Anion exchange membrane, preparation method and application thereof

Through the grafting technology of ethylene-vinyl alcohol copolymer and 4-imidazole formaldehyde, and the covalent cross-linking of poly4-vinyl benzyl chloride, an efficient anion exchange membrane is constructed, which solves the problem of both anion exchange membrane and The challenges of high ionic conductivity, alkali resistance stability and mechanical properties enable efficient fuel cell performance.

CN118659014BActive Publication Date: 2024-10-29BEI JING ZHI QING KE JI YOU XIAN GONG SI
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411123529.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-10-29
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

Existing anion exchange membranes have challenges in high ionic conductivity, high alkali resistance stability and high mechanical properties, making it difficult to achieve excellent chemical stability, dimensional stability and mechanical properties at the same time.

Method used

Using ethylene-vinyl alcohol copolymer as the main chain, through the grafting of 4-imidazole formaldehyde and p-trifluoromethylbenzaldehyde, a microscopic phase separation ion conduction channel is constructed, and poly4-vinyl benzyl chloride is used as the main chain. Covalent cross-linking is performed to improve mechanical properties and alkali stability.

Benefits of technology

It achieves an anion exchange membrane with high ionic conductivity, low swelling rate and high alkali resistance stability. It has good film-forming properties and mechanical properties and is suitable for efficient fuel cell applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118659014B_ABST
    Figure CN118659014B_ABST
Patent Text Reader

Abstract

The present invention proposes an anion exchange membrane and a preparation method and application, the method comprising: in the presence of a first organic solvent and a free radical initiator, 4-vinylbenzyl chloride monomer is polymerized to obtain poly-4-vinylbenzyl chloride; in the presence of a second organic solvent and hydrochloric acid, ethylene-vinyl alcohol copolymer is reacted with 4-imidazole carboxaldehyde and p-trifluoromethylbenzaldehyde to obtain acetalized ethylene-vinyl alcohol copolymer; in the presence of a third organic solvent, poly-4-vinylbenzyl chloride and acetalized ethylene-vinyl alcohol copolymer are fully mixed, and trimethylamine solution is added thereto, and after the solvent is volatilized and the alkali is replaced, an anion exchange membrane for a fuel cell with high ionic conductivity and high alkali resistance stability is obtained. The preparation process of the anion exchange membrane of the present invention is simple, the film is uniform and transparent, and has the characteristics of high dimensional stability, high ionic conductivity, high strength, and strong chemical stability, and is suitable for use in anion exchange membrane fuel cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of anion exchange membrane fuel cells, and in particular relates to an anion exchange membrane and a preparation method and application thereof. Background Art

[0002] With the breakthroughs in key technologies and key materials of fuel cells, people have shown increasing interest in proton exchange membrane fuel cell (PEMFC) vehicles in recent years, especially in long-distance and heavy-duty applications. However, the main reason limiting the large-scale commercial application of proton exchange membrane fuel cells is that they rely on expensive catalysts and proton exchange membranes. Switching the charge-conducting protons to hydroxides can produce cost-effective anion exchange membrane fuel cells (AEMFCs). The development of high-performance and durable AEMFCs requires anion exchange membranes (AEMs) with excellent chemical stability, high ionic conductivity (ionic conductivity at 80°C is higher than 100 mS cm -1 ), high dimensional stability (swelling rate at 80°C is less than 20%) and excellent mechanical properties.

[0003] At present, researchers mostly choose non-polar main chains as the polymer backbone for preparing AEMs to improve the alkali resistance of the material. Although studies have shown that the alkaline stability of piperidine (DMP) cations is 21 times higher than that of the benchmark benzyltrimethylammonium (BTMA), when grafted onto polymers, considering the cation grafting efficiency, as well as the effects of water content, electronic effects, and spatial stereo effects on chemical stability, BTMA is still an excellent candidate cation. In order to balance ionic conductivity and dimensional stability, it is a smarter approach to construct microscopic phase separation than to increase the ion content. In order to obtain mechanical properties that are both rigid and flexible, in recent years, researchers have focused on how to make the prepared AEMs have both rigid structural units and flexible structural units.

[0004] In the literature (Journal of Membrane Science 2023, 687, 122045), the authors selected rigid poly(p-terphenylpiperidine) (PAP) as the main chain and used expandable flexible dipyridinium cations as crosslinkers to synthesize AEMs. At room temperature and 100% relative humidity, the mechanical strength of the obtained AEMs was 24.6~40.4 MPa, and the elongation at break was 12.4%~20.8%. Due to microphase separation, the AEMs can obtain higher ion conductivity at moderate ion exchange capacity. The PTP-DPC / C6-50% with the best comprehensive performance has an ion exchange capacity of 1.79 mmol / g, and its OH at 80°C is 1.79 mmol / g. - The conductivity is 131.2 mS / cm, and the maximum power density of the H2 / O2 fuel cell assembled with it is 616.2 mW / cm at 80°C. 2Due to the high alkali resistance of the main chain and cations, the ionic conductivity loss rate of PTP-DPC / C6-50% was 10.3% after immersion in 2 mol / L sodium hydroxide solution at 80℃ for 1080 hours. Unfortunately, the material has poor dimensional stability, and the swelling rate of PTP-DPC / C6-50% at 80℃ is as high as 32.9%.

