A silicon-carbon composite negative electrode material using one-dimensional material to enhance structural stability and a preparation method thereof

By dispersing surface hydroxyl modified nano-one-dimensional materials in porous carbon framework, combined with chemical vapor deposition and carbonization treatment, the problem of structural degradation of silicon-based anode materials during the deliquification process is solved, and the circulation of lithium-ion batteries is significantly improved Stability and electrochemical properties.

CN118658996BActive Publication Date: 2024-11-15BEIJING IAMETAL NEW ENERGY TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411139863.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-15
Estimated Expiration
2044-08-20

AI Technical Summary

Technical Problem

Volume changes in silicon-based anode material during the deliquification process lead to structural degradation and unstable solid electrolyte interface layer, reducing the cyclic stability of lithium-ion batteries. It is difficult for the prior art to effectively improve the structural strength of porous carbon skeletons and sub-nano silicon. Stability of particles.

Method used

By uniformly dispersing the surface hydroxyl modified nano-one-dimensional material in the porous carbon framework, a one-dimensional material-reinforced silicon-carbon composite anode material is formed, and the silicon source is introduced into the carbon framework by chemical vapor deposition, combining carbonization and activation treatment, Enhance the structural strength of the carbon framework and improve the dispersion and binding force of nano-one-dimensional materials through surface hydroxylation modification.

Benefits of technology

The cyclic stability and electrochemical performance of silicon-based anode materials are significantly improved, especially under high magnification conditions, which significantly improves the structural stability and electron transmission capabilities of the materials and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118658996B_ABST
    Figure CN118658996B_ABST
Patent Text Reader

Abstract

The present invention relates to a silicon-carbon composite negative electrode material that utilizes one-dimensional materials to enhance structural stability and a preparation method thereof. The silicon-carbon composite negative electrode material is a porous carbon material dispersed with nano one-dimensional materials as a skeleton, and a silicon source gas is compounded into the porous carbon skeleton by chemical vapor deposition; the porous carbon material uniformly dispersed with the nano one-dimensional materials is a nano one-dimensional material with surface hydroxyl modified dispersed in a liquid resin precursor, and a curing agent is added, and the material is cured and sintered. The one-dimensional material is uniformly dispersed in the particles of the silicon-carbon composite negative electrode material, providing a skeleton function to support the integrity of the particles, and at the same time ensuring the structural stability of the silicon-carbon composite negative electrode material when the volume changes during the charge and discharge process. The preparation method of the present invention is simple, conducive to industrial implementation, and the silicon-carbon composite material has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of batteries, and in particular relates to a silicon-carbon composite negative electrode material that utilizes one-dimensional materials to enhance structural stability and a preparation method thereof. Background Art

[0002] Using high-capacity anode materials to replace traditional graphite anodes is currently the most effective way to achieve higher energy density lithium-ion batteries. Silicon-based anode materials store lithium through alloying reactions with lithium, and their theoretical specific capacity can reach 4200 mAh / g, which is considered to be the most promising alternative. However, the practical application of silicon-based anodes also faces huge challenges. Silicon-based anode materials undergo huge volume changes during the process of lithium insertion and extraction, which leads to particle fragmentation and pulverization, causing severe structural degradation of silicon material particles and the formation of an unstable solid electrolyte interface layer, which reduces the cycle stability of the battery.

[0003] In order to solve the problems faced by the above-mentioned silicon-based negative electrode materials, many pioneering studies have shown that reducing the characteristic size of silicon materials to the nanometer level can allow silicon particles to withstand huge volume strains without breaking and provide excellent electrochemical performance. For example, the volume strain caused by sub-nanometer-sized (<1nm) silicon particles is much smaller than that of larger-sized silicon particles. Therefore, sub-nanometer-level silicon materials show excellent kinetics and cycle excellence, which can meet the practical standards of silicon-based negative electrode materials. At present, there are not many methods for preparing silicon materials with sub-nanometer dimensions. The main research direction is still at the nanometer level or at the level of several nanometers, such as silicon nanosheets, silicon nanowires, silicon nanotubes, etc., whose macroscopic size is still a few nanometers or even tens of nanometers, and cannot effectively improve the electrochemical performance of the material. Although alloying, redox method, sol-gel method, chemical vapor deposition method and mechanical grinding can further significantly reduce the size of silicon materials, they all have limitations in achieving uniform sub-nanometer-level preparation.

