A method and device for repairing a metal sheath of a high voltage cable body
Through the pretreatment and spraying steps of high-voltage cable metal sheaths in cold additive process, the problems of thermal scalding and poor performance caused by thermal brazing are solved, and efficient and low-cost in-situ repair is achieved to ensure the performance after repair. The original metal sheath is equivalent.
Patent Information
- Application Number
- CN202411142767.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-20
AI Technical Summary
In the prior art, when repairing high-voltage cable metal sheath, the thermal brazing process leads to thermal scalding of non-metallic materials, and the mechanical and electrical properties are very different from the original metal structure after repair, resulting in economic burden and long construction period.
Using cold additive process, the first, second and third layers of cold additive are pretreated and sprayed, and the metal sheath is repaired at the set temperature to ensure the mechanical and electrical properties and the original metal sheath after repair. quite.
In-situ repair without thermal scalds is achieved. After repair, the combination of strength and tensile strength is high, the density is high, the resistance is not increased, the construction period is short, the cost is low, and the mechanical and electrical properties are comparable to the original metal sheath.
Smart Images

Figure CN118659263B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of cable repair, and in particular, relates to a method and device for repairing a metal sheath of a high-voltage cable body. Background Art
[0002] During the installation and operation of the cable, the metal sheath needs to play the role of waterproof protection, mechanical pressure resistance and electrical performance of the cable. When the layer is damaged due to external factors, the currently available metal sealing process is hot brazing, which requires brazing at a temperature of nearly 300 degrees, which will cause heat burns to the non-metallic materials in contact with the metal sheath. Moreover, after repair, its mechanical and electrical properties are very different from the original metal structure, so in-situ repair is implemented. The usual practice is to replace a small section of cable at the fault location, or even replace an entire section of cable. Such an operation costs hundreds of thousands or even millions of dollars to complete, which will greatly cause economic burdens and prolong the construction period.
[0003] The existing Chinese patent application number: 202111237379.4 discloses a method for removing and repairing the outer sheath when repairing the buffer layer of a high-voltage cable. The method performs a sheath withstand voltage test on the cable to be repaired before repair; prepares the filling solder in advance, removes the outer sheath of the cable, and performs a 45° chamfer on the cut outer sheath and the incision; repairs the buffer layer of the cut outer sheath, and after the repair, the cut outer sheath is docked at the incision, and welded with the filling solder, and finally treated with insulating self-adhesive tape, waterproof tape and PVC tape. It can only be used after passing the sheath withstand voltage test again, but this technology has the disadvantages of complex operation, high cost and long construction period.
[0004] Therefore, there is an urgent need to find a body repair solution that can be implemented at the cable operation and installation site, which can solve the in-situ repair of the metal sheath, complete the waterproof seal, and restore the metal sheath's mechanical resistance to lateral pressure. Summary of the invention
[0005] In order to solve the deficiencies in the prior art, the present invention provides a method and device for repairing cracks in a metal sheath of a high-voltage cable body, so as to overcome the deficiencies in the prior art.
[0006] The present invention adopts the following technical solution.
[0007] The invention discloses a method for repairing a metal sheath of a high-voltage cable body, comprising the following steps:
[0008] S1. Pre-treat defective parts of the metal sheath and the cable;
[0009] S2, spray the first layer of cold additive material on the defective parts pretreated by S1 to pre-seal the metal sheath;
[0010] S3, spraying a second layer of cold additive material on the metal sheath pre-sealed in S2, pre-repairing the metal sheath, and then continuing to spray a third layer of cold additive material to complete the repair of the metal sheath at a set temperature;
[0011] S4. After repairing S3, polish and clean the metal sheath.
[0012] Preferably, in S1, the pretreatment includes grinding the cracked position of the metal sheath and processing the ground cable substrate.
[0013] Preferably, the cracked position of the metal sheath is polished until a conical smooth surface is formed at the opening, the cracked position includes an opening and a crack, the ratio of the opening diameter or lateral dimension to the depth after polishing is greater than 3, and the maximum inclination angle is not greater than 30 degrees, and the ratio of the crack width to depth after polishing is not less than 3.
[0014] Preferably, the processing of the cable substrate includes sandblasting or grinding, the sandblasting speed of the sandblasting is 30-60 m / s; the distance between the nozzle and the defective part is 50-300 mm; the sandblasting flow rate of the sandblasting is 200-600 g / min; the powder particle size of the sandblasting is 20-80 mesh.
