evenly spread them on a carbon-coated aluminum foil, and vacuum dry them at 60°C for 3.5 hours, and then vacuum dry them at 120°C for 11 hours to obtain a high discharge capacity lithium nickel manganese oxide positive electrode material. Example 3
[0041] A method for preparing a lithium nickel manganese oxide positive electrode material with a high discharge specific capacity, the method for preparing a lithium nickel manganese oxide positive electrode material with a high discharge specific capacity comprising the following preparation steps:
[0042] (1) Manganese sulfate and nickel sulfate were added to pure water at a molar ratio of 3:1 to prepare a 2 mol / L solution, and the solution was input into a liquid-phase stirred reactor using a peristaltic pump under a nitrogen atmosphere. The precipitant solution was then input into the liquid-phase stirred reactor using a peristaltic pump at a volume ratio of 1:1.2. The precipitant solution was added at 55°C and 50 r / min, and the pH was maintained at 8.1. After the precipitant solution was completely added, the solution was reacted for 20 hours, filtered, and vacuum dried at 90°C for 8 hours to obtain a nickel manganese carbonate precursor;
[0043] (2) lithium carbonate, nickel manganese carbonate precursor, aluminum hydroxide, and ruthenium oxide were fully mixed in a mass ratio of 1:5.75:0.11:0.11, poured into a mortar and ground for 1.5 hours, calcined at 200°C for 1 hour, 370°C for 1.5 hours, 570°C for 1 hour, and 900°C for 20 hours in an oxygen atmosphere, cooled to 700°C for annealing for 10 hours, and the heating rate during the calcination process was 10°C / min to obtain aluminum / ruthenium doped nickel manganese oxide;
[0044] (3) Aluminum / ruthenium doped lithium nickel manganese oxide, pyrrole, sodium dodecylbenzene sulfonate and pure water were mixed in a mass ratio of 1:0.055:0.0006:60, and ultrasonically dispersed for 12 minutes. A 20 g / L ferric chloride solution equal to the mass of pure water was added dropwise in an ice water bath at 150 r / min, 6 drops per second. After the addition was completed, the reaction was continued for 15 hours, filtered, washed with pure water 5 times, and vacuum dried at 70°C for 10 hours to obtain lithium nickel manganese oxide with high discharge specific capacity;
[0045] (4) Pour high discharge capacity lithium nickel manganese oxide and a conductive agent into a mortar and grind them for 40 minutes respectively. Mix high discharge capacity lithium nickel manganese oxide, the conductive agent and the composite binder in a mass ratio of 8:1:1, pour them into a ball mill, stir them for 15 minutes using a high-speed oscillating ball mill, evenly spread them on a carbon-coated aluminum foil, and vacuum dry them at 60°C for 4 hours, and then vacuum dry them at 120°C for 12 hours to obtain a high discharge capacity lithium nickel manganese oxide positive electrode material.
[0046] Comparative Example 1
[0047] A method for preparing a lithium nickel manganese oxide positive electrode material with a high discharge specific capacity, the method for preparing a lithium nickel manganese oxide positive electrode material with a high discharge specific capacity comprising the following preparation steps:
[0048] (1) Manganese sulfate and nickel sulfate were added to pure water at a molar ratio of 3:1 to prepare a 2 mol / L solution, and the solution was input into a liquid-phase stirred reactor using a peristaltic pump under a nitrogen atmosphere. The precipitant solution was then input into the liquid-phase stirred reactor using a peristaltic pump at a volume ratio of 1:1.2. The precipitant solution was added at 55°C and 60 r / min, and the pH was maintained at 8.1. After the precipitant solution was completely added, the reaction was continued for 19 hours, filtered, and vacuum dried at 85°C for 9 hours to obtain a nickel manganese carbonate precursor;
[0049] (2) lithium carbonate and nickel manganese carbonate precursors were fully mixed at a mass ratio of 1:5.98, poured into a mortar and ground for 1.5 hours, calcined at 190°C for 1 hour, 360°C for 1.5 hours, 560°C for 1 hour, and 900°C for 20 hours under an oxygen atmosphere, cooled to 700°C and annealed for 11 hours. The heating rate during the calcination process was 10°C / min to obtain lithium nickel manganese oxide;
[0050] (3) Mix lithium nickel manganese oxide, pyrrole, sodium dodecylbenzene sulfonate and pure water in a mass ratio of 1:0.05:0.0005:55, and ultrasonically disperse for 11 minutes. Add 20g / L ferric chloride solution equal to the mass of pure water in an ice water bath at 150r / min, 6 drops per second. After the addition is completed, react for 13 hours, filter, wash with pure water 4 times, and vacuum dry at 65°C for 11 hours to obtain lithium nickel manganese oxide with high discharge specific capacity;
[0051] (4) Pour high discharge capacity lithium nickel manganese oxide and a conductive agent into a mortar and grind them for 35 minutes respectively. Mix high discharge capacity lithium nickel manganese oxide, the conductive agent and the composite binder in a mass ratio of 8:1:1, pour them into a ball mill, stir them for 12 minutes using a high-speed oscillating ball mill, evenly spread them on a carbon-coated aluminum foil, and vacuum dry them at 60°C for 3.5 hours, and then vacuum dry them at 120°C for 11 hours to obtain a high discharge capacity lithium nickel manganese oxide positive electrode material.