[0004] Introducing a gaseous silicon source into a carbon skeleton with a microporous structure is an effective method for preparing sub-nano silicon materials. For example, introducing gaseous silane into a microporous carbon skeleton by chemical vapor infiltration, and cracking the gaseous silane to form sub-nano silicon under appropriate conditions can significantly improve the cycle stability of silicon-based materials. Commonly used carbon skeleton materials are generally prepared by high-temperature cracking and carbonization of polymer materials and biomass materials, pore-forming activation, etc. Since polymer materials and biomass materials are hard carbon after cracking, they have many defects, and the activation pore-forming destroys their structural stability. Therefore, conventional porous carbon skeleton materials have poor structural stability and are difficult to withstand the rolling process in the battery preparation process and the stress generated by the volume expansion of silicon materials, which will also cause particle damage and rapid performance decay. Therefore, improving the structural strength of the carbon skeleton loaded with sub-nano silicon particles becomes the key point to further optimize the performance of silicon-based negative electrode materials.

[0005] The prior art uses one-dimensional nanomaterials as raw materials to prepare silicon-carbon composite negative electrode materials, generally as a conductive agent, and a binder and a negative electrode active material to make a slurry, and then prepare the negative electrode material. One-dimensional nanomaterials such as carbon nanotubes only play a conductive role, and do not play a role in enhancing the structural strength of the particles themselves and improving the electron transmission capacity inside the particles. There are reports in the prior art that use one-dimensional nanomaterials and hard carbon precursors to mix and prepare silicon-carbon composite negative electrode materials. For example, CN117174885A reports a silicon-carbon negative electrode material and its preparation method and application, in which an organic carbon source such as asphalt is added together with carbon nanotubes, but the patent does not use the interaction between carbon nanotubes and other organic carbon sources, but only uses them as additives, and this method cannot effectively improve the structural strength of the material itself. In addition, patent CN116825994A discloses a silicon-carbon composite silicon-based negative electrode material, in which the steps involve adding carbon nanotubes to the hard carbon precursor and then performing secondary sintering. This patent involves evenly mixing a solid-phase hard carbon precursor and carbon nanotubes before sintering. There is no interaction between the carbon nanotubes and the hard carbon precursor, and they cannot improve the structural strength of the material, maintain structural stability, or enhance the ability of electron transport within the material. Summary of the invention

[0006] The purpose of the present invention is to improve the structural stability of porous carbon materials loaded with sub-nanometer silicon material carriers, and to provide a silicon-carbon composite negative electrode material with enhanced structural stability of one-dimensional materials and a preparation method thereof. Nano one-dimensional materials with good structural strength are uniformly dispersed in the precursor material for preparing the porous carbon skeleton, and the one-dimensional materials are uniformly fixed in the porous carbon skeleton during the carbonization process of the precursor of the porous carbon skeleton, so that the overall structural strength of the carbon skeleton is enhanced, and the structural stability of the sub-nanometer silicon particle material when the volume changes during the lithium insertion and extraction process is maintained, thereby improving the cycle stability of the silicon-based negative electrode material.

[0007] The first purpose of the present invention is to provide a silicon-carbon composite negative electrode material that utilizes one-dimensional materials to enhance structural stability. The material is a porous carbon material with nano one-dimensional materials uniformly dispersed as a skeleton, and a silicon source gas is composited into the porous carbon skeleton through chemical vapor deposition; the porous carbon material with nano one-dimensional materials uniformly dispersed is a nano one-dimensional material with surface hydroxyl modified dispersed in a liquid resin precursor, and a curing agent is added, and the material is cured and sintered.

[0008] Furthermore, the mass proportion of silicon material in the silicon-carbon composite material is 30-80%, preferably 40-60%, and the median particle size of the silicon-carbon composite material is 1-30 μm, preferably 2-20 μm.

