ASA thermal paste composite film and preparation method thereof, film-covered board and preparation method thereof
By using acrylic resin and rutile titanium dioxide in ASA composite film, combined with pentaerythritol stearate, the problem of insufficient performance of ASA composite film when bending is solved, and higher impact and anti-aging properties are achieved. The replacement of spraying technology in the laminated plate improves service life and scope of application.
Patent Information
- Application Number
- CN202411172743.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-26
AI Technical Summary
The existing ASA composite film has a narrow range of application when bending continuously, with poor crease resistance and mechanical properties, making it difficult to replace the board spraying process and film marks are prone to occur during the pressing process.
AS resin is replaced by acrylic resin, and rutile titanium dioxide and pentaerythritol stearate are added to improve the impact and anti-aging properties of the composite film. By adjusting the compatibility and adhesion of the resin and titanium dioxide, the composite film is improved. Mechanical properties and service life, and use weather-resistant, crease-free ASA hot-patted composite film in the laminated plate instead of spraying process.
It significantly improves the impact, compression and anti-aging properties of ASA composite film, expands its scope of application, reduces production costs, and provides a longer service life in outdoor environments, while avoiding equipment when spraying profiles. High requirements and uneven coating problems.
Abstract
Description
Technical Field
[0001] The present invention relates to the field of ASA composite films, and in particular to an ASA thermal bonding composite film and a preparation method thereof, a film-coated plate and a preparation method thereof. Background Art
[0002] The patent application number CN113278117A filed by the applicant on May 25, 2021, and the patent titled ASA resin, ASA fold-free white film and preparation method thereof discloses a method for preparing ASA fold-free white film, which uses the ASA resin prepared by the disclosed process in combination with AS resin and functional additives to prepare ASA fold-free white film. However, it was found during use that the application range of ASA fold-free white film is relatively narrow when it is continuously bent. When the distance between adjacent bends is less than 6 cm, white marks may appear and the overall impact resistance and compression resistance are relatively weak, which limits its use scenarios. Summary of the invention
[0003] The object of the present invention is to provide an ASA thermal bonding composite film and a preparation method thereof, so as to solve the problem that the existing ASA composite film has poor crease resistance and mechanical properties.
[0004] The present invention also aims to provide a film-coated board and a preparation method thereof, which can replace the spraying process of the board and will not cause film marks when pressing after coating.
[0005] The embodiments of the present invention are implemented by the following technical solutions:
[0006] A weather-resistant and crease-free ASA thermal bonding composite film comprises, by weight, 40-60 parts of ASA rubber powder, 20-40 parts of acrylic resin, 5-10 parts of rutile titanium dioxide, and 1-2 parts of pentaerythritol stearate.
[0007] The applicant applied for a patent with publication number CN113278117A on May 25, 2021, and the patent name is ASA resin, ASA non-fold white film and preparation method thereof. The patent discloses a method for preparing ASA non-fold white film, which uses ASA resin prepared by the disclosed process, combined with AS resin and functional additives to prepare ASA non-fold white film. It is well known that during the preparation process of the board, it is often necessary to use a spraying process to form a protective layer on its surface, which not only plays a decorative role, but also plays a protective role, reducing oxidation corrosion and physical damage. After the applicant prepared the ASA non-fold white film, the applicant conceived a solution to apply it to the production process of the board, and to replace the spraying process of the board with a coating to solve the problem that some special-shaped boards are difficult to spray evenly everywhere during the spraying process, and the performance requirements of the spraying equipment are high. The ASA non-fold white film is covered on the board and then pressed. It can replace the spraying process and solve the problem of uneven protective layer on the surface of the board. The applicant found in the application process that although ASA non-folding white film can be applied to most special-shaped plates, it still has certain defects in two usage scenarios. First, when the metal plate material is relatively hard and has a certain thickness, the pressure or impact force required for pressing may exceed the bearing limit of ASA non-folding white film; second, when the plate has multiple bends and the distance between adjacent bends is short during the pressing process, ASA non-folding white film may have creases, making it difficult to replace the spraying process. Therefore, the focus of the present invention is to solve the above two problems.
[0008] The present invention changes the composite film-forming process of ASA resin and AS resin, replaces AS resin with acrylic resin and adds rutile titanium dioxide, titanium dioxide is a polycrystalline compound, mainly including rutile titanium dioxide, anatase titanium dioxide and plate titanium dioxide in nature, wherein the plate titanium dioxide crystal form is unstable, so the other two crystal forms are mainly used in the market. The single crystal of anatase is composed of 4 carbon dioxide molecules, the lattice is relatively large, the combination is relatively loose, the crystal arrangement has directionality, and a sheet structure similar to mica is uniformly formed on the polycrystalline combination, so the lattice stability is poor, the phase contrast is small, and the crystal hardness is small. The single crystal of rutile titanium dioxide is composed of 2 TiO2 molecules, the lattice is relatively small, the combination is tight, and the lattice arrangement has no directionality, but is a divergent spatial arrangement, and the polycrystalline combination is a relatively dense spatial reticular structure, so the density is large in the stability of the lattice, and the hardness is also large. The crystals of rutile titanium dioxide are relatively slender and prismatic, usually rutile crystals, while anatase titanium dioxide is mostly approximately regular octahedrons. When the composite film is subjected to impact force, the grain boundaries under the rutile titanium dioxide crystal form can move under the impact of external force, which has a certain energy consumption effect, and thus the impact resistance of the composite film provided by the present invention is improved. In addition, the titanium dioxide surface has a certain adsorption capacity for oxygen, wherein the oxygen absorption capacity of rutile titanium dioxide is less than that of anatase titanium dioxide. The system after adding rutile titanium dioxide has better rheological properties than the pure resin system, which is convenient for subsequent molding. Since the present invention is to compound rutile titanium dioxide with resin, it is also necessary to consider the aging problem of the resin, reduce the adsorption of oxygen by rutile titanium dioxide, and then the present invention also uses pentaerythritol stearate, which can not only promote the dispersion of rutile titanium dioxide when mixed with the other two resins, but also form a film on the surface of rutile titanium dioxide, block its photoactivated points, reduce the adsorption of oxygen, and then increase the anti-aging performance of the composite film. The crystals of rutile titanium dioxide are dense network structures. After being compounded with the resin in this case, they can also improve the strength of the composite film and increase its pressure-bearing capacity.