[0052] Comparative Example 2
[0053] A method for preparing a lithium nickel manganese oxide positive electrode material with a high discharge specific capacity, the method for preparing a lithium nickel manganese oxide positive electrode material with a high discharge specific capacity comprising the following preparation steps:
[0054] (1) Manganese sulfate and nickel sulfate were added to pure water at a molar ratio of 3:1 to prepare a 2 mol / L solution, and the solution was input into a liquid-phase stirred reactor using a peristaltic pump under a nitrogen atmosphere. The precipitant solution was then input into the liquid-phase stirred reactor using a peristaltic pump at a volume ratio of 1:1.2. The precipitant solution was added at 55°C and 60 r / min, and the pH was maintained at 8.1. After the precipitant solution was completely added, the reaction was continued for 19 hours, filtered, and vacuum dried at 85°C for 9 hours to obtain a nickel manganese carbonate precursor;
[0055] (2) lithium carbonate, nickel manganese carbonate precursor, aluminum hydroxide, and ruthenium oxide were fully mixed in a mass ratio of 1:5.74:0.1:0.11, poured into a mortar and ground for 1.5 hours, calcined at 190°C for 1 hour, 360°C for 1.5 hours, 560°C for 1 hour, and 900°C for 20 hours in an oxygen atmosphere, cooled to 700°C and annealed for 11 hours. The heating rate during the calcination process was 10°C / min, and aluminum / ruthenium doped nickel manganese oxide was obtained;
[0056] (3) Pour aluminum / ruthenium-doped lithium nickel manganese oxide and a conductive agent into a mortar and grind them for 35 minutes respectively. Mix the high discharge capacity lithium nickel manganese oxide, the conductive agent and the composite binder in a mass ratio of 8:1:1, pour them into a ball mill, stir them for 12 minutes using a high-speed oscillating ball mill, evenly spread them on a carbon-coated aluminum foil, and vacuum dry them at 60°C for 3.5 hours, and then vacuum dry them at 120°C for 11 hours to obtain a high discharge capacity lithium nickel manganese oxide positive electrode material.