[0009] Furthermore, the one-dimensional nanomaterial includes, but is not limited to, carbon nanotubes, carbon nanowires, carbon nanorods, carbon fibers, metal nanowires, silicon nanowires, glass fibers, aluminum silicate fibers, and aluminum oxide fibers; the diameter of the one-dimensional nanomaterial is 0.5-100 nm, and the length is 0.1-10 μm. Preferably, the diameter of the one-dimensional nanomaterial is 0.6-50 nm, and the length is 0.2-5 μm.

[0010] Furthermore, the mass ratio of the liquid resin oligomer, the modified nano one-dimensional material, and the curing agent is 100:1-2:0.5-1; further, the curing agent is selected from at least one of hexamethylenetetramine, ammonium chloride, and benzenesulfonyl chloride.

[0011] The present invention performs surface hydroxylation modification on the nano one-dimensional material, so that the nano one-dimensional material can be evenly dispersed inside or inside and on the surface of the silicon-carbon composite material particles, providing a skeleton function to support the silicon-carbon composite material, while ensuring the structural stability of the silicon-carbon composite negative electrode material when the volume changes during the charge and discharge process. If the surface of the nano one-dimensional material is not modified by hydroxylation, it is not conducive to the combination of the one-dimensional material and the carbon substrate, and the support function of the carbon substrate cannot be effectively provided, thereby affecting the overall stability of the material.

[0012] Furthermore, the surface hydroxylation modification method of the nano one-dimensional material is carried out using an acid-base oxidation method, in which the nano one-dimensional material is placed in an acidic or alkaline environment for treatment, and then an oxidation reaction is performed to generate hydroxyl functional groups on the surface of the carbon nanotube. This method utilizes the corrosion of the surface of the carbon nanotube by acid and alkali, and the further oxidation of the corrosion products by the oxidant, thereby forming hydroxyl groups on the surface of the carbon nanotube. The hydroxyl content is characterized by the Boehm titration method, and the hydroxyl content is preferably 1%-3%. Too high a hydroxyl concentration will cause the one-dimensional material to have reduced conductivity and too tight a bond with the carbon substrate to lose flexibility. Too low a hydroxyl concentration will cause a loose bond with the carbon substrate, reducing the effect of enhancing structural stability.

[0013] In a preferred technical scheme of the present invention, the surface hydroxyl-modified nano one-dimensional material is prepared by a preparation method comprising the following steps: the nano one-dimensional material is placed in a mixed acid of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 1:1-3, heated in a water bath at 40-60°C for 2-5h, neutralized, separated, washed, and dried to obtain the surface hydroxyl-modified nano one-dimensional material.

[0014] Hydroxylation on the surface of nano-one-dimensional materials can introduce hydrophilic hydroxyl groups, significantly enhancing the hydrophilicity and dispersibility of the one-dimensional materials in water. This helps the stable dispersion of the one-dimensional materials in the solution, while providing active sites for further chemical modification and reaction, improving their processing and application performance, increasing the binding force with phenolic resin, so that the phenolic resin and nano-one-dimensional materials form a structure similar to "reinforced concrete", and improving the structural stability and particle strength of the composite carbon substrate.

[0015] Furthermore, a porous carbon material uniformly dispersed with nano one-dimensional materials is obtained by a preparation method comprising the following steps: adding modified nano one-dimensional materials and a curing agent to a liquid resin oligomer, heating for curing reaction, and obtaining a solid resin; and carbonizing the solid resin at high temperature under an inert atmosphere to activate pores, and obtaining a porous carbon material uniformly dispersed with nano one-dimensional materials.

[0016] Furthermore, the pore volume of the porous carbon material is 0.4-1.2 cm 3 / g, preferably 0.5-1.1 cm 3 / g; pore size distribution is micro-mesopores, wherein the volume proportion of micropores (pore size <2 nm) is 50-98%, preferably 60-95%, and the volume proportion of mesopores (pore size 2-50 nm) is 2-50%, preferably 5-40%.