[0009] After replacing AS resin with acrylic resin, the selection of a reasonable ratio overcomes the shortcomings of a single resin. The plasticity and service life of the ASA composite film are increased. At the same time, compared with the composite of ASA resin and titanium dioxide alone, the possibility of silver streaks during composite molding can be reduced after adding acrylic resin.
[0010] The acrylic resin may be acrylic resin, acrylate resin or epoxy acrylate resin, preferably acrylate resin.
[0011] Preferably, the composite film further comprises, by weight, 0.4-0.6 parts of antioxidant, 0.2-0.5 parts of ultraviolet absorber and 0.2-0.5 parts of light stabilizer.
[0012] The aging resistance and service life of the composite film can be further improved by adding various additives. According to actual needs, 3-5 parts of pigments can be added to the composite film to increase the appearance and reduce light absorption. The antioxidant can be one or more of BHT, TBP and TBHQ, the ultraviolet absorber can be one or more of UV-P, UV-328, and BP-12, and the light stabilizer can be UV-770 light stabilizer.
[0013] Preferably, the preparation method of the ASA rubber powder comprises:
[0014] S100, in parts by weight, 100-300 parts of deionized water, 5-30 parts of acrylate, 0.1-5 parts of comonomer, 0.5-5 parts of OP-10, 0.1-1 parts of sodium bicarbonate, 0.01-0.1 parts of hydrogen peroxide-ferrous salt; then replaced with inert gas three times, stirred and heated to 65-80°C, reacted for 0.5-2 hours, and kept warm for 0.5-2 hours, the comonomer is a blend of ethylene glycol diacrylate and diallyl maleate in a mass ratio of 1:1;
[0015] S200, adding a mixed solution consisting of 40-50 parts by weight of butyl acrylate and 0.1-10 parts by weight of a comonomer and 0.02-0.2 parts by weight of hydrogen peroxide-ferrous salt to the reaction system within 1-5 hours, and keeping the mixture at 70-80° C. for 0.5-2 hours after the addition, wherein the comonomer is a blend of ethylene glycol diacrylate and diallyl maleate in a mass ratio of 1:1;
[0016] S300, then add 30-50 parts by weight of methyl methacrylate and 0.01-0.2 parts by weight of hydrogen peroxide-ferrous salt to the reaction system within 1-3 hours, and control the reaction temperature at 70-80°C. After the addition, add 0.1-1 parts of EDTA at 75-80°C, and keep warm for 0.5-2 hours. Finally, filter, salt out, wash and dry the obtained emulsion to obtain ASA rubber powder.
[0017] The specific preparation process of ASA rubber powder has been disclosed in the patent with publication number CN113278117A, and the patent name is ASA resin, ASA non-folding white film and preparation method thereof. Since rutile titanium dioxide needs to be added to the composite film of the present invention, it is necessary to consider the precipitation of titanium dioxide during the long-term use of the composite film, especially when the present invention needs to use titanium dioxide to increase the impact resistance and pressure resistance of the composite film, when the addition amount of titanium dioxide is high, titanium dioxide is more likely to precipitate. Therefore, the inventor selected a specific technical solution that is more compatible with rutile titanium dioxide in the technical solution under the aforementioned patent, increasing the compatibility of titanium dioxide with ASA rubber powder and acrylic resin, and reducing the precipitation of titanium dioxide. Although the titanium dioxide precipitation problem under this technical solution has been improved, the iron ions remaining in the resin during the reaction of hydrogen peroxide-ferrous salt will promote the aging of the composite film, seriously affecting the service life of the composite film, and will also cause color changes, heat resistance and transparency reduction and other problems, aging will also increase the possibility of titanium dioxide precipitation, so solving the aging problem can further reduce the precipitation of titanium dioxide, thus the present invention improves the ASA rubber powder preparation process, adding a small amount of EDTA, EDTA can not only form a stable complex with iron ions, reduce the oxidizability of iron ions, but also participate in the grafting reaction of the system, improve the adhesion of ASA primary rubber powder and rutile titanium dioxide when blended, and improve the compatibility of rutile titanium dioxide and resin. Having good bonding between the two phases can make stress effectively transferred between the phases when it occurs, thereby consuming more energy, so the impact resistance and compression resistance of the ASA thermal paste composite film can also be effectively improved.
[0018] A method for preparing the weather-resistant and crease-free ASA thermal adhesive composite film comprises:
[0019] D100, add the raw materials into a high-speed mixer according to the proportion, and stir at a stirring speed of 800-1300r / min for 15-30min to form a mixture;
[0020] D200, after adding the mixed material into the twin-screw extruder, a cylindrical composite material is formed, and the heating temperature of the twin-screw extruder is 140-220°C;
[0021] D300, after sending the cylindrical composite material to the calender, it is calendered into sheets at 160-200°C, and then rolled up to obtain the ASA thermal bonding composite film.