[0005] In the literature (ACS Applied Polymer Materials 2024, 6, 5039-5048), in order to obtain AEMs with high alkali resistance and high dimensional stability, the authors synthesized a series of cross-linked anion exchange membranes SEBS-C6-MDA-TPIPx (x represents the degree of cross-linking) with poly (styrene-b-(ethylene-co-butylene)-b-styrene) (SEBS) and poly (terphenyl piperidine) (TPIP) without polar groups as the main chain. At room temperature and 100% relative humidity, the mechanical strength of the target AEMs is 8.11~24.61 MPa, and the elongation at break is 284.66%~787.28%. When SEBS-C6-MDA-TPIP15% was immersed in 2 mol / L sodium hydroxide solution at 80℃ for 2200 hours, its ion conductivity loss rate was 20.81%. However, the ionic conductivity of this material is relatively low. The ionic conductivity of SEBS-C6-MDA-TPIP15% with the best comprehensive performance is 86.76 mS / cm at 80°C. The maximum power density of the H2 / O2 fuel cell assembled from SEBS-C6-MDA-TPIP15% at 80°C is only 221 mW / cm 2 .

[0006] In summary, there are still challenges in developing anion exchange membranes that have high ionic conductivity, high alkali resistance, high dimensional stability and high mechanical properties. Summary of the invention

[0007] The purpose of the present invention is to provide an anion exchange membrane for a fuel cell with high ionic conductivity and high alkali resistance and stability and a preparation method thereof. Since the hydrophobic side chain can induce microscopic phase separation and construct an efficient ion conduction channel, this type of anion exchange membrane has the characteristics of high ionic conductivity. Since there are covalent crosslinks between the polymer main chains, this type of anion exchange membrane has the characteristics of high strength and low swelling rate. Since the polymer main chain does not contain polar groups, the anion exchange membrane prepared by the present invention also has the characteristics of high alkali resistance and stability.

[0008] According to one aspect of the present invention, there is provided an anion exchange membrane having a structure shown in Formula I:

[0009] Formula I;

[0010] In formula I, x, y, and z represent the proportion of structural units in the polymer;

[0011] The value range of x is 0.05~0.25; the value range of y is 0.30~0.60; the value range of z is 0.35~0.45.

[0012] According to another aspect of the present invention, there is provided a method for preparing the above anion exchange membrane, the method comprising the following steps:

[0013] S1: Under an inert atmosphere, subjecting a mixture I containing a 4-vinylbenzyl chloride monomer, an initiator, and a first organic solvent to a polymerization reaction to obtain poly-4-vinylbenzyl chloride;

[0014] S2: reacting a mixture II containing 4-imidazolecarboxaldehyde, p-trifluoromethylbenzaldehyde, ethylene-vinyl alcohol copolymer, a second organic solvent, and hydrochloric acid with I to obtain an acetalized ethylene-vinyl alcohol copolymer;

[0015] S3: dissolving the poly (4-vinylbenzyl chloride) in a third organic solvent to obtain a poly (4-vinylbenzyl chloride) solution;

[0016] dissolving the acetalized ethylene-vinyl alcohol copolymer in a fourth organic solvent to obtain an acetalized ethylene-vinyl alcohol copolymer solution;

[0017] mixing the poly-4-vinylbenzyl chloride solution with the acetalized ethylene-vinyl alcohol copolymer solution to obtain a mixed solution;

[0018] The mixed solution is reacted with trimethylamine to form a reaction II, and then dried to obtain a halogen-type anion exchange membrane;

[0019] The halogen-type anion exchange membrane is subjected to ion exchange with an alkaline solution to obtain the anion exchange membrane.

[0020] On the basis of the above technical solution, preferably, in the step S1, the mass volume ratio of the 4-vinyl benzyl chloride monomer, the initiator and the first organic solvent is: (4-8 g): (0.15-0.30 g): (35-70 mL).

[0021] On the basis of the above technical solution, preferably, in the step S1, the mass volume ratio of the 4-vinyl benzyl chloride monomer, the initiator, and the first organic solvent is independently selected from any value of 4 g: 0.15 g: 35 mL, 6 g: 0.2 g: 50 mL, 8 g: 0.30 g: 70 mL, or a range value between any two of the above.

[0022] On the basis of the above technical solution, preferably, in step S1, the first organic solvent is tetrahydrofuran.

[0023] On the basis of the above technical solution, preferably, the initiator is a free radical initiator.

[0024] On the basis of the above technical solution, preferably, the free radical initiator is azobisisobutyronitrile.

[0025] On the basis of the above technical solution, preferably, the inert atmosphere is selected from at least one of nitrogen, argon and helium.