[0017] A second object of the present invention is to provide a method for preparing the above-mentioned silicon-carbon composite negative electrode material, comprising the following steps:

[0018] (S1) Surface modification of nano one-dimensional materials: The nano one-dimensional materials are placed in a mixture of concentrated nitric acid and concentrated sulfuric acid (volume ratio 1:1-3), and heated in a water bath at 40-60°C for 2-5 hours to cause an oxidation reaction on the surface of the carbon nanotubes. Subsequently, ammonia water is used to neutralize the mixture to pH = 6-7 and the mixture is separated and dried.

[0019] The inventors found that the degree of surface hydroxyl modification of the nano one-dimensional material should be controlled to a certain extent, that is, heating in a water bath at 50-70°C for 2-4 hours. If the time is too long, the degree of hydroxylation will be too high, which will cause the surface charge density to be too high, thereby increasing the electrostatic repulsion between the one-dimensional materials, which will affect its dispersion stability in certain solvents and increase the defects of the one-dimensional materials, thereby affecting its mechanical properties. If the time is too short, the degree of oxidation is insufficient, and the purpose of increasing the binding force with the phenolic resin cannot be effectively achieved.

[0020] (S2) Preparation of a one-dimensional material composite carbon material precursor: reacting phenolic monomers and aldehyde monomers to obtain liquid phenolic resin oligomers, uniformly dispersing the surface-modified nano one-dimensional material, adding a curing agent after uniform stirring, and heating to cure, thereby obtaining a solid phenolic resin uniformly dispersed with the one-dimensional material;

[0021] The phenol monomers include, but are not limited to, phenol, o-cresol, m-cresol, p-cresol and other cresols, o-ethylphenol, m-ethylphenol, p-ethylphenol and other ethylphenols, isopropylphenol, butylphenol, p-tert-butylphenol and other butylphenols, p-tert-amylphenol, p-octylphenol, p-nonylphenol, p-cumylphenol and other alkylphenols, fluorophenol, chlorophenol, bromophenol, iodophenol and other halogenated phenols, p-phenylphenol, Aminophenol, 2,3-xylenol, 2,4-xylenol, 2,5-xylenol, 2,6-xylenol, 3,4-xylenol, 3,5-xylenol and other xylenols; the aldehyde monomers include but are not limited to formaldehyde, acetaldehyde, propionaldehyde, glutaraldehyde, furfural; the molar ratio of the phenol monomer to the aldehyde monomer is between 1:1 and 1:2, the reaction process needs to be carried out in the presence of an alkaline catalyst, the alkaline catalyst includes but is not limited to lithium hydroxide, lithium carbonate, sodium hydroxide, sodium carbonate, sodium bicarbonate, potassium hydroxide, potassium carbonate, potassium bicarbonate, ammonia water; the reaction needs to be carried out in the presence of a solvent, and according to the characteristics of the dispersed one-dimensional material, the solvent can be an aqueous solvent or an oil solvent; the curing agent is hexamethylenetetramine.

[0022] (S3) Preparation of a porous carbon substrate composited with a one-dimensional material: crushing the solid phenolic resin uniformly dispersed with the one-dimensional material into a suitable particle size, heating to 600-1000° C. for pyrolysis and carbonization to obtain a carbon substrate composited with a one-dimensional material, and then subjecting the carbon substrate composited with the one-dimensional material to a high-temperature activation and pore-forming treatment to obtain a porous carbon substrate composited with a one-dimensional material;

[0023] The crushing can be carried out by a jaw crusher or a roller crusher, the pyrolysis carbonization can be carried out by a box furnace, a tube furnace, a push plate kiln, or a roller kiln, and the high-temperature activation pore formation can be achieved by physical activation or chemical activation. The physical activation is also called gas activation, which is a commonly used method for preparing porous carbon materials. It mainly uses an oxidizing gas (such as water vapor, CO2, air or a mixed gas thereof) as an activator to react with a carbon precursor or a carbonized material to form a rich pore structure inside. The chemical activation method refers to adding certain chemical reagents, such as KOH and / or NaOH, during the carbonization process of the carbon precursor, and utilizing the decomposition of these reagents and the etching of the carbon matrix to form a developed pore structure.