[0022] The basic condition for powder mixing is that the particles move with each other under the action of external force. Obviously, the interaction force between particles has an important influence on the interaction between particles. Many material factors that affect mixing, such as particle size and surface morphology, will affect the mixing process by affecting the adhesion between particles. For the directional mixing process, the regulation of the interaction force between powders is the key influencing factor of the mixing process. When powders are mixed, the adhesion between particles will affect the final mixing effect. During the mixing process, the interaction between particles of powders with adhesion is stronger, and the particles in motion are more likely to drive the surrounding particles to move relative to each other. Under the action of suitable hybrid power, generally for powders with medium adhesion, under the action of suitable hybrid power, the mixing efficiency will be greatly improved. Therefore, another purpose of the present invention to select pentaerythritol stearate is to improve the adhesion between ions and improve the mixing efficiency.
[0023] ASA rubber powder becomes molten after being heated in a twin-screw extruder, while titanium dioxide is in a solid state. In order to stably suspend titanium dioxide in the molten ASA rubber powder, the comonomer selected in the ASA preparation process of the present invention is a blend of ethylene glycol diacrylate and diallyl maleate in a mass ratio of 1:1, so that the molten ASA rubber powder has a suitable viscosity. With a reasonable melting temperature and the dispersing effect of pentaerythritol stearate, titanium dioxide can be stably suspended, thereby increasing the uniformity of titanium dioxide in the cylindrical composite material.
[0024] A film-coated board comprises: a board, a PET / PE composite film and the weather-resistant and crease-free ASA thermal adhesive composite film; the inner surface of the board is coated with the PET / PE composite film; the outer surface of the board is coated with the weather-resistant and crease-free ASA thermal adhesive composite film.
[0025] Although PET / PE composite film has excellent anti-crease ability and is cheap, its weather resistance, chemical resistance and mechanical properties are average. It is often used indoors and has a short service life in outdoor environments. The price of PVDF film with good weather resistance is very high. Therefore, the applicant conceived a solution to use the ASA thermal bonding composite film provided by the present invention in combination with PET / PE, so that the board can not only be used outdoors for a long time, but also have a low manufacturing cost. The inner layer of the board is coated with PET / PE composite film, and the outer layer is made of ASA thermal bonding composite film with good weather resistance. Since the inner layer of the board will not be exposed to wind, frost, rain, snow and other environments that reduce the service life of the composite film during use, the inner layer can be made of PET / PE composite film, which can reduce its manufacturing cost while ensuring the quality of the film-coated board.
[0026] A method for preparing a film-coated board, when the board is a metal board, a weather-resistant and crease-free ASA thermal bonding composite film and an adhesive film are hot-pressed to obtain an outer film, a PET / PE composite film and an adhesive film are hot-pressed to obtain an inner film, the metal board is heated to a board temperature of 180-210° C., and then pressed in the order of a lower layer as the inner film, a middle layer as the metal board, and an upper layer as the outer film, and the film-coated board is obtained after cooling;
[0027] When the board is a wood board or bamboo board, one side of the weather-resistant and crease-free ASA thermal bonding composite film is heated and melted at 150-170°C, and then covered with the board and pressed. Then, the opposite side of the weather-resistant and crease-free ASA thermal bonding composite film is coated with glue and the PET / PE composite film is pasted on the board to finally obtain a laminated board.
[0028] The surface temperature of the metal plate is greater than 150°C during pressing. Since the stability of direct hot pressing bonding between the ASA composite film provided by the present invention and the metal plate is not good, when the plate is a metal plate, the ASA composite film is bonded with an adhesive film, and the adhesive film can be a polyurethane adhesive film. During the profiling process of the metal-coated board, the metal-coated board made with the ASA film will not have creases during the profiling process, replacing the spraying process, solving the problems of poor spraying uniformity and high equipment requirements when spraying special-shaped materials, and it also has a high service life when used in outdoor environments, and the production cost is also greatly reduced. However, when the plate is a wooden board or a bamboo board, the ASA hot-stick composite film provided by the present invention has good bonding properties, and the adhesive film is no longer needed. The acid-bonded group in the ASA membrane structure provided in this case constitutes an active group, which can form a covalent bond with the hydroxyl group on the cellulose to play a fixing role, and the long carbon chain olefin group can have a conical hole covering the surface of the cellulose. In order to reduce the operating accuracy of ASA thermal bonding composite film during hot melting, the film thickness can be appropriately increased. During hot melting, a heating plate with the same specifications as the film can be selected. The heating plate is movable and can be heated when it abuts against the film.
[0029] Preferably, the distance between adjacent bends on the weather-resistant and crease-free ASA thermal bonding composite film is greater than or equal to 2.5 cm.
[0030] The patent with publication number CN113278117A and patent name "A kind of ASA resin, ASA non-fold white film and preparation method thereof" provides an ASA non-fold white film. When the ASA non-fold white film is pressed on the metal plate, if the distance between adjacent bends is less than 6cm, white horizontal lines may appear. After the present invention improves its components and preparation method, the distance is significantly reduced, which can greatly improve the application range of the ASA thermal bonding composite film.