[0057] Comparative Example 3
[0058] A method for preparing a lithium nickel manganese oxide positive electrode material with a high discharge specific capacity, the method for preparing a lithium nickel manganese oxide positive electrode material with a high discharge specific capacity comprising the following preparation steps:
[0059] (1) Manganese sulfate and nickel sulfate were added to pure water at a molar ratio of 3:1 to prepare a 2 mol / L solution, and the solution was input into a liquid-phase stirred reactor using a peristaltic pump under a nitrogen atmosphere. The precipitant solution was then input into the liquid-phase stirred reactor using a peristaltic pump at a volume ratio of 1:1.2. The precipitant solution was added at 55°C and 60 r / min, and the pH was maintained at 8.1. After the precipitant solution was completely added, the reaction was continued for 19 hours, filtered, and vacuum dried at 85°C for 9 hours to obtain a nickel manganese carbonate precursor;
[0060] (2) lithium carbonate, nickel manganese carbonate precursor, aluminum hydroxide, and ruthenium oxide were fully mixed in a mass ratio of 1:5.74:0.1:0.11, poured into a mortar and ground for 1.5 hours, calcined at 190°C for 1 hour, 360°C for 1.5 hours, 560°C for 1 hour, and 900°C for 20 hours in an oxygen atmosphere, cooled to 700°C and annealed for 11 hours. The heating rate during the calcination process was 10°C / min, and aluminum / ruthenium doped nickel manganese oxide was obtained;
[0061] (3) Aluminum / ruthenium doped lithium nickel manganese oxide, pyrrole, sodium dodecylbenzene sulfonate and pure water were mixed in a mass ratio of 1:0.05:0.0005:55, and ultrasonically dispersed for 11 minutes. A 20 g / L ferric chloride solution equal to the mass of pure water was added dropwise in an ice water bath at 150 r / min, 6 drops per second. After the addition was completed, the reaction was continued for 13 hours, filtered, washed with pure water 4 times, and vacuum dried at 65°C for 11 hours to obtain lithium nickel manganese oxide with high discharge specific capacity;
[0062] (4) Pour high discharge capacity lithium nickel manganese oxide and a conductive agent into a mortar and grind them for 35 minutes respectively. Mix high discharge capacity lithium nickel manganese oxide, the conductive agent and the composite binder in a mass ratio of 8:1:1, pour them into a ball mill, stir them for 12 minutes using a high-speed oscillating ball mill, evenly spread them on aluminum foil, and vacuum dry them at 60°C for 3.5 hours, and then vacuum dry them at 120°C for 11 hours to obtain a high discharge capacity lithium nickel manganese oxide positive electrode material.
[0063] Comparative Example 4
[0064] A method for preparing a lithium nickel manganese oxide positive electrode material with a high discharge specific capacity, the method for preparing a lithium nickel manganese oxide positive electrode material with a high discharge specific capacity comprising the following preparation steps:
[0065] (1) Manganese sulfate and nickel sulfate were added to pure water at a molar ratio of 3:1 to prepare a 2 mol / L solution, and the solution was input into a liquid-phase stirred reactor using a peristaltic pump under a nitrogen atmosphere. The precipitant solution was then input into the liquid-phase stirred reactor using a peristaltic pump at a volume ratio of 1:1.2. The precipitant solution was added at 55°C and 60 r / min, and the pH was maintained at 8.1. After the precipitant solution was completely added, the reaction was continued for 19 hours, filtered, and vacuum dried at 85°C for 9 hours to obtain a nickel manganese carbonate precursor;
[0066] (2) lithium carbonate, nickel manganese carbonate precursor, aluminum hydroxide, and ruthenium oxide were fully mixed in a mass ratio of 1:5.74:0.1:0.11, poured into a mortar and ground for 1.5 hours, calcined at 190°C for 1 hour, 360°C for 1.5 hours, 560°C for 1 hour, and 900°C for 20 hours in an oxygen atmosphere, cooled to 700°C and annealed for 11 hours. The heating rate during the calcination process was 10°C / min, and aluminum / ruthenium doped nickel manganese oxide was obtained;
[0067] (3) Aluminum / ruthenium doped lithium nickel manganese oxide, pyrrole, sodium dodecylbenzene sulfonate and pure water were mixed in a mass ratio of 1:0.05:0.0005:55, and ultrasonically dispersed for 11 minutes. A 20 g / L ferric chloride solution equal to the mass of pure water was added dropwise in an ice water bath at 150 r / min, 6 drops per second. After the addition was completed, the reaction was continued for 13 hours, filtered, washed with pure water 4 times, and vacuum dried at 65°C for 11 hours to obtain lithium nickel manganese oxide with high discharge specific capacity;
[0068] (4) By mass, 8 parts of high discharge capacity lithium nickel manganese oxide and 1 part of conductive agent were poured into a mortar and mixed evenly, and ground for 35 minutes. 1 part of polyvinylidene fluoride and 25 parts of N-methylpyrrolidone were mixed evenly, and stirred at 300 r / min until dissolved. The mixed high discharge capacity lithium nickel manganese oxide and conductive agent were added and poured into a ball mill together. The mixture was stirred for 20 minutes using a high-speed oscillating ball mill, and the mixture was evenly applied on a carbon-coated aluminum foil. The mixture was vacuum dried at 60°C for 3.5 hours, and then vacuum dried at 120°C for 11 hours to obtain a high discharge capacity lithium nickel manganese oxide positive electrode material.