[0015] Preferably, in S2, the working pressure for spraying the first layer of cold additive material is 1-3.5 MPa; the gas flow rate is 30-40 m3 / h; the spraying distance is 20-30 mm; and the horizontal moving speed during spraying is 0.1 m / s-0.5 m / s.
[0016] Preferably, in S3, the working pressure for spraying the second layer of cold additive material is 3-4 MPa, the gas flow rate is 40-60 m3 / h, the spraying distance is 20-30 mm, and the horizontal moving speed during spraying is 0.1 m / s-0.4 m / s.
[0017] Preferably, the second layer of spraying material includes: argon atomized pure aluminum powder and atomized pure copper powder, the argon atomized pure aluminum powder has a particle size of 25-70 microns and an average particle size of 45 microns; the atomized pure copper powder has a particle size of 15-70 microns and an average particle size of 45 microns; the mixing ratio is 40-60% by weight of copper powder and the rest is aluminum powder.
[0018] Preferably, in S3, the working pressure for spraying the third layer of cold additive material is 1-3.5 MPa, the gas flow rate is 30-40 m3 / h, the spraying distance is 20-30 mm, and the horizontal moving speed during spraying is 0.1 m / s-0.5 m / s;
[0019] Preferably, in S3, after spraying the third layer of cold additive material, the thickness of the metal sheath at the defective portion is 1.03 to 1.10 times the thickness of the original metal sheath.
[0020] The second aspect of the present invention discloses a repair device for a metal sheath of a high-voltage cable body, which is used to implement the above-mentioned method for repairing a metal sheath of a high-voltage cable body, comprising:
[0021] Pretreatment equipment, used to pretreat defective parts of the metal sheath and cables;
[0022] The spraying equipment is used to spray the defective parts of the metal sheath three times according to the set working pressure, gas flow rate and spraying distance, and is used for pre-sealing, pre-repairing and repairing the defective parts of the metal sheath respectively.
[0023] The beneficial effect of the present invention is that, compared with the prior art,
[0024] (1) The repair method of the present invention adopts a cold additive process. The repair process does not need to be carried out at high temperature, and will not cause thermal burns to the cable and non-metallic materials in contact with the metal sheath. The repaired metal sheath has good bonding strength and tensile strength, high density, and no increase in resistance. Its mechanical and electrical properties are equivalent to those of the original metal sheath.
[0025] (2) The repair method of the present invention can realize in-situ repair of the metal sheath, and the repair period is short, the energy consumption and cost are low, and it has good application prospects in the field of cable metal sheath repair. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The invention is a flow chart of a method for repairing a metal sheath of a high voltage cable body. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. The embodiments described in this application are only part of the embodiments of the present invention, not all of them. Based on the spirit of the present invention, other embodiments obtained by ordinary technicians in this field without creative work are all within the scope of protection of the present invention.
[0028] Considering that the metal sheath needs to bear a certain lateral pressure and waterproof sealing function, the technology currently used to seal the cable metal sheath is generally lead-sealed hot brazing technology. However, considering that this technology requires fire during on-site repair, it will cause safety hazards on site and even on the product. Therefore, the current solution is to replace the entire section or part of the metal sheath to deal with the damaged section.
[0029] However, cracking may involve various forms. The present invention takes into account various aluminum metal additive processing methods that can be used on site, and finally adopts cold additive technology and uses aluminum powder material for spraying to complete the in-situ repair of the high-voltage cable metal sheath. While completing mechanical reinforcement and metal sheath sealing, surface anti-corrosion treatment can also be completed simultaneously.
[0030] At present, high-voltage cables are composed of a conductor core (copper / aluminum), an inner shielding layer (organic material), an insulating layer (organic material), an outer shielding layer (organic material), a metal sheath (aluminum or lead) and an outer sheath (cross-linked polyethylene, rubber and other organic materials) from the inside to the outside. For the repair of the metal sheath in the present invention, since the cable connection repair is carried out from the inside to the outside, the above materials already exist inside the metal sheath when repairing it. Due to the presence of organic materials, the metal sheath must not exceed 110 degrees Celsius during the entire repair process, otherwise the internal organic layer will be thermally damaged or even fail.