[0031] The present invention has at least the following beneficial effects:
[0032] The present invention replaces the resin in the existing ASA composite film with an acrylic resin and adds rutile titanium dioxide, which can greatly improve its mechanical properties and can be used in scenarios where the impact force is large during pressing due to the material and thickness of the plate; the use of pentaerythritol stearate can not only improve the dispersibility of titanium dioxide when mixed with the resin, but also form a coating on the surface of titanium dioxide, thereby improving the anti-aging performance of the ASA composite film; after the preparation method of the ASA composite film is improved, the compatibility of titanium dioxide and the resin matrix can be increased, and the precipitation of titanium dioxide can be reduced after the composite film is used for a long time, but the residual iron ions in the resin after the improvement will accelerate the aging of the resin, The aforementioned problem is solved by adding EDTA. After EDTA participates in the grafting reaction, the adhesion of ASA primary glue powder when blended with rutile titanium dioxide and acrylic resin can be improved, the compatibility of rutile titanium dioxide and resin can be improved, and the mechanical properties of the composite film can be improved. The film-coated board provided by the present invention replaces the board spraying process with the weather-resistant and crease-free ASA thermal bonding composite film, thereby avoiding the problem of high equipment requirements or uneven product coating caused by the difficulty of spraying special-shaped profiles. When the weather-resistant and crease-free ASA thermal bonding composite film provided by the present invention is composited with a wooden board or a bamboo board, the use of glue can be reduced, the cost is low, and the environmental protection performance is better. DETAILED DESCRIPTION
[0033] In order to make the purpose, method scheme and advantages of the embodiments of the present invention clearer, the method scheme in the embodiments of the present invention is clearly and completely described. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0034] Embodiment 1: A method for preparing a weather-resistant, crease-free ASA thermal adhesive composite film, comprising:
[0035] D100, by weight, add 40 parts of ASA rubber powder, 20 parts of acrylic resin, 5 parts of rutile titanium dioxide, 1 part of pentaerythritol stearate, 0.4 parts of TBP, 0.2 parts of UV-P and 0.2 parts of UV-770 into a high-speed mixer, and stir at a stirring speed of 800 r / min for 15 minutes to form a mixture;
[0036] The preparation method of the ASA rubber powder comprises:
[0037] S100, in parts by weight, 100 parts of deionized water, 5 parts of acrylate, 0.1 parts of comonomer, 0.5 parts of OP-10, 0.1 parts of sodium bicarbonate, 0.01 parts of hydrogen peroxide-ferrous salt; then replaced with inert gas three times, stirred and heated to 65°C, reacted for 0.5 hours, and kept warm for 0.5 hours, the comonomer is a blend of ethylene glycol diacrylate and diallyl maleate in a mass ratio of 1:1;
[0038] S200, adding a mixed solution consisting of 40 parts of butyl acrylate and 0.1 parts of a comonomer and 0.02 parts of hydrogen peroxide-ferrous salt to the reaction system within 1 hour, and keeping the mixture at 70° C. for 0.5 hours after the addition, wherein the comonomer is a blend of ethylene glycol diacrylate and diallyl maleate in a mass ratio of 1:1;
[0039] S300, then add 30 parts of methyl methacrylate and 0.01 parts of hydrogen peroxide-ferrous salt to the reaction system within 1 hour, and control the reaction temperature at 70°C. After the addition, add 0.1 parts of EDTA at 75°C, and keep warm for 0.5 hours. Finally, filter, salt out, wash and dry the obtained emulsion to obtain ASA rubber powder.
[0040] D200, after adding the mixed material into the twin-screw extruder, a cylindrical composite material is formed, and the heating temperature of the twin-screw extruder is 140°C;
[0041] D300, after sending the cylindrical composite material to the calender, it is calendered into sheets at 160°C, and then rolled up to obtain the ASA thermal bonding composite film.
[0042] Embodiment 2: A method for preparing a weather-resistant, crease-free ASA thermal adhesive composite film, comprising:
[0043] D100, by weight, add 60 parts of ASA rubber powder, 40 parts of acrylic resin, 10 parts of rutile titanium dioxide, 2 parts of pentaerythritol stearate, 0.6 parts of TBP, 0.5 parts of UV-P and 0.5 parts of UV-770 into a high-speed mixer, and stir at a stirring speed of 1300 r / min for 30 minutes to form a mixture;
[0044] The preparation method of the ASA rubber powder comprises:
[0045] S100, in parts by weight, 300 parts of deionized water, 30 parts of acrylate, 5 parts of comonomer, 5 parts of OP-10, 1 part of sodium bicarbonate, 0.1 part of hydrogen peroxide-ferrous salt; then replaced with inert gas three times, stirred and heated to 80°C, reacted for 2 hours, and kept warm for 2 hours, wherein the comonomer is a blend of ethylene glycol diacrylate and diallyl maleate in a mass ratio of 1:1;
[0046] S200, adding a mixed solution consisting of 50 parts of butyl acrylate and 10 parts of a comonomer and 0.2 parts of hydrogen peroxide-ferrous salt to the reaction system within 5 hours, and keeping the mixture at 80° C. for 2 hours after the addition is complete, wherein the comonomer is a blend of ethylene glycol diacrylate and diallyl maleate in a mass ratio of 1:1;
[0047] S300, then add 50 parts of methyl methacrylate and 0.2 parts of hydrogen peroxide-ferrous salt to the reaction system within 3 hours, and control the reaction temperature at 80°C. After the addition, add 1 part of EDTA at 80°C, and keep warm for 2 hours. Finally, filter, salt out, wash and dry the obtained emulsion to obtain ASA rubber powder.