[0069] Comparative Example 5
[0070] A method for preparing a lithium nickel manganese oxide positive electrode material with a high discharge specific capacity, the method for preparing a lithium nickel manganese oxide positive electrode material with a high discharge specific capacity comprising the following preparation steps:
[0071] (1) Manganese sulfate and nickel sulfate were added to pure water at a molar ratio of 3:1 to prepare a 2 mol / L solution, and the solution was input into a liquid-phase stirred reactor using a peristaltic pump under a nitrogen atmosphere. The precipitant solution was then input into the liquid-phase stirred reactor using a peristaltic pump at a volume ratio of 1:1.2. The precipitant solution was added at 55°C and 60 r / min, and the pH was maintained at 8.1. After the precipitant solution was completely added, the reaction was continued for 19 hours, filtered, and vacuum dried at 85°C for 9 hours to obtain a nickel manganese carbonate precursor;
[0072] (2) lithium carbonate, nickel manganese carbonate precursor, aluminum hydroxide, and ruthenium oxide were fully mixed in a mass ratio of 1:5.74:0.1:0.11, poured into a mortar and ground for 1.5 hours, preheated at 500°C for 4 hours, calcined at 900°C for 20 hours, cooled to 700°C for annealing for 11 hours, and the heating rate during the calcination process was 10°C / min to obtain aluminum / ruthenium doped lithium nickel manganese oxide;
[0073] (3) Aluminum / ruthenium doped lithium nickel manganese oxide, pyrrole, sodium dodecylbenzene sulfonate and pure water were mixed in a mass ratio of 1:0.05:0.0005:55, and ultrasonically dispersed for 11 minutes. A 20 g / L ferric chloride solution equal to the mass of pure water was added dropwise in an ice water bath at 150 r / min, 6 drops per second. After the addition was completed, the reaction was continued for 13 hours, filtered, washed with pure water 4 times, and vacuum dried at 65°C for 11 hours to obtain lithium nickel manganese oxide with high discharge specific capacity;
[0074] (4) Pour high discharge capacity lithium nickel manganese oxide and a conductive agent into a mortar and grind them for 35 minutes respectively. Mix high discharge capacity lithium nickel manganese oxide, the conductive agent and the composite binder in a mass ratio of 8:1:1, pour them into a ball mill, stir them for 12 minutes using a high-speed oscillating ball mill, evenly spread them on a carbon-coated aluminum foil, and vacuum dry them at 60°C for 3.5 hours, and then vacuum dry them at 120°C for 11 hours to obtain a high discharge capacity lithium nickel manganese oxide positive electrode material.
[0075] The half-cell assembly method used in the subsequent test cases is as follows:
[0076] The prepared high discharge capacity lithium nickel manganese oxide positive electrode material was cut into 10 mm diameter round pole pieces with smooth edges using a punching machine. The remaining materials were assembled into button-type half-cells according to GB / T 43093-2023 for subsequent testing.
[0077] Test Example 1
[0078] First charge and discharge specific capacity test: Use a current density of 0.1C for the first charge and discharge specific capacity test, define 1C as 140mA / g, charge at constant current to 4.95V, discharge at constant current to 3.0V, and record the data.
[0079] The results are shown in Table 1.
[0080] Table 1
[0081]
[0082] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 5 in Table 1, it can be found that the high discharge specific capacity lithium nickel manganese oxide positive electrode material prepared by the present invention has a high charge and discharge specific capacity and good coulombic efficiency.
[0083] By comparison, the charge-discharge specific capacity and coulombic efficiency of Examples 1 to 3 are greater than those of Comparative Example 1, indicating that the doping of aluminum and ruthenium elements improves the charge-discharge specific capacity and improves the lithium ion and electron transmission efficiency.
[0084] By comparison, the charge-discharge specific capacity of Examples 1 to 3 is greater than that of Comparative Example 5, indicating that the step calcination system allows each step to fully react, reduces the generation of impurity phases, and improves the charge-discharge specific capacity.
[0085] Test Example 2
[0086] High and low temperature cycle performance test: Use a current density of 0.5C to conduct a cycle performance test on a high discharge capacity lithium nickel manganese oxide positive electrode material, define 1C as 140mA / g, low temperature as 25°C, high temperature as 55°C, 2500 low temperature cycles, 1500 high temperature cycles. The low temperature discharge capacity of the battery at a current density of 0.5C is measured in advance to be 137.6mAh / g, and the high temperature discharge capacity is 134.4mAh / g. Record the data.