[0026] On the basis of the above technical scheme, preferably, in the step S2, the mass volume ratio of the ethylene-vinyl alcohol copolymer, 4-imidazolecarboxaldehyde, p-trifluoromethylbenzaldehyde and the second organic solvent is: (0.5~6 g): (0.28~3.36 g): (0.255~3.06 g): (10~37.5 mL).

[0027] On the basis of the above technical scheme, preferably, in the step S2, the mass volume ratio of the ethylene-vinyl alcohol copolymer, 4-imidazolecarboxaldehyde, p-trifluoromethylbenzaldehyde, and the second organic solvent is independently selected from 0.5 g: 0.28 g: 0.255 g: 10 mL, 2 g: 1.12 g: 1.02 g: 25 mL, 2 g: 0.84 g: 1.52 g: 25 mL, 2 g: 0.56 g: 2.03 g: 25 mL, 2 g: 0.42 g: 2.28 g: 25 mL, 2 g: 0.34 g: 2.44 g: 25 mL, 4 g: 0.56 g: 2.03 g: 30 mL, 6 g: 3.36 g: 3.06 g: 37.5 mL, or any value in the range between any two of the above.

[0028] On the basis of the above technical solution, preferably, the second organic solvent is dimethyl sulfoxide.

[0029] On the basis of the above technical solution, preferably, the hydrochloric acid is added to adjust the pH value of the mixture I to 3-4.

[0030] On the basis of the above technical scheme, preferably, in the step S3, the usage ratio of the poly 4-vinylbenzyl chloride, the third organic solvent, the acetalized ethylene-vinyl alcohol copolymer, the fourth organic solvent, and trimethylamine is: (0.06~0.24 g): (2~8 mL): (0.02~0.08 g): (4~15 mL): (49.2~196.7 μL).

[0031] On the basis of the above technical scheme, preferably, in the step S3, the dosage ratio of the poly 4-vinylbenzyl chloride, the third organic solvent, the acetalized ethylene-vinyl alcohol copolymer, the fourth organic solvent, and trimethylamine is independently selected from any value of 0.06 g: 2 mL: 0.02 g: 4 mL: 49.2 μL, 0.12 g: 4 mL: 0.04 g: 6 mL: 100 μL, 0.18 g: 5 mL: 0.06 g: 10 mL: 147.5 μL, 0.24 g: 8 mL: 0.08 g: 15 mL: 196.7 μL, or a range value between any two of the above.

[0032] On the basis of the above technical solution, preferably, the third organic solvent and the fourth organic solvent are both dimethyl sulfoxide.

[0033] On the basis of the above technical solution, preferably, the alkaline solution is selected from KOH solution and / or NaOH solution.

[0034] Based on the above technical solution, preferably, the temperature of the alkaline solution is 40-80°C.

[0035] On the basis of the above technical solution, preferably, the temperature of the alkaline solution is independently selected from any value of 40°C, 50°C, 60°C, 70°C, 80°C or a range between any two of the above.

[0036] Based on the above technical solution, preferably, the concentration of the alkaline solution is 1~2 mol / L.

[0037] Based on the above technical solution, preferably, in the step S1, the polymerization reaction temperature is 30-60° C., and the polymerization reaction time is 8-12 h.

[0038] On the basis of the above technical solution, preferably, in the step S1, the temperature of the polymerization reaction is independently selected from any value of 30°C, 40°C, 50°C, 60°C or a range between any two of the above.

[0039] On the basis of the above technical solution, preferably, in the step S1, the polymerization reaction time is independently selected from any value among 8 h, 9 h, 10 h, 11 h, 12 h or a range between any two of the above.

[0040] On the basis of the above technical solution, preferably, in the step S2, the dissolution temperature of the ethylene-vinyl alcohol copolymer is 50-80°C.

[0041] On the basis of the above technical solution, preferably, in the step S2, the dissolution temperature of the ethylene-vinyl alcohol copolymer is independently selected from any value of 50°C, 60°C, 70°C, 80°C or a range between any two of the above.

[0042] Based on the above technical solution, preferably, the temperature of reaction I is 60-100° C., and the time of reaction I is 5-8 h.

[0043] On the basis of the above technical solution, preferably, the temperature of the reaction I is independently selected from any value of 60°C, 70°C, 80°C, 90°C, 100°C or a range between any two of the above.

[0044] On the basis of the above technical solution, preferably, the time of the reaction I is independently selected from any value among 5 h, 6 h, 7 h, 8 h or a range between any two of the above.

[0045] On the basis of the above technical solution, preferably, in the step S3, the drying temperature is 70-90°C.

[0046] On the basis of the above technical solution, preferably, in step S3, the drying temperature is independently selected from any value of 70°C, 75°C, 80°C, 85°C, 90°C or a range between any two of the above.

[0047] On the basis of the above technical solution, preferably, the ion exchange between the halogen-type anion exchange membrane and the alkaline solution is performed by immersing the halogen-type anion exchange membrane in the alkaline solution.