[0024] (S4) Vapor deposition of silicon source: crushing the porous carbon substrate composited with the one-dimensional material into a suitable particle size, putting it into a reactor and introducing a silicon-containing process gas, wherein the silicon-containing process gas penetrates into the pores of the porous carbon substrate composited with the one-dimensional material and cracks, thereby obtaining a silicon-carbon composite material in which the one-dimensional material is uniformly dispersed;

[0025] Furthermore, the reactor is a vertical fluidized bed reactor or a horizontal rotary kiln reactor; the silicon-containing process gas is selected from at least one of monosilane and disilane. The amount of silicon-containing process gas introduced is such that silicon accounts for 30-80% of the final silicon-carbon composite negative electrode material.

[0026] The reaction conditions for the vapor deposition of the silicon source are to introduce silane gas and nitrogen into the reactor at a volume ratio of 1:5-10 within a temperature range of 400-600°C, so that the silane gas and nitrogen are fully contacted with the porous carbon in the reactor and deposited inside the porous carbon. The deposition time is 8-15 hours.

[0027] In a preferred technical solution of the present invention, after the step (S4) of vapor deposition of the silicon source, there is also a step (S5) of coating the silicon-carbon composite material: the silicon-carbon composite material in which the above-mentioned one-dimensional material is uniformly dispersed is subjected to vapor phase carbon coating by chemical vapor deposition to obtain a silicon-carbon composite material coated with an electron transport layer.

[0028] Furthermore, the gas phase carbon coating refers to the pyrolysis of gaseous carbon sources such as methane, acetylene, ethylene, propane, and propylene at high temperature and coating them on the particle surface of the composite material to enhance the electron transport capacity of the composite material. Furthermore, the thickness of the carbon coating layer is 1-20 nm, preferably 5-10 nm.

[0029] The third object of the present invention is to provide the use of the silicon-carbon composite material as a negative electrode material in a lithium ion battery.

[0030] The present invention disperses a one-dimensional nano material with surface hydroxyl modified in a liquid resin precursor, and controls the degree of hydroxyl modification to achieve uniform, stable and firm dispersion of the one-dimensional nano material in a porous carbon skeleton, which can significantly improve structural stability, maintain the structural stability of sub-nanometer silicon particle materials when volume changes occur during lithium insertion and extraction, and thus improve the cycle stability of silicon-based negative electrode materials, especially the cycle stability under high rate conditions can be significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a scanning electron microscope photograph of the silicon-carbon composite material obtained in Example 1;

[0032] Figure 2 is the X-ray diffraction spectrum of the silicon-carbon composite material obtained in Example 1;

[0033] Figure 3 1 is the charge and discharge curve of the silicon-carbon composite material obtained in Example 1;

[0034] Figure 4 This is the cycle performance curve of the silicon-carbon composite material prepared in Example 1. DETAILED DESCRIPTION

[0035] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments.

[0036] The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.

[0037] The scanning electron microscope (SEM) was JEOL-6701F, and the transmission electron microscope (TEM) was JEM-2100F.

[0038] X-ray diffraction analyzer (XRD, Rigaku D / max 2500, Cu Kα).

[0039] Example 1

[0040] (S1) Surface modification of carbon nanotubes: Carbon nanotubes (diameter 1.5 nm, length 0.8 um) were placed in a mixture of concentrated nitric acid and concentrated sulfuric acid in a volume ratio of 1:3, heated in a water bath at 50°C for 2 h, neutralized with ammonia water to pH 7, centrifuged, washed, and dried to obtain surface-modified carbon nanotubes. The hydroxyl content of the obtained surface-modified carbon nanotubes was characterized by Boehm titration. The hydroxyl content of the obtained surface-modified carbon nanotubes was 1.14%.