[0087] The results are shown in Table 2.
[0088] Table 2
[0089]
[0090] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 5 in Table 2, it can be found that the high discharge specific capacity lithium nickel manganese oxide positive electrode material prepared by the present invention has a good high and low temperature cycle life.
[0091] By comparison, the high and low temperature capacity retention rates of Examples 1 to 3 are greater than those of Comparative Example 1, indicating that the doping of aluminum and ruthenium effectively improves the stability of the spinel structure, and the inhibition of impurity phase formation also reduces its impact on capacity loss during the cycle, thereby improving the high and low temperature cycle life.
[0092] By comparison, the high and low temperature capacity retention rates of Examples 1 to 3 are greater than those of Comparative Example 2, indicating that the polypyrrole coating significantly reduces the corrosion of the transition metal solution and the electrolyte to the electrode, greatly reduces the capacity loss during the cycle, and improves the high and low temperature cycle life.
[0093] By comparison, the high and low temperature capacity retention rates of Examples 1 to 3 are greater than that of Comparative Example 3, indicating that the carbon coating protection of the aluminum foil prevents the current collector from being corroded by the electrolyte, reduces the capacity loss caused by the contact failure between the current collector and the active material, and improves the high and low temperature cycle life.
[0094] By comparison, the high and low temperature capacity retention rates of Examples 1 to 3 are greater than those of Comparative Example 4, indicating that the composite binder exhibits good viscosity under a high voltage working environment. At the same time, the good wettability of the aqueous binder also ensures sufficient contact between the electrolyte and the active material, thereby improving the high and low temperature cycle life.
[0095] By comparison, the high and low temperature capacity retention rates of Examples 1 to 3 are greater than those of Comparative Example 5, indicating that the better microstructure brought about by the step calcination leads to less capacity loss and improves the high and low temperature cycle life.
[0096] Test Example 3
[0097] Rate performance test: At room temperature, use current densities of 0.1C, 0.5C, 1C, 2C, 5C, 10C, 20C, and 40C for 5 cycles respectively, defining 1C as 140mA / g, to test the rate performance of high discharge capacity lithium nickel manganese oxide positive electrode materials and record the data.
[0098] The results are shown in Table 3.
[0099] Table 3
[0100]
[0101] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 5 in Table 3, it can be found that the high discharge specific capacity lithium nickel manganese oxide positive electrode material prepared by the present invention has good rate performance.
[0102] By comparison, the rate discharge specific capacity of Examples 1 to 3 is greater than that of Comparative Example 1, indicating that the doping of aluminum and ruthenium inhibits the formation of impurity phases and increases the Mn 2+ The ion content weakens the Jan-Taylor effect, improves conductivity, and enhances rate performance.
[0103] By comparison, the rate discharge capacity of Examples 1 to 3 is greater than that of Comparative Example 2, indicating that the polypyrrole coating protects the internal high-discharge capacity lithium nickel manganese oxide from corrosion by the electrolyte, preventing the Mn 2+ The dissolution of ions improves rate performance.
[0104] By comparison, the rate discharge specific capacity of Examples 1 to 3 is greater than the rate discharge specific capacity of Comparative Example 3, indicating that the introduction of the carbon-coated aluminum foil protects the aluminum foil from the corrosion of the electrolyte and reduces the contact failure effect between the active material and the aluminum foil current collector.
[0105] By comparison, the rate discharge specific capacity of Examples 1 to 3 is greater than that of Comparative Example 4, indicating that the use of the composite binder improves the adhesion under high voltage and high current, reduces the contact failure effect between the active material and the aluminum foil current collector, and reduces the Mn 2+ The dissolution of ions improves rate performance.
[0106] By comparison, the rate discharge specific capacity of Examples 1 to 3 is greater than that of Comparative Example 5, indicating that the material generated by the step calcination has a better microscopic morphology, and the step heating avoids the breakage of the microscopic microspheres, so that it has better electrochemical performance and improves the rate performance.