[0031] like Figure 1 As shown, the present invention provides a method for repairing a metal sheath of a high-voltage cable body, the repair method comprising the following steps:
[0032] S1. Pre-treat the metal sheath and high-voltage cable;
[0033] In a preferred but non-limiting embodiment of the present invention, S1 specifically comprises:
[0034] S1.1, grind the opening of the metal sheath until a conical smooth surface of ≥45° is formed at the opening, ensuring that there are no obvious debris on the fracture and adjacent areas to facilitate subsequent cold additive processing;
[0035] S1.2, after polishing, the high voltage cable (base material) is subjected to sandblasting or polishing to remove the oxide layer on its surface.
[0036] It is worth noting that for openings, the ratio of the diameter or lateral dimension to the depth after grinding is greater than 3, and the maximum inclination angle is not greater than 30 degrees; for cracks, the ratio of the width and depth after grinding is not less than 3, and the crack terminal must also meet this requirement.
[0037] Furthermore, in S1.2, the blasting speed of the sandblasting treatment is 30 to 60 m / s, preferably 40 to 50 m / s; the distance between the nozzle and the defective part is 50 to 300 mm, preferably 80 to 150 mm; the blasting flow rate of the sandblasting treatment is 200 to 600 g / min, preferably 415 g / min; the powder particle size of the sandblasting treatment is 20 to 80 mesh, preferably 40 to 80 mesh.
[0038] S2, spraying the first layer of cold additive material on the pre-treated defective part to pre-seal the metal sheath;
[0039] In a preferred but non-limiting embodiment of the present invention, in S2, a handheld cold additive device is used to perform cold additive treatment on the defective parts of the metal sheath, and a first layer of cold additive is sprayed to establish a smooth transition matrix on the surface of the metal sheath, while the adjacent area of the protective coating is protected.
[0040] In order to achieve the best coating performance of the material, the working pressure of the first layer of cold additive spraying is 1-3.5MPa, preferably 2-3MPa; the gas flow rate is 30-40m 3 / h, the preferred gas flow rate is 35-38m 3 / h; the spraying distance is 20 to 30 mm, preferably 25 mm, and the spraying distance is the distance between the nozzle and the defective part.
[0041] The horizontal moving speed during spraying is 0.1m / s to 0.5m / s, preferably 0.3m / s. When the area of the defect to be repaired is small, the horizontal moving speed can be appropriately reduced.
[0042] Further preferably, the first layer of spraying material is aluminum alloy powder, and its composition and mass percentage are:
[0043] Copper Cu: 0-0.5%, manganese Mn: 0-1%, magnesium Mg: 0.5-5%, zinc Zn: 0.2-0.5%, chromium Cr: 0.04-0.35%, titanium Ti: 0.1-0.7%, silicon Si: 0.3-0.6%, iron Fe: ≤0.6%, aluminum Al: balance.
[0044] S3, spraying a second layer of cold additive material on the pre-sealed metal sheath to pre-repair the metal sheath, and then continuing to spray a third layer of cold additive material to complete the repair of the metal sheath at a set temperature;
[0045] In a preferred but non-limiting embodiment of the present invention, in S3, the working pressure for spraying the second layer of cold additive material is 1-4 MPa, preferably 2.5-3.5 MPa; the gas flow rate is 30-50 m 3 / h, the preferred gas flow rate is 35-38m 3 / h; the spraying distance is 20 to 30 mm, preferably the spraying distance is 25 mm; the horizontal moving speed during spraying is 0.1 m / s to 0.5 m / s, preferably the horizontal moving speed is 0.3 m / s.
[0046] In order to better realize the repair function of the sheath, the inventors used aluminum-copper composite powder with better performance. The second layer of spraying material is obtained by mixing the following raw materials by mass fraction: 1. Argon gas atomized pure aluminum powder, with a particle size of 25-70 microns and an average particle size of 45 microns; 2. Gas atomized pure copper powder, with a particle size of 15-70 microns and an average particle size of 45 microns. The mixing ratio is: copper powder is 40-60% by weight, and the rest is aluminum powder.
[0047] In a preferred but non-limiting embodiment of the present invention, the working pressure for spraying the third layer of cold additive is 1-3.5 MPa, preferably 2.5-3 MPa; the gas flow rate is 30-40 m 3 / h, the preferred gas flow rate is 35-38m 3 / h; the spraying distance is 20 to 30 mm, preferably the spraying distance is 25 mm; the horizontal moving speed during spraying is 0.1 m / s to 0.5 m / s, preferably the horizontal moving speed is 0.3 m / s.