[0048] D200, after adding the mixed material into the twin-screw extruder, a cylindrical composite material is formed, and the heating temperature of the twin-screw extruder is 220°C;
[0049] D300, after sending the cylindrical composite material to the calender, it is calendered into sheets at 200°C, and then rolled up to obtain the ASA thermal bonding composite film.
[0050] Embodiment 3: A method for preparing a weather-resistant, crease-free ASA thermal adhesive composite film, comprising:
[0051] D100, by weight, add 50 parts of ASA rubber powder, 25 parts of acrylic resin, 8 parts of rutile titanium dioxide, 1.5 parts of pentaerythritol stearate, 0.5 parts of TBP, 0.3 parts of UV-P and 0.4 parts of UV-770 into a high-speed mixer, and stir at a stirring speed of 1100 r / min for 25 minutes to form a mixture;
[0052] The preparation method of the ASA rubber powder comprises:
[0053] S100, in parts by weight, 150 parts of deionized water, 17 parts of acrylate, 3.4 parts of comonomer, 2.7 parts of OP-10, 0.6 parts of sodium bicarbonate, 0.06 parts of hydrogen peroxide-ferrous salt; then replaced with inert gas three times, stirred and heated to 70°C, reacted for 1.5 hours, and kept warm for 1 hour, the comonomer is a blend of ethylene glycol diacrylate and diallyl maleate in a mass ratio of 1:1;
[0054] S200, adding a mixture of 45 parts of butyl acrylate and 5.6 parts of a comonomer and 0.16 parts of hydrogen peroxide-ferrous salt to the reaction system within 3 hours, and keeping the mixture at 75° C. for 1.5 hours after the addition, wherein the comonomer is a blend of ethylene glycol diacrylate and diallyl maleate in a mass ratio of 1:1;
[0055] S300, then add 40 parts of methyl methacrylate and 0.13 parts of hydrogen peroxide-ferrous salt to the reaction system within 1-3 hours, and control the reaction temperature at 75°C. After the addition, add 0.6 parts of EDTA at 77°C, and keep warm for another hour. Finally, filter, salt out, wash and dry the obtained emulsion to obtain ASA rubber powder.
[0056] D200, after adding the mixed material into the twin-screw extruder, a cylindrical composite material is formed, and the heating temperature of the twin-screw extruder is 200°C;
[0057] D300, after sending the cylindrical composite material to the calender, it is calendered into sheets at 180°C, and then rolled up to obtain the ASA thermal bonding composite film.
[0058] Comparative Example 1: This comparative example provides a preparation method in which the components do not contain pentaerythritol stearate.
[0059] A method for preparing a weather-resistant, crease-free ASA thermal adhesive composite film, comprising:
[0060] D100, by weight, add 50 parts of ASA rubber powder, 25 parts of acrylic resin, 8 parts of rutile titanium dioxide, 0.5 parts of TBP, 0.3 parts of UV-P and 0.4 parts of UV-770 into a high-speed mixer, and stir at a stirring speed of 1100 r / min for 25 minutes to form a mixture;
[0061] The preparation method of the ASA rubber powder comprises:
[0062] S100, in parts by weight, 150 parts of deionized water, 17 parts of acrylate, 3.4 parts of comonomer, 2.7 parts of OP-10, 0.6 parts of sodium bicarbonate, 0.06 parts of hydrogen peroxide-ferrous salt; then replaced with inert gas three times, stirred and heated to 70°C, reacted for 1.5 hours, and kept warm for 1 hour, the comonomer is a blend of ethylene glycol diacrylate and diallyl maleate in a mass ratio of 1:1;
[0063] S200, adding a mixture of 45 parts of butyl acrylate and 5.6 parts of a comonomer and 0.16 parts of hydrogen peroxide-ferrous salt to the reaction system within 3 hours, and keeping the mixture at 75° C. for 1.5 hours after the addition, wherein the comonomer is a blend of ethylene glycol diacrylate and diallyl maleate in a mass ratio of 1:1;
[0064] S300, then add 40 parts of methyl methacrylate and 0.13 parts of hydrogen peroxide-ferrous salt to the reaction system within 1-3 hours, and control the reaction temperature at 75°C. After the addition, add 0.6 parts of EDTA at 77°C, and keep warm for another hour. Finally, filter, salt out, wash and dry the obtained emulsion to obtain ASA rubber powder.
[0065] D200, after adding the mixed material into the twin-screw extruder, a cylindrical composite material is formed, and the heating temperature of the twin-screw extruder is 200°C;
[0066] D300, after sending the cylindrical composite material to the calender, it is calendered into sheets at 180°C, and then rolled up to obtain the ASA thermal bonding composite film.
[0067] Comparative Example 2: In this comparative example, ASA rubber powder was prepared according to the patent with publication number CN113278117A and patent name of ASA resin, ASA non-folding white film and preparation method thereof.