[0048] Based on the above technical solution, preferably, the soaking time is 12 to 24 hours.

[0049] On the basis of the above technical solution, preferably, the soaking time is independently selected from any value among 12 h, 14 h, 16 h, 18 h, 20 h, 22 h, 24 h or a range value between any two of the above.

[0050] On the basis of the above technical solution, preferably, during the soaking, the fresh alkali solution is replaced 3 to 5 times.

[0051] On the basis of the above technical solution, preferably, in step S1, the terminator of the polymerization reaction is methanol.

[0052] On the basis of the above technical solution, preferably, in step S2, after the reaction is completed, the pH of the solution is adjusted to 7-8 with 1 mol / L sodium hydroxide; further preferably, the reaction precipitant is deionized water.

[0053] On the basis of the above technical solution, preferably, in step S3, the mixed solution is poured into a mold again, and then dried at 70-90° C. to obtain a halogen-type anion exchange membrane.

[0054] According to another aspect of the present invention, there is provided an application of the anion exchange membrane as described above, or the anion exchange membrane prepared by the preparation method as described above in a fuel cell.

[0055] In the present invention, ethylene-vinyl alcohol copolymer is selected as the main chain. On the one hand, the hydroxyl groups on the structure can react with 4-imidazole formaldehyde to graft a crosslinking agent. On the other hand, the hydroxyl groups on the structure can react with trifluoromethylbenzaldehyde to graft a hydrophobic side chain, which helps to induce microphase separation in the anion exchange membrane and promote ion conduction. The acetal has strong alkali resistance, which can ensure that the anion exchange membrane has high alkali resistance. Thirdly, the polymer structural unit part does not contain hydroxyl groups, which helps to improve the mechanical properties of the anion exchange membrane. Poly 4-vinylbenzyl chloride is selected as the main chain of the ion component. On the one hand, the benzyl chloride groups on the main chain help to react with the crosslinking agent grafted with the ethylene-vinyl alcohol copolymer, which ensures that the anion exchange membrane has a low swelling rate. On the other hand, the benzyl chloride groups on the main chain help to graft cations. Thirdly, the main chain does not contain polar groups, which ensures that the anion exchange membrane has high alkali resistance.

[0056] The beneficial effects that the present invention can produce include:

[0057] 1) The anion exchange membrane preparation method provided by the present invention has simple steps, is easy to implement large-scale production, and has wide applicability.

[0058] 2) The anion exchange membrane preparation method provided by the present invention can achieve adjustable physical and chemical properties by adjusting the grafting degree of 4-imidazolecarboxaldehyde and p-trifluoromethylbenzaldehyde.

[0059] 3) The anion exchange membrane provided by the present invention is uniform and transparent and has good film-forming performance.

[0060] 4) The anion exchange membrane provided by the present invention cross-links poly-4-vinylbenzyl chloride and ethylene-vinyl alcohol copolymer through 4-imidazole formaldehyde, so that the prepared anion exchange membrane has the characteristics of good film forming property, low swelling rate and good mechanical properties.

[0061] 5) The anion exchange membrane provided by the present invention is grafted with trifluoromethylbenzaldehyde, and the hydrophobic effect of fluorine helps the anion exchange membrane to construct hydrophilic and hydrophobic ion channels, thereby improving the ion conductivity of the anion exchange membrane.

[0062] 6) The main chain of the anion exchange membrane provided by the present invention does not contain polar groups and has high alkali resistance and stability.

[0063] 7) The anion exchange membrane provided by the present invention has high application value in hydrogen-oxygen and hydrogen-air fuel cells. BRIEF DESCRIPTION OF THE DRAWINGS

[0064] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0065] Figure 1 This is a physical picture of an anion exchange membrane for a fuel cell with high ionic conductivity and high alkali resistance and stability according to Example 4 of the present invention.

[0066] Figure 2 It is the Fourier transform infrared spectra of Examples 1 to 5 of the present invention.

[0067] Figure 3 These are small-angle X-ray scattering diagrams of Examples 1 to 5 of the present invention.

[0068] Figure 4 The performance curves of hydrogen-oxygen (H2-O2) and hydrogen-air (H2-Air) single cells measured under the test conditions of 100% relative humidity and 80°C battery operating temperature of Example 4 of the present invention are shown.

[0069] Figure 5 The schematic diagram is a method for preparing an anion exchange membrane for a fuel cell with high ionic conductivity and high alkali resistance stability according to the present invention. DETAILED DESCRIPTION

[0070] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0071] The present invention is further illustrated by the following examples.

[0072] 4-Vinylbenzyl chloride, 4-imidazolecarboxaldehyde, and p-trifluoromethylbenzaldehyde used in the following examples were purchased from Shanghai MacLean Biochemical Technology Co., Ltd., a methanol solution of trimethylamine (3.2 M) was purchased from Beijing Bailingwei Technology Co., Ltd., and ethylene-vinyl alcohol copolymer was purchased from Kuraray Co., Ltd., with a brand name of F171B (vinyl alcohol content of 68%).