[0041] (S2) Preparation of carbon material precursor composited with one-dimensional material: First, add 11.8 kg of meta-diphenol to the reactor, then add 275 g of sodium hydroxide solution with a solid content of 30%, stir evenly, add 11.6 kg of 37% formaldehyde solution, heat to 85 ° C and react at a constant temperature for 2 hours, then cool to 40 ° C, add appropriate amount of citric acid to adjust pH = 8, and obtain 15.2 kg of liquid phenolic resin oligomer. Add 200 g of surface-modified carbon nanotubes obtained in step (S1), stir for 2 hours to make them uniformly dispersed in the above-mentioned liquid phenolic resin oligomer, then use a homogenizer to quickly break up the carbon nanotubes, add 100 g of hexamethylenetetramine, heat to 90 ° C and react at a constant temperature for 2 hours, and obtain a solid phenolic resin uniformly dispersed with one-dimensional materials.

[0042] (S3) Preparation of porous carbon substrate composited with one-dimensional materials: The solid phenolic resin uniformly dispersed with carbon nanotubes obtained in step (S2) was heated to 650°C for 2 hours under nitrogen protection to obtain a carbonized material; the carbonized material was then added to an activation furnace reactor, heated to 900°C and reacted by alkali activation method for 1 hour (the alkali was KOH, and the mass ratio of the alkali to the activated carbon was 2:1), cooled, cleaned and dried to obtain a porous carbon substrate composited with carbon nanotubes; the pore volume was 0.85 cm 3 / g, pore size: 90% micropores (<2nm), 10% mesopores (2-10nm).

[0043] (S4) Vapor deposition of silicon source: The carbon nanotube composite porous carbon substrate obtained in step 2 is placed in a vertical fluidized bed reactor, monosilane gas is introduced at 500°C, and the total amount of monosilane gas introduced is adjusted so that the mass proportion of silicon material is 50%, thereby obtaining a silicon-carbon composite negative electrode material with sub-nanometer silicon deposition.

[0044] (S5) Coating of silicon-carbon composite materials: The temperature of the deposited silicon-carbon composite material is raised to 700°C, and an appropriate amount of acetylene gas is introduced to perform carbon coating by chemical vapor deposition. After reacting for 2 hours, the temperature is lowered and the material is discharged to obtain a carbon-coated silicon-carbon composite material. The thickness of the carbon coating layer is 10 nm.

[0045] Figure 1 This is a scanning electron microscope photograph of the silicon-carbon composite material prepared in Example 1. The particle size is about 7 μm, and the carbon nanotubes are evenly dispersed on the surface and inside of the material.

[0046] Figure 2 The XRD diffraction pattern of the silicon-carbon composite material obtained in Example 1 was analyzed by an X-ray diffraction analyzer (XRD, Rigaku D / max 2500, Cu Kα). It can be seen that the material is amorphous as a whole, and no obvious silicon crystal peak is found.

[0047] Example 2

[0048] Other conditions and operations were the same as those in Example 1, except that in step (S1), water bath heating was performed at 50° C. for 3 h. The hydroxyl content of the obtained surface-modified carbon nanotubes was 2.01%.

[0049] Example 3

[0050] Other conditions and operations were the same as those in Example 1, except that in step (S1), water bath heating was performed at 50° C. for 4 h. The hydroxyl content of the obtained surface-modified carbon nanotubes was 2.78%.

[0051] Example 4

[0052] Other conditions and operations were the same as those in Example 1, except that in step (S1), water bath heating was performed at 50° C. for 5 h. The hydroxyl content of the obtained surface-modified carbon nanotubes was 3.37%.

[0053] Example 5

[0054] Other conditions and operations are the same as those in Example 2, except that in step (S1), the carbon nanotubes are replaced by carbon fibers, and the hydroxyl content of the obtained surface-modified carbon fibers is 1.72%.

[0055] Example 6

[0056] Other conditions and operations are the same as those in Example 2, except that in step (S4), the total amount of silane gas introduced is such that the silicon content accounts for 55%.

[0057] Comparative Example 1

[0058] The other operations are the same as those in Example 2, except that step (S1) is omitted, that is, the surface modification of the carbon nanotubes is not performed. In step (S2), 200 g of unmodified carbon nanotubes are added.