[0048] Further preferably, the composition and mass percentage of the aerosolized powder of the third layer of spraying material are as follows:
[0049] Copper Cu: 0-0.3%, manganese Mn: 1.0-1.5%, magnesium Mg: 0.2-0.6%, zinc Zn: 0.25%, chromium Cr: 0.1%, titanium Ti: 0.1%, silicon Si: 0.6%, iron Fe: 0.7%, aluminum Al: balance.
[0050] Further preferably, after spraying the third layer of cold additive, the thickness of the metal sheath at the defective part is 1.03 to 1.10 times the thickness of the original metal sheath. If the thickness is insufficient, the local resistance will increase, causing abnormal temperature rise and leading to cable failure.
[0051] It is worth noting that the set temperature means that during any spraying and additive process, if the area of the defect is relatively small, the temperature of the cable substrate must be checked every three minutes. When the temperature exceeds 100 degrees, clean and dry compressed air can be used for cooling, or intermittent spray deposition can be used to prevent burns due to temperature rise.
[0052] The interval spray deposition refers to when there are multiple points to be repaired in the same area, and each point is relatively small, if continuous spraying will cause the temperature to exceed 100 degrees, it will cause thermal burns to the cable. Therefore, spray the points 1, 2, 3, 4, 5, etc. to be repaired in turn. When point 1 is close to 100 degrees, stop the operation and start the operation of point 2, and so on. This can not only ensure the construction temperature, but also improve the operation efficiency.
[0053] S4. After repairing S3, grind and clean the metal sheath.
[0054] In a preferred but non-limiting embodiment of the present invention, in S4, after the addition is completed, there should be no sharp protrusions at the repair position. If there are any, they must be polished to be smooth in time before the subsequent insulation layer repair can be carried out.
[0055] Embodiment 2 of the present invention discloses a device for repairing a metal sheath of a high-voltage cable body, which is used to implement the method for repairing a metal sheath of a high-voltage cable body, comprising:
[0056] Pretreatment equipment, used to pretreat defective parts of the metal sheath and cables;
[0057] The spraying equipment is used to spray the defective parts of the metal sheath three times according to the set working pressure, gas flow rate and spraying distance, and is used for pre-sealing, pre-repairing and repairing the defective parts of the metal sheath respectively. Example
[0058] The present invention is further described below by means of specific examples. These embodiments are only intended to illustrate the present invention but are not intended to limit the scope of the present invention. Example 1
[0059] The defective part (opening position) of the metal sheath is ground until the opening has a smooth transition of a cone of not less than 45° to ensure that there are no obvious debris in the fracture and adjacent areas. After grinding, the defective part is sandblasted with a sandblasting speed of 40m / s, a distance of 100mm between the nozzle and the defective part, a sandblasting flow rate of 415g / min, and a powder particle size of 60 mesh for sandblasting.
[0060] Handheld cold additive equipment is used to perform cold additive treatment on the defective parts of the metal sheath. The first layer of cold additive is sprayed to establish a smooth transition matrix on the surface of the metal sheath. The working pressure of the first layer of cold additive is 2.5MPa, and the gas flow rate is 36m 3 / h, the distance between the nozzle and the defective part during spraying is 25mm, the horizontal moving speed during spraying is 0.3m / s, and the spraying material composition of the first layer of cold additive is: copper Cu: 0.25%, manganese Mn: 0.5%, magnesium Mg: 3%, zinc Zn: 0.4%, chromium Cr: 0.2%, titanium Ti: 0.5%, silicon Si: 0.5%, iron Fe: 0.3%, aluminum Al: balance.
[0061] After spraying the first layer of cold additive, continue to spray the second layer of cold additive. The working pressure of spraying the second layer of cold additive is 3MPa and the gas flow rate is 38m 3 / h, the distance between the nozzle and the defective part during spraying is 25mm, and the horizontal moving speed during spraying is 0.3m / s.
[0062] The second layer of spraying material is obtained by mixing the following raw materials by mass fraction: 1. Argon gas atomized pure aluminum powder, particle size is 25-70 microns, average particle size is 45 microns. 2. Gas atomized pure copper powder, particle size is 15-70 microns, average particle size is 45 microns. Mixing ratio: copper powder is 40-60% by weight, and the rest is aluminum powder.