[0073] The specific test methods for the test items of the following embodiments and comparative examples are as follows:

[0074] (1) Ion exchange capacity:

[0075] The Mohr titration method was used to test the ion exchange capacity of AEM, and the calculation formula is as follows: c (AgNO3) is the concentration of AgNO3 solution, v (AgNO3) is the volume of AgNO3 solution consumed, m dry(Cl - ) is the dry weight of the AEM.

[0076]

[0077] IEC is the ion exchange capacity.

[0078] (2) Gel degree test:

[0079] The gelation fraction (GF) of AEM was calculated by recording the mass change after AEM was immersed in dimethyl sulfoxide at 80 °C for 24 h. The dry weight before measurement was m before , after soaking, washing and drying, the mass is m after The ratio of the two is the gel degree. The greater the gel degree, the more thorough the cross-linking degree.

[0080]

[0081] GF% is the gel degree.

[0082] (3) Dimensional stability:

[0083] First record the dry film size x dry(OH) , then test the counter ion as OH - The size of AEM after full swelling with water at different temperatures is recorded as x hyd(OH) , the formula for calculating dimensional stability is as follows:

[0084]

[0085] SD is the swelling ratio.

[0086] (4) Water content:

[0087] Take the anion as OH - AEM, wipe the water on its surface with filter paper, and weigh its mass W in the saturated water state hydThe membrane was then placed in a vacuum drying oven at 65°C and fully dried for 12 hours until the mass of the membrane no longer decreased, and then its mass W was measured. dry , the formula for calculating the moisture content is as follows:

[0088]

[0089] (5) Ionic conductivity: The present invention uses the AC impedance method to measure the ionic resistance of the anion exchange membrane. The measurement frequency range is 1 Hz-4 MHz, the potential amplitude is 5 mV, and the measured resistance Nyquist curve is fitted. The intersection of the curve and the real axis Z' is the ionic resistance value of the anion exchange membrane. R .

[0090] The formula for calculating conductivity is as follows:

[0091]

[0092] σ is the ionic conductivity, is the distance between the two electrodes, R is the ionic resistance of the sample being measured, S is the cross-sectional area of ​​the membrane.

[0093] (6) Mechanical strength: The mechanical property test includes the tensile strength and elongation at break of the polymer to be tested. The operating rate of the instrument stretching is 5 mm / min.

[0094] (7) Alkali resistance stability: The stability test conditions of the embodiment are 80°C and immersion in 2 mol / L KOH solution for 2280 hours.

[0095] (8) Fuel cell: The cell operating temperature is 80°C, the gas flow rate of H2 and O2 is 500 sccm, the back pressure is 0.2 MPa, and the cathode and anode both use carbon-supported platinum as catalysts with a catalyst loading of 0.4 mg / cm 2 .

[0096] In order to achieve the above object, the present invention provides a method for preparing an anion exchange membrane for a fuel cell with high ionic conductivity and high alkali resistance stability, the preparation method comprising:

[0097] (1) in the presence of a first organic solvent and a protective gas, polymerizing 4-vinylbenzyl chloride monomer under the initiation of an initiator to obtain poly-4-vinylbenzyl chloride;

[0098] (2) reacting 4-imidazolecarboxaldehyde and p-trifluoromethylbenzaldehyde with the ethylene-vinyl alcohol copolymer in the presence of a second organic solvent and hydrochloric acid to obtain an acetalized ethylene-vinyl alcohol copolymer;

[0099] (3) dissolving the poly 4-vinylbenzyl chloride in a third organic solvent to obtain a poly 4-vinylbenzyl chloride solution; dissolving the acetalized ethylene-vinyl alcohol copolymer in a fourth organic solvent to obtain an acetalized ethylene-vinyl alcohol copolymer solution; mixing the two solutions to obtain a mixed solution; reacting the mixed solution with trimethylamine to obtain a reaction solution; drying the reaction solution to obtain a halogen-type anion exchange membrane; and finally, subjecting the halogen-type anion exchange membrane to ion exchange with an alkaline solution to obtain the anion exchange membrane for a fuel cell with high ionic conductivity and high alkaline resistance stability, wherein the anion is hydroxide.

[0100] The chemical reaction formula corresponding to the preparation method is as follows Figure 5 shown.

[0101] Example 1

[0102] like Figure 1 As shown, this embodiment provides an anion exchange membrane for a fuel cell with high ionic conductivity and high alkali resistance and stability and a preparation method thereof, which specifically includes the following steps:

[0103] (1) Preparation of poly (4-vinylbenzyl chloride): Under nitrogen protection, 6 g of 4-vinylbenzyl chloride was dissolved in 50 mL of tetrahydrofuran. After heating to 60°C, 0.2 g of azobisisobutyronitrile was added and the reaction was continued for 10 hours until the solution became viscous. The product was precipitated in methanol and filtered to obtain a crude product, which was then washed with methanol 4 times and dried in a vacuum drying oven at 40°C to obtain poly (4-vinylbenzyl chloride).