[0059] Comparative Example 2

[0060] The other operations are the same as those in Example 2, except that step (S2) is changed to: 11.8 kg of m-diphenol is added to the reactor, and then 275 g of a sodium hydroxide solution with a solid content of 30% is added, and after stirring evenly, 11.6 kg of a 37% formaldehyde solution is added, and the temperature is raised to 85° C. and the reaction is carried out at a constant temperature for 2 hours, and then the temperature is lowered to 40° C., and an appropriate amount of citric acid is added to adjust the pH to 8 to obtain 15.2 kg of liquid phenolic resin oligomers, and 100 g of hexamethylenetetramine is added, and the reaction is heated to 90° C. and the reaction is carried out at a constant temperature for 2 hours to obtain a solid phenolic resin, and 200 g of surface-modified carbon nanotubes with a hydroxyl content of 2.01% are added, and ball milling is carried out to obtain a solid phenolic resin dispersed with a one-dimensional material.

[0061] Application Examples

[0062] The electrochemical properties of the silicon-based negative electrode materials prepared in the examples and comparative examples were tested according to the following method: the prepared silicon-carbon composite material, carbon black and carboxymethyl cellulose (CMC) were mixed with styrene-butadiene rubber (SBR) composite binder in a mass ratio of 80:10:10 to form a slurry (wherein the mass ratio of CMC to SBR was 1:1), the slurry was uniformly coated on a copper foil current collector, and vacuum dried for 12 h to form a working electrode; a lithium sheet was used as a counter electrode, a glass fiber membrane (purchased from Whatman, UK) was used as a separator, 1 mol / L LiPF6 (the solvent was a mixture of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1) was used as an electrolyte, 1% VC and 5% FEC were added to the electrolyte, and button cells were assembled in an argon atmosphere in a Braun inert gas glove box in Germany.

[0063] The silicon-carbon composite material prepared in Example 1 was subjected to electrochemical analysis test, and the results are as follows: Figure 3 The charge and discharge range is 0-1.5 V. When charged and discharged at a current density of 0.2C, the material capacity can reach 1818.3 mAh / g, and the first cycle coulomb efficiency is 92.1%. Figure 4 This is a capacity retention curve of a battery after 100 cycles at 0.2C, and the capacity retention is as high as 99.1%, proving that the silicon-carbon composite material obtained by the present invention has a high capacity and excellent cycle performance.

[0064] The negative electrode materials of other embodiments and comparative examples were subjected to charge and discharge tests according to the above method, and the results are shown in Table 1 below:

[0065] Table 1 Electrochemical performance test

[0066] .

[0067] In summary, the preparation method of the present invention is simple and efficient, and the obtained silicon-carbon composite material has high first coulombic efficiency, excellent structural stability and cycle performance, and excellent electrochemical performance when used as a negative electrode material for lithium-ion batteries.

Claims

1. A silicon-carbon composite negative electrode material that uses one-dimensional materials to enhance structural stability, which is a porous carbon material with nano one-dimensional materials dispersed as the skeleton, and a silicon source gas is compounded into the porous carbon skeleton by chemical vapor deposition; the porous carbon material with nano one-dimensional materials dispersed is a nano one-dimensional material with surface hydroxyl modified dispersed in a liquid phenolic resin oligomer precursor, and a curing agent is added to cure and sinter the nano one-dimensional material; the nano one-dimensional material includes carbon nanotubes, carbon nanowires, carbon nanorods, carbon fibers, metal nanowires, silicon nanowires, glass fibers, aluminum silicate fibers, and aluminum oxide fibers; the nano one-dimensional material has a diameter of 0.5-100 nm and a length of 0.1-10 μm; The mass ratio of liquid resin oligomer, modified nano one-dimensional material and curing agent is 100:1-2:0.5-1; the curing agent is selected from at least one of hexamethylenetetramine, ammonium chloride and benzenesulfonyl chloride; The hydroxyl content of the surface hydroxyl-modified nano one-dimensional material is 1%-3%.

2. The silicon-carbon composite negative electrode material according to claim 1, characterized in that: The mass proportion of silicon material in the silicon-carbon composite negative electrode material is 30-80%, and the median particle size of the silicon-carbon composite negative electrode material is 1-30 μm.