[0068] A method for preparing a weather-resistant, crease-free ASA thermal adhesive composite film, comprising:
[0069] D100, by weight, add 50 parts of ASA rubber powder, 25 parts of acrylic resin, 8 parts of rutile titanium dioxide, 1.5 parts of pentaerythritol stearate, 0.5 parts of TBP, 0.3 parts of UV-P and 0.4 parts of UV-770 into a high-speed mixer, and stir at a stirring speed of 1100 r / min for 25 minutes to form a mixture;
[0070] The preparation method of the ASA rubber powder comprises:
[0071] S100, in parts by weight, 150 parts of deionized water, 17 parts of acrylate, 3.4 parts of comonomer, 2.7 parts of OP-10, 0.6 parts of sodium bicarbonate, 0.06 parts of potassium persulfate; then replaced with inert gas three times, stirred and heated to 70°C, reacted for 1.5 hours, and kept warm for 1 hour, the comonomer is a blend of ethylene glycol diacrylate and allyl methacrylate in a mass ratio of 1:1;
[0072] S200, adding a mixture of 45 parts of butyl acrylate and 5.6 parts of a comonomer and 0.16 parts of potassium persulfate to the reaction system within 3 hours, and keeping the mixture at 75° C. for 1.5 hours after the addition, wherein the comonomer is a blend of ethylene glycol diacrylate and allyl methacrylate in a mass ratio of 1:1;
[0073] S300, then add 40 parts of methyl methacrylate and 0.13 parts of potassium persulfate to the reaction system within 1-3 hours, and control the reaction temperature at 75°C. After the addition, add 0.6 parts of EDTA at 77°C, and keep warm for another hour. Finally, filter, salt out, wash and dry the obtained emulsion to obtain ASA rubber powder.
[0074] D200, after adding the mixed material into the twin-screw extruder, a cylindrical composite material is formed, and the heating temperature of the twin-screw extruder is 200°C;
[0075] D300, after sending the cylindrical composite material to the calender, it is calendered into sheets at 180°C, and then rolled up to obtain the ASA thermal bonding composite film.
[0076] Comparative Example 3: In this comparative example, the electrolyte used in the preparation of ASA was replaced with potassium persulfate.
[0077] A method for preparing a weather-resistant, crease-free ASA thermal adhesive composite film, comprising:
[0078] D100, by weight, add 50 parts of ASA rubber powder, 25 parts of acrylic resin, 8 parts of rutile titanium dioxide, 1.5 parts of pentaerythritol stearate, 0.5 parts of TBP, 0.3 parts of UV-P and 0.4 parts of UV-770 into a high-speed mixer, and stir at a stirring speed of 1100 r / min for 25 minutes to form a mixture;
[0079] The preparation method of the ASA rubber powder comprises:
[0080] S100, in parts by weight, 150 parts of deionized water, 17 parts of acrylate, 3.4 parts of comonomer, 2.7 parts of OP-10, 0.6 parts of sodium bicarbonate, 0.06 parts of potassium persulfate; then replaced with inert gas three times, stirred and heated to 70°C, reacted for 1.5 hours, and kept warm for 1 hour, the comonomer is a blend of ethylene glycol diacrylate and diallyl maleate in a mass ratio of 1:1;
[0081] S200, adding a mixed solution consisting of 45 parts of butyl acrylate and 5.6 parts of a comonomer and 0.16 parts of potassium persulfate to the reaction system within 3 hours, and keeping the mixture at 75° C. for 1.5 hours after the addition, wherein the comonomer is a blend of ethylene glycol diacrylate and diallyl maleate in a mass ratio of 1:1;
[0082] S300, then add 40 parts of methyl methacrylate and 0.13 parts of potassium persulfate to the reaction system within 1-3 hours, and control the reaction temperature at 75°C. After the addition, add 0.6 parts of EDTA at 77°C, and keep warm for another hour. Finally, filter, salt out, wash and dry the obtained emulsion to obtain ASA rubber powder.
[0083] D200, after adding the mixed material into the twin-screw extruder, a cylindrical composite material is formed, and the heating temperature of the twin-screw extruder is 200°C;
[0084] D300, after sending the cylindrical composite material to the calender, it is calendered into sheets at 180°C, and then rolled up to obtain the ASA thermal bonding composite film.
[0085] Comparative Example 4: In this comparative example, the comonomer was replaced during the preparation of ASA rubber powder.
[0086] A method for preparing a weather-resistant, crease-free ASA thermal adhesive composite film, comprising:
[0087] D100, by weight, add 50 parts of ASA rubber powder, 25 parts of acrylic resin, 8 parts of rutile titanium dioxide, 1.5 parts of pentaerythritol stearate, 0.5 parts of TBP, 0.3 parts of UV-P and 0.4 parts of UV-770 into a high-speed mixer, and stir at a stirring speed of 1100 r / min for 25 minutes to form a mixture;
[0088] The preparation method of the ASA rubber powder comprises:
[0089] S100, in parts by weight, 150 parts of deionized water, 17 parts of acrylate, 3.4 parts of comonomer, 2.7 parts of OP-10, 0.6 parts of sodium bicarbonate, 0.06 parts of hydrogen peroxide-ferrous salt; then replaced with inert gas three times, stirred and heated to 70°C, reacted for 1.5 hours, and kept warm for 1 hour, the comonomer is a blend of ethylene glycol diacrylate and diallyl maleate in a mass ratio of 1:1;
[0090] S200, adding a mixed solution consisting of 45 parts of butyl acrylate and 5.6 parts of a comonomer and 0.16 parts of hydrogen peroxide-ferrous salt to the reaction system within 3 hours, and keeping the mixture at 75° C. for 1.5 hours after the addition, wherein the comonomer is a blend of ethylene glycol diacrylate and diallyl maleate in a mass ratio of 1:1;
[0091] S300, then add 40 parts of methyl methacrylate and 0.13 parts of hydrogen peroxide-ferrous salt to the reaction system within 1-3 hours, and control the reaction temperature at 75°C. After the addition, add 0.6 parts of EDTA at 77°C, and keep warm for another hour. Finally, filter, salt out, wash and dry the obtained emulsion to obtain ASA rubber powder.