[0063] Then the third cold additive was sprayed. The working pressure of the third layer of cold additive was 2.5MPa and the gas flow rate was 36m 3 / h, the distance between the nozzle and the defective part during spraying is 25mm, the horizontal moving speed during spraying is 0.2m / s, and the spraying material composition of the third layer of cold additive is: copper Cu: 0.2%, manganese Mn: 1.25%, magnesium Mg: 0.4%, zinc Zn: 0.25%, chromium Cr: 0.1%, titanium Ti: 0.1%, silicon Si: 0.6%, iron Fe: 0.7%, aluminum Al: balance.
[0064] After spraying the third layer of cold additive, the thickness of the metal sheath at the defective part is 1.05 times the thickness of the original metal sheath. During any spraying process of cold additive, if the area of the defect to be repaired is relatively small, the temperature of the cable substrate needs to be checked every three minutes. When the temperature exceeds 100°C, clean and dry compressed air should be used for cooling, or the method of spraying and depositing at intervals should be used to prevent burns due to temperature rise.
[0065] After the cold additive manufacturing is completed, the repaired part is polished and smoothed, and the repair of the metal sheath is completed.
[0066] The bonding strength of the repaired metal sheath was measured to be 80MPa, the tensile strength was 85MPa, the density was 99.5%, and its resistance was detected to be 9.2μΩ, with no problem of increased resistance. Example 2
[0067] The defective part (opening position) of the metal sheath is ground until the opening is a smooth conical transition of not less than 45° to ensure that there are no obvious debris in the fracture and adjacent areas. After grinding, the defective part is sandblasted with a sandblasting speed of 50m / s, a distance of 80mm between the nozzle and the defective part, a sandblasting flow rate of 450g / min, and a powder particle size of 40 mesh.
[0068] Handheld cold additive equipment is used to perform cold additive treatment on the defective parts of the metal sheath. The first layer of cold additive is sprayed to establish a smooth transition matrix on the surface of the metal sheath. The working pressure of the first layer of cold additive is 3MPa, and the gas flow rate is 38m 3 / h, the distance between the nozzle and the defective part during spraying is 30 mm, the horizontal moving speed during spraying is 0.5m / s, and the aerosolized powder composition of the spraying material of the first layer of cold additive is: copper Cu: 0.5%, manganese Mn: 1%, magnesium Mg: 5%, zinc Zn: 0.5%, chromium Cr: 0.35%, titanium Ti: 0.7%, silicon Si: 0.6%, iron Fe: 0.6%, aluminum Al: balance.
[0069] After spraying the first layer of cold additive, continue to spray the second layer of cold additive. The working pressure of spraying the second layer of cold additive is 2.5MPa and the gas flow rate is 38m 3 / h, the distance between the nozzle and the defective part during spraying is 25mm, and the horizontal moving speed during spraying is 0.3m / s.
[0070] The second layer of spraying material is obtained by mixing the following raw materials by mass fraction: 1. Argon gas atomized pure aluminum powder, particle size is 25-70 microns, average particle size is 45 microns. 2. Gas atomized pure copper powder, particle size is 15-70 microns, average particle size is 45 microns. Mixing ratio: copper powder is 40-60% by weight, and the rest is aluminum powder.
[0071] Then the third cold additive is sprayed. The working pressure of the third layer of cold additive is 3MPa and the gas flow rate is 35m 3 / h, the distance between the nozzle and the defective part during spraying is 20mm, the horizontal moving speed during spraying is 0.2m / s, and the spraying material composition of the third layer of cold additive is: copper Cu: 0.3%, manganese Mn: 1.5%, magnesium Mg: 0.6%, zinc Zn: 0.25%, chromium Cr: 0.1%, titanium Ti: 0.1%, silicon Si: 0.6%, iron Fe: 0.7%, aluminum Al: balance. After spraying the third layer of cold additive, the thickness of the metal sheath at the defective part is 1.07 times the thickness of the original metal sheath. In any process of spraying cold additive, if the area of the defective part to be repaired is relatively small, the temperature of the cable matrix must be detected every three minutes. When the temperature exceeds 100°C, clean and dry compressed air must be used for cooling, or the method of spraying and depositing at intervals must be used to prevent burns caused by temperature rise.
[0072] After the cold additive manufacturing is completed, the repaired part is polished and smoothed, and the repair of the metal sheath is completed.