[0104] (2) Preparation of acetalized ethylene-vinyl alcohol copolymer: 2 g of ethylene-vinyl alcohol copolymer was dissolved in 25 mL of dimethyl sulfoxide at 60°C. After the ethylene-vinyl alcohol copolymer was completely dissolved, it was naturally cooled to room temperature, and the pH was adjusted to 3-4 with hydrochloric acid. Then, 1.12 g of 4-imidazolecarboxaldehyde and 1.02 g of p-trifluoromethylbenzaldehyde were added, and stirred at 80°C for 6 h. The pH was adjusted to 7-8 with 1 mol / L sodium hydroxide, and the solution was dripped into deionized water to obtain a white precipitate. The precipitate was broken with a wall breaker and repeatedly washed with deionized water. Finally, it was placed in a vacuum drying oven and dried at 60°C to obtain the acetalized ethylene-vinyl alcohol copolymer.

[0105] (3) Preparation of anion exchange membrane: 0.18 g of poly (4-vinylbenzyl chloride) was dissolved in 5 mL of dimethyl sulfoxide to obtain a poly (4-vinylbenzyl chloride) solution. 0.06 g of acetalized ethylene-vinyl alcohol copolymer was dissolved in 10 mL of dimethyl sulfoxide at 60°C to obtain an acetalized ethylene-vinyl alcohol copolymer solution. The above solutions were mixed evenly at 60°C, stirred for 1 h, cooled to 30°C, 147.5 uL of trimethylamine methanol solution was added to the above mixed solution, reacted for 30 min, and the obtained solution was poured into a 8 cm × 8 cm glass plate and dried in an oven at 80°C to obtain a halogen-type anion exchange membrane. Then it was immersed in a 1 mol / L potassium hydroxide solution at 60°C for 12 hours, during which fresh alkali solution was replaced 3 times. Finally, the residual floating alkali on the membrane surface was rinsed with deionized water until the pH of the aqueous solution was 7, thereby obtaining a hydrogen-bonded cross-linked anion exchange membrane based on a rigid main chain and a flexible main chain with hydroxide as the anion, wherein x was 0.2278, y was 0.3722, and z was 0.4.

[0106] The ion exchange capacity of the anion exchange membrane was measured to be 1.81 mmol / g; the gel degree was 98.6%; the swelling rate at 80℃ was 13.3%, the water content was 89.4%, and the ion conductivity was 125.8 mS / cm; the tensile strength and elongation at break at room temperature were 19.5 MPa and 3.9%, respectively. After being immersed in 2M hot alkali (80℃, KOH) for 2280 h, the retention rates of mass, ion exchange capacity and ion conductivity at 80℃ were 87.3%, 81.3% and 82.9%, respectively.

[0107] Example 2

[0108] The difference between this embodiment and embodiment 1 is that in step (2), the amount of 4-imidazolecarboxaldehyde used is 0.84 g, and the amount of p-trifluoromethylbenzaldehyde used is 1.52 g. Wherein, x is 0.17, y is 0.43, and z is 0.4.

[0109] The ion exchange capacity of the anion exchange membrane was measured to be 1.77 mmol / g; the gel degree was 99.1%; the swelling rate at 80℃ was 15.0%, the water content was 92.0%, and the ion conductivity was 137.8 mS / cm; the tensile strength and elongation at break at room temperature were 20.6 MPa and 6.2%, respectively. After being immersed in 2M hot alkali (80℃, KOH) for 2280 h, the retention rates of mass, ion exchange capacity and ion conductivity at 80℃ were 89.5%, 86.9% and 82.7%, respectively.

[0110] Example 3

[0111] The difference between this embodiment and embodiment 1 is that in step (2), the amount of 4-imidazolecarboxaldehyde used is 0.56 g, and the amount of p-trifluoromethylbenzaldehyde used is 2.03 g. Wherein, x is 0.1122, y is 0.4878, and z is 0.4.

[0112] The ion exchange capacity of the anion exchange membrane was measured to be 1.75 mmol / g; the gel degree was 98.9%; the swelling rate at 80℃ was 12.3%, the water content was 72.7%, and the ion conductivity was 140.8 mS / cm; the tensile strength and elongation at break at room temperature were 23.3 MPa and 5.7%, respectively. After being immersed in 2M hot alkali (80℃, KOH) for 2280 h, the retention rates of mass, ion exchange capacity and ion conductivity at 80℃ were 85.8%, 85.4% and 85.6%, respectively.

[0113] Example 4

[0114] The difference between this embodiment and embodiment 1 is that in step (2), the amount of 4-imidazolecarboxaldehyde used is 0.42 g, and the amount of p-trifluoromethylbenzaldehyde used is 2.28 g. Wherein, x is 0.085, y is 0.515, and z is 0.4.