[0092] D200, after adding the mixed material into the twin-screw extruder, a cylindrical composite material is formed, and the heating temperature of the twin-screw extruder is 200°C;
[0093] D300, after sending the cylindrical composite material to the calender, it is calendered into sheets at 180°C, and then rolled up to obtain the ASA thermal bonding composite film.
[0094] Comparative Example 5: In this comparative example, EDTA was not added to S300.
[0095] A method for preparing a weather-resistant, crease-free ASA thermal adhesive composite film, comprising:
[0096] D100, by weight, add 50 parts of ASA rubber powder, 25 parts of acrylic resin, 8 parts of rutile titanium dioxide, 1.5 parts of pentaerythritol stearate, 0.5 parts of TBP, 0.3 parts of UV-P and 0.4 parts of UV-770 into a high-speed mixer, and stir at a stirring speed of 1100 r / min for 25 minutes to form a mixture;
[0097] The preparation method of the ASA rubber powder comprises:
[0098] S100, in parts by weight, 150 parts of deionized water, 17 parts of acrylate, 3.4 parts of comonomer, 2.7 parts of OP-10, 0.6 parts of sodium bicarbonate, 0.06 parts of hydrogen peroxide-ferrous salt; then replaced with inert gas three times, stirred and heated to 70°C, reacted for 1.5 hours, and kept warm for 1 hour, the comonomer is a blend of ethylene glycol diacrylate and diallyl maleate in a mass ratio of 1:1;
[0099] S200, adding a mixture of 45 parts of butyl acrylate and 5.6 parts of a comonomer and 0.16 parts of hydrogen peroxide-ferrous salt to the reaction system within 3 hours, and keeping the mixture at 75° C. for 1.5 hours after the addition, wherein the comonomer is a blend of ethylene glycol diacrylate and diallyl maleate in a mass ratio of 1:1;
[0100] S300, then add 40 parts of methyl methacrylate and 0.13 parts of hydrogen peroxide-ferrous salt to the reaction system within 1-3 hours, control the reaction temperature at 75°C, keep warm at 77°C for 1 hour after the addition, and finally obtain the ASA rubber powder by filtering, salting out, washing and drying the obtained emulsion.
[0101] D200, after adding the mixed material into the twin-screw extruder, a cylindrical composite material is formed, and the heating temperature of the twin-screw extruder is 200°C;
[0102] D300, after sending the cylindrical composite material to the calender, it is calendered into sheets at 180°C, and then rolled up to obtain the ASA thermal bonding composite film.
[0103] Comparative Example 6: This comparative example directly adopts the patent with publication number CN113278117A and patent name of ASA resin, ASA non-folding white film and preparation method thereof to prepare ASA composite film.
[0104] A method for preparing a weather-resistant, crease-free ASA thermal adhesive composite film, comprising:
[0105] The first step is to put 200L of deionized water, 20g of butyl acrylate, 0.5g of ethylene glycol diacrylate, 0.5g of allyl methacrylate, 2g of sodium dodecyl sulfate, 0.5g of sodium bicarbonate, and 0.02g of potassium persulfate into a polymerization kettle equipped with a stirring device and a cooler, and then replace with nitrogen three times, stir and heat up; the reaction temperature is controlled at 75°C, react for 1 hour, and keep warm for 1 hour.
[0106] In the second step, a mixed solution consisting of 40 g of butyl acrylate, 0.8 g of ethylene glycol diacrylate, 0.8 g of allyl methacrylate and 0.05 g of potassium persulfate was added dropwise over 2.5 hours; the reaction temperature was controlled at 75°C and the mixture was kept warm for another hour after the addition was completed.
[0107] In the third step, 40g of methyl methacrylate and 0.04g of potassium persulfate were added dropwise over 1.5 hours; the reaction temperature was controlled at 75°C, and after the addition was completed, the temperature was kept for another hour, and then kept at 80°C for another hour to obtain a latex-like graft copolymer latex with an average particle size of 60nm.
[0108] The obtained emulsion was filtered, and then salted out with a 1% calcium chloride aqueous solution, washed with water, filtered, and dried to obtain a powdery graft copolymer high-rubber powder.
[0109] 60 parts of the graft copolymer high-rubber powder, 30 parts of AS resin, 0.4 parts of antioxidant, 0.4 parts of UV, 0.1 parts of release agent and pigment are mixed, granulated by a twin-screw extruder, and then film-drawn by a film-drawing machine to obtain an ASA film.
[0110] Folding test: A folding test was carried out on the ASA thermal bonding composite film prepared according to the preparation method of Examples 1-3 and Comparative Examples 1-6. The ASA thermal bonding composite film was bent at different locations, with the distance between adjacent bends being 2.5 cm, the number of bends being 4, and the bend angle being 70 degrees. The creases were observed, and the test results are shown in Table 1.
[0111] Table 1
[0112] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Fold White none none none ++ +++ ++ ++ +++ ++++
[0113] The number of + signs represents the severity of the whitening.
[0114] Impact strength test: For each group of experiments, 5 specimens of composite membrane products were made, and the experimental results were averaged. The test method was to test on a simply supported beam double V-notch impact machine in accordance with the provisions of GB / T9341. The test results are shown in Table 2.
[0115] Table 2
[0116] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 <![CDATA[Impact strength / kJ / m 2 > 18.7 16.4 20.1 12.5 10.7 15.3 13.6 15.8 13.4
[0117] Aging resistance test: After the composite film product was aged in hot air at 100°C for 5 days, an impact strength test was performed according to the above impact strength test method and the impact strength retention rate was calculated. The test results are shown in Table 3.