[0073] The bonding strength of the repaired metal sheath was measured to be 81MPa, the tensile strength was 86MPa, the density was 99.6%, and its resistance was detected to be 8.8μΩ, with no problem of increased resistance. Example 3
[0074] The defective part (opening position) of the metal sheath is ground until the opening is a smooth transition of a cone of not less than 45° to ensure that there are no obvious debris in the fracture and adjacent areas. After grinding, the defective part is sandblasted with a sandblasting speed of 45m / s, a distance of 105mm between the nozzle and the defective part, a sandblasting flow rate of 400g / min, and a powder particle size of 80 mesh.
[0075] Handheld cold additive equipment is used to perform cold additive treatment on the defective parts of the metal sheath. The first layer of cold additive is sprayed to establish a smooth transition matrix on the surface of the metal sheath. The working pressure of the first layer of cold additive is 2MPa, and the gas flow rate is 35m 3 / h, the distance between the nozzle and the defective part during spraying is 20mm, the horizontal moving speed during spraying is 0.2m / s, and the spraying material of the first layer of cold additive is gas atomized alloy powder with the following composition: copper Cu: 0.1%, manganese Mn: 0.1%, magnesium Mg: 0.5%, zinc Zn: 0.2%, chromium Cr: 0.04%, titanium Ti: 0.1%, silicon Si: 0.3%, iron Fe: 0.1%, aluminum Al: balance.
[0076] After spraying the first layer of cold additive, continue to spray the second layer of cold additive. The working pressure of spraying the second layer of cold additive is 3.5MPa and the gas flow rate is 37m 3 / h, the distance between the nozzle and the defective part during spraying is 25mm, and the horizontal moving speed during spraying is 0.5m / s.
[0077] The second layer of spraying material is obtained by mixing the following raw materials by mass fraction: 1. Argon gas atomized pure aluminum powder, particle size is 25-70 microns, average particle size is 45 microns. 2. Gas atomized pure copper powder, particle size is 15-70 microns, average particle size is 45 microns. Mixing ratio: copper powder is 40-60% by weight, and the rest is aluminum powder.
[0078] Then the third cold additive was sprayed. The working pressure of the third layer of cold additive was 2.5MPa and the gas flow rate was 36m 3 / h, the distance between the nozzle and the defective part during spraying is 25mm, the horizontal moving speed during spraying is 0.3m / s, and the spraying material composition of the third layer of cold additive is: copper Cu: 0.01%, manganese Mn: 1.0%, magnesium Mg: 0.2%, zinc Zn: 0.25%, chromium Cr: 0.1%, titanium Ti: 0.1%, silicon Si: 0.6%, iron Fe: 0.7%, aluminum Al: balance. After spraying the third layer of cold additive, the thickness of the metal sheath at the defective part is 1.03 times the thickness of the original metal sheath. In any spraying process of cold additive, if the area of the defective part to be repaired is relatively small, the temperature of the cable matrix must be detected every three minutes. When the temperature exceeds 100°C, clean and dry compressed air must be used for cooling, or the method of spraying and deposition at intervals must be used to prevent burns caused by temperature rise.
[0079] After the cold additive manufacturing is completed, the repaired part is polished and smoothed, and the repair of the metal sheath is completed.
[0080] The bonding strength of the repaired metal sheath was measured to be 80MPa, the tensile strength was 84MPa, the density was 99.3%, and its resistance was detected to be 10μΩ, with no problem of increased resistance.
[0081] The beneficial effect of the present invention is that, compared with the prior art,
[0082] (1) The repair method of the present invention adopts a cold additive process. The repair process does not need to be carried out at high temperature, and will not cause thermal burns to the cable and non-metallic materials in contact with the metal sheath. The repaired metal sheath has good bonding strength and tensile strength, high density, and no increase in resistance. Its mechanical and electrical properties are equivalent to those of the original metal sheath.
[0083] (2) The repair method of the present invention can realize in-situ repair of the metal sheath, and the repair period is short, the energy consumption and cost are low, and it has good application prospects in the field of cable metal sheath repair.