[0115] The ion exchange capacity of the anion exchange membrane was measured to be 1.75 mmol / g; the gel degree was 98.7%; the swelling rate at 80℃ was 12.3%, the water content was 69.8%, and the ion conductivity was 148.5 mS / cm; the tensile strength and elongation at break at room temperature were 26.6 MPa and 3.8%, respectively. After being immersed in 2M hot alkali (80℃, KOH) for 2280 h, the retention rates of mass, ion exchange capacity and ion conductivity at 80℃ were 89.1%, 87.2% and 87.6%, respectively.

[0116] Example 5

[0117] The difference between this embodiment and embodiment 1 is that in step (2), the amount of 4-imidazolecarboxaldehyde used is 0.34 g, and the amount of p-trifluoromethylbenzaldehyde used is 2.44 g. Wherein, x is 0.068, y is 0.532, and z is 0.4.

[0118] The ion exchange capacity of the anion exchange membrane was measured to be 1.77 mmol / g; the gel degree was 97.8%; the swelling rate at 80℃ was 42.3%, the water content was 275.9%, and the ion conductivity was 135.9 mS / cm; the tensile strength and elongation at break at room temperature were 27.1 MPa and 4.4%, respectively. After being immersed in 2M hot alkali (80℃, KOH) for 2280 h, the retention rates of mass, ion exchange capacity and ion conductivity at 80℃ were 85.1%, 81.5% and 86.9%, respectively.

[0119] Preferably, Example 4 is selected for fuel cell characterization, such as Figure 4 As shown, the maximum discharge power density of hydrogen-oxygen is 895 mW / cm 2 , the maximum current density is 1602 mA / cm 2 ; The maximum discharge power density of hydrogen-air is 692 mW / cm 2 , the maximum current density is 1199 mA / cm 2 ;

[0120] Figure 1 The optical photograph of Example 4 is provided. The film is uniform and transparent, indicating that the anion exchange membrane has good film-forming properties.

[0121] Figure 2 The Fourier transform infrared spectra of Examples 1 to 5 are shown. In all the examples, the imidazole ring can be observed at 1630 and 790 cm -1 The characteristic signal peak at 1067 cm -1 The CF signal peak at 1013 cm -1 The signal peaks of the product COC after aldol condensation; the quaternary ammonium groups can be observed at 1489 and 976 cm -1 CN absorption peak at .

[0122] Figure 3 The small angle X-ray scattering diagrams of Examples 1 to 5 are shown. Obvious scattering peaks can be observed in all the examples, indicating that the examples have a long-range ordered structure of hydrophilic and hydrophobic phase separation. As the F content increases, the scattering angles of Examples 1 to 5 shift to small angles, which are 14.1, 14.0, 13.9, 13.8 and 13.7 nm, respectively. -1 , calculated by the Bragg equation, the corresponding ion cluster distances are 0.445, 0.448, 0.452, 0.455 and 0.458 nm, respectively. This hydrophilic and hydrophobic phase separation structure helps to form a continuous and broad ion channel, thereby promoting ion conduction.

[0123] Comparative Example (ACS Applied Polymer Materials 2024, 6, 5039-5048)

[0124] In order to obtain an anion exchange membrane with excellent comprehensive performance, the authors of the literature used poly(styrene-b-(ethylene-co-butylene)-b-styrene) (SEBS) and poly(terphenylpiperidine) (TPIP) as the main chain, and used N-containing heterocyclic cations to ensure that the prepared anion exchange membrane has high alkali resistance and stability; the methylene bromide grafted on SEBS reacts with the piperidine N on TPIP to produce cross-linking and generate cations, which helps to limit the swelling of the anion exchange membrane and increase the ion content of the membrane material; the fluorine-containing structure on TPIP helps the anion exchange membrane to produce phase separation and promote ion conduction.

[0125] The literature reveals that the anion exchange membrane has an ion exchange capacity of 2.91~3.42 mmol / g; a water content of 76.2~98.4% at 80℃, and a swelling rate of 19.1~25.4%; a tensile strength of 15.2~24.6 MPa at room temperature; an ionic conductivity of no more than 86.76 mS / cm at 80℃; and a loss of 19.1~22.5% after immersion in a 2M NaOH solution at 80℃ for 2200 h. Taking SEBS-C6-MDA-TPIP15% with the best comprehensive performance as an example, its ion exchange capacity is 3.11 mmol / g; a water content of 88.8% at 80℃, and a swelling rate of 23.2%; an ionic conductivity of less than 86.76 mS / cm at 80℃; and a tensile strength of 18.7 MPa at room temperature. After the stability test, the retention rate of ionic conductivity was 79.2%. The maximum discharge power density of hydrogen-oxygen single cell at 80℃ is 221 mW / cm 2 , the maximum discharge current is 460 mA / cm 2 .