3. The silicon-carbon composite negative electrode material according to claim 1, characterized in that: The surface hydroxyl-modified nano one-dimensional material is prepared by a preparation method comprising the following steps: the nano one-dimensional material is placed in a mixed acid of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 1:1-3, heated in a water bath at 40-60°C for 2-5h, neutralized, separated, washed, and dried to obtain the surface hydroxyl-modified nano one-dimensional material.

4. The silicon-carbon composite negative electrode material according to claim 1, characterized in that: The pore volume of porous carbon materials is 0.5-1.1 cm 3 / g; the pore size distribution is micropores and mesopores, among which the volume of micropores accounts for 50-98% and the volume of mesopores accounts for 2-50%.

5. The method for preparing the silicon-carbon composite negative electrode material according to any one of claims 1 to 4, characterized in that: The following steps are involved: (S1) Surface modification of nano one-dimensional materials: placing the nano one-dimensional material in a mixed acid of concentrated nitric acid and concentrated sulfuric acid in a volume ratio of 1:1-3, heating in a water bath at 40-60° C. for 2-4 hours, neutralizing to pH=6-7, separating and drying, and obtaining a nano one-dimensional material with surface hydroxyl modified; (S2) Preparation of a one-dimensional material composite carbon material precursor: reacting phenolic monomers and aldehyde monomers to obtain a liquid phenolic resin oligomer, dispersing a surface hydroxyl-modified nano one-dimensional material in the liquid phenolic resin oligomer, adding a curing agent after mixing evenly, and heating and curing to obtain a solid phenolic resin uniformly dispersed with the one-dimensional material; (S3) Preparation of a porous carbon substrate composited with one-dimensional materials: crushing a solid phenolic resin uniformly dispersed with one-dimensional materials, heating it to 600-1000° C. for pyrolysis and carbonization to obtain a carbon substrate composited with one-dimensional materials, and then subjecting the carbon substrate composited with one-dimensional materials to high-temperature activation and pore-forming treatment to obtain a porous carbon substrate composited with one-dimensional materials; (S4) Vapor deposition of silicon source: The porous carbon substrate composited with the above-mentioned one-dimensional material is crushed, put into a reactor and introduced with a silicon-containing process gas, and the vapor deposition of the silicon-containing process gas is carried out at 400-600°C to obtain a silicon-carbon composite negative electrode material with enhanced structural stability using a one-dimensional material.

6. The preparation method according to claim 5, characterized in that: In step (S2), the phenol monomer includes phenol, o-cresol, m-cresol, p-cresol, o-ethylphenol, m-ethylphenol, p-ethylphenol, isopropylphenol, butylphenol, p-tert-butylphenol, p-tert-amylphenol, p-octylphenol, p-nonylphenol, p-cumylphenol, fluorophenol, chlorophenol, bromophenol, iodophenol, p-phenylphenol, aminophenol, 2,3-xylenol, 2,4-xylenol, 2,5-xylenol, 2,6-xylenol, 3,4-xylenol or 3,5-xylenol; the aldehyde monomer includes formaldehyde, acetaldehyde, propionaldehyde, glutaraldehyde or furfural; the molar ratio of the phenol monomer to the aldehyde monomer is 1:1-2; and / or In step (S4), the silicon-containing process gas is selected from at least one of monosilane and disilane, and the amount of silicon-containing process gas introduced satisfies that the silicon in the final silicon-carbon composite negative electrode material accounts for 30-80%; the reaction conditions for the vapor deposition of the silicon source are within the temperature range of 400-600°C, silane gas and nitrogen are introduced into the reactor in a volume ratio of 1:5-10, and the silane gas and nitrogen are fully contacted with the porous carbon in the reactor and deposited into the porous carbon, and the deposition time is 8-15h.

7. The preparation method according to claim 5, characterized in that: After the step (S4) of vapor deposition of silicon source, there is a step (S5) of coating the silicon-carbon composite material: the silicon-carbon composite negative electrode material with enhanced structural stability of the one-dimensional material is vapor-carbon coated by chemical vapor deposition to obtain a silicon-carbon composite material coated with an electron transport layer.