[0118] Table 3
[0119] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Retention rate / % 94.2 87.6 95.1 75.3 80.7 81.5 74.9 67.4 86.7
[0120] From the experimental results of Examples 1 to 3, it can be seen that the weather-resistant, crease-free ASA thermal bonding composite film prepared by the preparation method of the present invention has good anti-whitening performance, impact strength and anti-aging performance when continuously bent.
[0121] From the comparison between Example 3 and Comparative Examples 1-6, it can be seen that the use of pentaerythritol stearate, the type of comonomer and electrolyte in the ASA rubber powder preparation process and the addition of EDTA can effectively improve the anti-whitening performance, impact strength and anti-aging performance of the finished product. At the same time, all the properties are higher than those of the ASA composite film prepared according to the patent with publication number CN113278117A and patent name of ASA resin, ASA non-whitening film and preparation method thereof.
[0122] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A weather-resistant, crease-free ASA thermal adhesive composite film, characterized in that: In parts by weight, it comprises: 40-60 parts of ASA rubber powder, 20-40 parts of acrylic resin, 5-10 parts of rutile titanium dioxide, and 1-2 parts of pentaerythritol stearate; The preparation method of the ASA rubber powder comprises: S100, in a polymerization kettle equipped with a stirring device and a cooler, 100-300 parts of deionized water, 5-30 parts of acrylate, 0.1-5 parts of comonomer, 0.5-5 parts of OP-10, 0.1-1 parts of sodium bicarbonate, and 0.01-0.1 parts of hydrogen peroxide-ferrous salt are added, by weight; then replaced with inert gas three times, stirred and heated to 65-80° C., reacted for 0.5-2 hours, and kept warm for 0.5-2 hours, wherein the comonomer is a blend of ethylene glycol diacrylate and diallyl maleate in a mass ratio of 1:1; S200, adding a mixed solution consisting of 40-50 parts by weight of butyl acrylate and 0.1-10 parts by weight of a comonomer and 0.02-0.2 parts by weight of hydrogen peroxide-ferrous salt to the reaction system within 1-5 hours, and keeping the mixture at 70-80° C. for 0.5-2 hours after the addition, wherein the comonomer is a blend of ethylene glycol diacrylate and diallyl maleate in a mass ratio of 1:1; S300, then add 30-50 parts by weight of methyl methacrylate and 0.01-0.2 parts by weight of hydrogen peroxide-ferrous salt to the reaction system within 1-3 hours, and control the reaction temperature at 70-80°C. After the addition, add 0.1-1 parts of EDTA at 75-80°C, and keep warm for 0.5-2 hours. Finally, filter, salt out, wash and dry the obtained emulsion to obtain ASA rubber powder.
2. The weather-resistant, crease-free ASA thermal adhesive composite film according to claim 1, characterized in that: In parts by weight, the invention also includes 0.4-0.6 parts of antioxidant, 0.2-0.5 parts of ultraviolet absorber and 0.2-0.5 parts of light stabilizer.
3. A method for preparing the weather-resistant, crease-free ASA thermal adhesive composite film according to claim 1 or 2, characterized in that: include: D100, add the raw materials into a high-speed mixer according to the proportion, and stir at a stirring speed of 800-1300r / min for 15-30min to form a mixture; D200, after adding the mixed material into the twin-screw extruder, a cylindrical composite material is formed, and the heating temperature of the twin-screw extruder is 140-220°C; D300, after sending the cylindrical composite material to the calender, it is calendered into sheets at 160-200°C, and then rolled up to obtain the ASA thermal bonding composite film.
4. A film-faced board, characterized in that: include: Plate material, PET / PE composite film and the weather-resistant and crease-free ASA thermal adhesive composite film according to claim 1 or 2; The inner surface of the plate is covered with the PET / PE composite film; the outer surface of the plate is covered with the weather-resistant and crease-free ASA thermal adhesive composite film.
5. A method for preparing the film-faced board according to claim 4, characterized in that: When the plate is a metal plate, the weather-resistant and crease-free ASA thermal bonding composite film and the adhesive film are hot-pressed to obtain an outer film, and the PET / PE composite film and the adhesive film are hot-pressed to obtain an inner film, and the metal plate is heated to a plate temperature of 180-210° C., and then pressed in the order of the lower layer being the inner film, the middle layer being the metal plate, and the upper layer being the outer film, and then cooled to obtain a film-coated plate; When the board is a wood board or bamboo board, one side of the weather-resistant and crease-free ASA thermal bonding composite film is heated and melted at 150-170°C, and then covered with the board and pressed. Then, the opposite side of the weather-resistant and crease-free ASA thermal bonding composite film is coated with glue and the PET / PE composite film is pasted on the board to finally obtain a laminated board.
6. The preparation method according to claim 5, characterized in that: The distance between adjacent bends on the weather-resistant, crease-free ASA thermal bonding composite film is greater than or equal to 2.5 cm.
Citation Information
Patent Citations
ASA resin, ASA fold-free white film and preparation method of ASA fold-free white film
CN113278117A
Preparation method for self-cleaning washing-resistant light-reflecting material
CN110258125A
Polymethyl methacrylate composite material and preparation method thereof
CN111961304A
Process for making poly(alkyl(meth)acrylate) rubber later, poly(meth)acrylate rubber-bassed graft copolymer made therefrom and molding composition containing poly(meth)acrylate rubber-based graft copo
CN1221758A
Methacrylic resin, methacrylic resin composition, and film
JP2017125185A