[0126] Table 1 shows the results of some test data of the anion exchange membrane (SEBS-C6-MDA-TPIP15%) with the best comprehensive performance in the above Examples 1 to 5 and the comparative example, as follows:

[0127] Table 1

[0128]

[0129] From the performance data in Table 1 above, it can be seen that the anion exchange membrane for a fuel cell with high ionic conductivity and high alkali resistance stability disclosed in Examples 1 to 5 of the present invention has the characteristics of high mechanical strength, high ionic conductivity, high alkali resistance stability, and high fuel cell performance. Compared with the comparative example, the embodiment has a lower ion exchange capacity and higher tensile strength; due to the good ion conduction channel, the embodiment has a higher hydroxide ion conductivity, and thus exhibits better single cell discharge performance.

[0130] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An anion exchange membrane, It is characterized in that The anion exchange membrane has a structure shown in Formula I: Formula I; In formula I, x, y, and z represent the proportion of structural units in the polymer; The value range of x is 0.05~0.25; the value range of y is 0.30~0.60; the value range of z is 0.35~0.

45.

2. The method for preparing the anion exchange membrane according to claim 1, It is characterized in that The preparation method comprises the following steps: S1: Under an inert atmosphere, subjecting a mixture I containing a 4-vinylbenzyl chloride monomer, an initiator, and a first organic solvent to a polymerization reaction to obtain poly-4-vinylbenzyl chloride; S2: reacting a mixture II containing 4-imidazolecarboxaldehyde, p-trifluoromethylbenzaldehyde, ethylene-vinyl alcohol copolymer, a second organic solvent, and hydrochloric acid with I to obtain an acetalized ethylene-vinyl alcohol copolymer; S3: dissolving the poly (4-vinylbenzyl chloride) in a third organic solvent to obtain a poly (4-vinylbenzyl chloride) solution; dissolving the acetalized ethylene-vinyl alcohol copolymer in a fourth organic solvent to obtain an acetalized ethylene-vinyl alcohol copolymer solution; mixing the poly-4-vinylbenzyl chloride solution with the acetalized ethylene-vinyl alcohol copolymer solution to obtain a mixed solution; The mixed solution is reacted with trimethylamine to form a reaction II, and then dried to obtain a halogen-type anion exchange membrane; The halogen-type anion exchange membrane is subjected to ion exchange with an alkaline solution to obtain the anion exchange membrane.

3. The preparation method according to claim 2, It is characterized in that In the step S1, the mass volume ratio of the 4-vinyl benzyl chloride monomer, the initiator, and the first organic solvent is: (4-8 g): (0.15-0.30 g): (35-70 mL).

4. The preparation method according to claim 2, It is characterized in that In the step S1, the first organic solvent is tetrahydrofuran; The initiator is a free radical initiator; The free radical initiator is azobisisobutyronitrile; The inert atmosphere is selected from at least one of nitrogen, argon and helium.

5. The preparation method according to claim 2, It is characterized in that In the step S2, the mass volume ratio of the ethylene-vinyl alcohol copolymer, 4-imidazole carboxaldehyde, p-trifluoromethylbenzaldehyde, and the second organic solvent is: (0.5-6 g): (0.28-3.36 g): (0.255-3.06 g): (10-37.5 mL); The second organic solvent is dimethyl sulfoxide; The hydrochloric acid is added to adjust the pH value of the mixture I to 3-4.

6. The preparation method according to claim 2, It is characterized in that In the step S3, the usage ratio of the poly-4-vinylbenzyl chloride, the third organic solvent, the acetalized ethylene-vinyl alcohol copolymer, the fourth organic solvent, and trimethylamine is: (0.06-0.24 g): (2-8 mL): (0.02-0.08 g): (4-15 mL): (49.2-196.7 μL); The third organic solvent and the fourth organic solvent are both dimethyl sulfoxide; The alkaline solution is selected from KOH solution and / or NaOH solution; The temperature of the alkaline solution is 40-80°C; The concentration of the alkaline solution is 1-2 mol / L.

7. The preparation method according to claim 2, It is characterized in that In the step S1, the polymerization reaction temperature is 30-60° C., and the polymerization reaction time is 8-12 h.

8. The preparation method according to claim 2, It is characterized in that In the step S2, the dissolution temperature of the ethylene-vinyl alcohol copolymer is 50-80° C.; The temperature of the reaction I is 60-100° C., and the time of the reaction I is 5-8 h.

9. The preparation method according to claim 2, It is characterized in that In step S3, the drying temperature is 70-90°C; The ion exchange between the halogen-type anion exchange membrane and the alkaline solution is performed by immersing the halogen-type anion exchange membrane in the alkaline solution; The soaking time is 12 to 24 hours; During the soaking, the fresh alkali solution is replaced 3 to 5 times.

10. Use of the anion exchange membrane according to claim 1 or the anion exchange membrane prepared by the preparation method according to any one of claims 2 to 9 in a fuel cell.

Citation Information

Patent Citations

  • Bipolar membrane and preparation method thereof

    CN112546873A

  • Cross-linked anion exchange membrane as well as preparation method and application thereof

    CN112751067A