[0107] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for preparing a high discharge specific capacity lithium nickel manganese oxide positive electrode material, characterized in that: The method comprises the following preparation steps: (1) Manganese sulfate and nickel sulfate were added to pure water at a molar ratio of 3:1 to prepare a 2 mol / L solution, and the solution was input into a liquid phase stirred reactor using a peristaltic pump under a nitrogen atmosphere. The precipitant solution was then input into the liquid phase stirred reactor using a peristaltic pump at a volume ratio of 1:1.
2. The precipitant solution was added at 50-55°C and 50-60 r / min. The speed of adding the precipitant solution was controlled to maintain the pH at 8.
1. After the precipitant solution was completely added, the solution was reacted for 18-20 hours, filtered, and vacuum dried at 80-90°C for 8-10 hours to obtain a nickel manganese carbonate precursor. (2) lithium carbonate, nickel manganese carbonate precursor, aluminum hydroxide, and ruthenium oxide are fully mixed in a mass ratio of 1:(5.73-5.75):(0.09-0.11):(0.1-0.11), poured into a mortar and ground for 1-1.5 hours, and step-calcined in an oxygen atmosphere to obtain aluminum / ruthenium-doped lithium nickel manganese oxide; (3) Aluminum / ruthenium doped lithium nickel manganese oxide, pyrrole, sodium dodecylbenzene sulfonate and pure water are mixed evenly according to the formula, ultrasonically dispersed for 10-12 minutes, and a 20 g / L ferric chloride solution equal to the mass of pure water is added dropwise in an ice water bath at 100-150 r / min, 5-6 drops per second. After the addition is completed, the reaction is carried out for 12-15 hours, filtered, washed with pure water 3-5 times, and vacuum dried at 60-70°C for 10-12 hours to obtain lithium nickel manganese oxide with high discharge specific capacity; (4) Pour high discharge capacity lithium nickel manganese oxide and conductive agent into a mortar and grind for 30-40 minutes respectively, mix high discharge capacity lithium nickel manganese oxide, conductive agent and composite binder in a mass ratio of 8:1:1, pour into a ball mill, stir for 10-15 minutes using a high-speed swing ball mill, evenly apply on a carbon-coated aluminum foil, vacuum dry at 60°C for 3-4 hours, and then vacuum dry at 120°C for 10-12 hours to obtain a high discharge capacity lithium nickel manganese oxide positive electrode material; The aluminum / ruthenium doped lithium nickel manganese oxide has an ordered P4332 space group structure; The step calcination is calcined at 180-200° C. for 1-1.5 h, calcined at 350-370° C. for 1.5-2 h, calcined at 550-570° C. for 1-1.5 h, calcined at 900° C. for 20 h, cooled to 700° C. for annealing for 10-12 h, and the heating rate during the calcination process is 10° C. / min; The composite binder is prepared by uniformly mixing guar gum, O-carboxymethyl chitosan and pure water in a mass ratio of 1:4:30, stirring at 70-80°C and 200-300 r / min until dissolved, and naturally cooling to room temperature; The substitution degree of the O-carboxymethyl chitosan is 60% to 70%.
2. The method for preparing a high discharge specific capacity lithium nickel manganese oxide positive electrode material according to claim 1, characterized in that: The precipitant solution in step (1) is prepared by uniformly mixing sodium carbonate, ammonia monohydrate and pure water in a mass ratio of 1:12:60, and stirring at room temperature at 150-250 r / min until dissolved.
3. The method for preparing a high discharge specific capacity lithium nickel manganese oxide positive electrode material according to claim 1, characterized in that: The formula of step (3) is aluminum / ruthenium doped lithium nickel manganese oxide, pyrrole, sodium dodecylbenzene sulfonate, and pure water in a mass ratio of 1:(0.045-0.055):(0.0005-0.0006):(50-60).
4. The method for preparing a high discharge capacity lithium nickel manganese oxide positive electrode material according to claim 1, characterized in that: The conductive agent in step (4) is acetylene black, and the median diameter is 1-3 μm.
5. A high discharge specific capacity lithium nickel manganese oxide positive electrode material prepared according to the method for preparing a high discharge specific capacity lithium nickel manganese oxide positive electrode material according to any one of claims 1 to 4.
6. Use of a high discharge specific capacity lithium nickel manganese oxide positive electrode material prepared by the method for preparing a high discharge specific capacity lithium nickel manganese oxide positive electrode material according to any one of claims 1 to 4 in a lithium ion battery.