[0084] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents, and any modifications or equivalent replacements that do not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. A method for repairing a metal sheath of a high voltage cable body, characterized in that: The following steps are involved: S1. Pre-treat defective parts of the metal sheath and the cable; S2, spray the first layer of cold additive material on the defective parts pretreated by S1 to pre-seal the metal sheath; The first layer of spraying material is aluminum alloy powder, and its composition and mass percentage are: copper Cu: 0-0.5%, manganese Mn: 0-1%, magnesium Mg: 0.5-5%, zinc Zn: 0.2-0.5%, chromium Cr: 0.04-0.35%, titanium Ti: 0.1-0.7%, silicon Si: 0.3-0.6%, iron Fe: ≤0.6%, aluminum Al: balance; S3, spraying a second layer of cold additive material on the metal sheath pre-sealed in S2, pre-repairing the metal sheath, and then continuing to spray a third layer of cold additive material to complete the repair of the metal sheath at a set temperature, wherein the set temperature is less than 100 degrees Celsius; The second layer of spraying material includes: argon gas atomized pure aluminum powder and gas atomized pure copper powder; The spraying material composition of the third layer of cold additive is: copper Cu: 0.01%, manganese Mn: 1.0%, magnesium Mg: 0.2%, zinc Zn: 0.25%, chromium Cr: 0.1%, titanium Ti: 0.1%, silicon Si: 0.6%, iron Fe: 0.7%, aluminum Al: balance; S4. After repairing S3, polish and clean the metal sheath.
2. The method for repairing the metal sheath of a high-voltage cable body according to claim 1, characterized in that: The pretreatment includes grinding the cracked position of the metal sheath and processing the ground cable substrate.
3. A method for repairing a metal sheath of a high-voltage cable body according to claim 2, characterized in that: The cracked position of the metal sheath is polished until a conical smooth surface is formed at the opening, the cracked position includes an opening and a crack, the ratio of the opening diameter or lateral dimension to the depth after polishing is greater than 3, and the maximum inclination angle is not greater than 30 degrees, and the ratio of the crack width to depth after polishing is not less than 3.
4. A method for repairing a metal sheath of a high-voltage cable body according to claim 2, characterized in that: The cable base is processed by sandblasting or grinding. When sandblasting is performed, the sandblasting speed is 30 to 60 m / s; the distance between the nozzle and the defective part is 50 to 300 mm; the sandblasting flow rate is 200 to 600 g / min; and the powder particle size of the sandblasting is 20 to 80 meshes.
5. A method for repairing a metal sheath of a high voltage cable body according to claim 1, characterized in that: In S2, the working pressure for spraying the first layer of cold additive is 1-3.5MPa; the gas flow rate is 30-40m 3 / h; spraying distance is 20-30mm; horizontal moving speed during spraying is 0.1m / s-0.5m / s.
6. A method for repairing a metal sheath of a high-voltage cable body according to claim 1, characterized in that: In S3, the working pressure for spraying the second layer of cold additive is 3-4 MPa, and the gas flow rate is 40-60m 3 / h, the spraying distance is 20-30mm, and the horizontal moving speed during spraying is 0.1m / s-0.4m / s.
7. A method for repairing a metal sheath of a high voltage cable body according to claim 1, characterized in that: The particle size of the argon atomized pure aluminum powder is 25-70 microns, with an average particle size of 45 microns; the particle size of the gas atomized pure copper powder is 15-70 microns, with an average particle size of 45 microns; the mixing ratio is 40-60% by weight of copper powder and the rest is aluminum powder.
8. A method for repairing a metal sheath of a high voltage cable body according to claim 1, characterized in that: In S3, the working pressure for spraying the third layer of cold additive is 1-3.5MPa, and the gas flow rate is 30-40m 3 / h, the spraying distance is 20-30mm, and the horizontal moving speed during spraying is 0.1m / s-0.5m / s.
9. A method for repairing a metal sheath of a high voltage cable body according to claim 1, characterized in that: In S3, after spraying the third layer of cold additive, the thickness of the metal sheath at the defective part is 1.03 to 1.10 times the thickness of the original metal sheath.
10. A repair device for a high-voltage cable body metal sheath, used for implementing a repair method for a high-voltage cable body metal sheath according to any one of claims 1 to 9, characterized in that: include: Pretreatment equipment, used to pretreat defective parts of the metal sheath and cables; The spraying equipment is used to spray the defective parts of the metal sheath three times according to the set working pressure, gas flow rate and spraying distance, and is used for pre-sealing, pre-repairing and repairing the defective parts of the metal sheath respectively.
Citation Information
Patent Citations
A method for removing and repairing the outer sheath during the repair of the buffer layer of a high-voltage cable.
CN113690808B
Conductive epoxy resin for pipeline repair and pipeline online repair method
CN104140640A
Method for breaking and repairing outer sheath in cooperation with repairing of high-voltage cable buffer layer
CN113690808A