A kind of degradable coating for heat transfer and preparation method thereof

By surface modification of titanium dioxide and acrylic compounds and mixing them with MMA resin and other materials, white ink with good dispersion properties is prepared, which solves the problem of easy precipitation of titanium dioxide and ensures the continuity and environmental protection of inkjet printing. sex.

CN118667385BActive Publication Date: 2024-11-15SHAANXI DONGFANG SPACEFLIGHT TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411143895.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-15
Estimated Expiration
2044-08-20

AI Technical Summary

Technical Problem

Titanium dioxide in existing white inks is prone to precipitation, resulting in reduced ink viscosity, unstable layering, and difficult to restore the original state, affecting the continuity and quality of inkjet printing.

Method used

By heating and insulating the titanium dioxide with acrylic compound and an organic solvent, a modified titanium dioxide is formed, and mixed with MMA resin, silicone modified acrylic resin emulsion and surfactant, a white ink with good dispersion properties is prepared.

Benefits of technology

Modified titanium dioxide maintains good dispersion performance in white ink, avoids ink agglomeration and precipitation, ensures the continuity and quality of inkjet printing, and the raw materials used are harmless and degradable substances, which have environmentally friendly advantages.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention belongs to the field of printing technology, and relates to a degradable coating for heat transfer and a preparation method thereof. The present invention provides a preparation method for a degradable coating for heat transfer, which comprises: mixing titanium dioxide, acrylic compounds and organic solvents, and obtaining modified titanium dioxide after heating and heat preservation reaction; mixing water and organic solvents, and then adding MMA resin and organosilicon modified acrylic resin emulsion, adding surfactant and the modified titanium dioxide after mixing evenly, and filtering after fully mixing to obtain white ink. The white ink prepared by the present invention has the advantages of being degradable and environmentally friendly, and solves the problems that white ink is prone to agglomeration and precipitation during inkjet printing, resulting in broken holes (broken needles), "ink dripping", "ink flying", "ink breaking", and nozzle clogging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of printing and relates to a degradable coating for heat transfer and a preparation method thereof. Background Art

[0002] Digital heat transfer printing includes sublimation transfer and digital heat transfer. Sublimation transfer uses disperse dyes as coloring pigments to make ink. First, use an inkjet printer to print the image on a special transfer paper, and then heat and pressurize to make the disperse dye sublimate at high temperature, and the image is transferred to the fabric. The difficulties in the development of ink are mainly concentrated in white ink. The first is the problem of whiteness and hiding power; the second is the problem of anti-settling of white ink, because under the low viscosity characteristics, the titanium dioxide of the ink coloring pigment itself is easy to precipitate. Roughly speaking, the higher the titanium dioxide content in the ink, the better the whiteness and hiding effect will be, but the higher the titanium dioxide content, the easier it is to precipitate. The ink is a nano-scale particle. The titanium dioxide in the white ink is ground into nano-scale to make a coating ink with low viscosity (3~5.5mPa·s). After being placed for a long time, precipitation is inevitable. However, the degree of stratification of precipitation, whether stirring after precipitation can restore the original state, and whether the nanoparticles after precipitation aggregate and become large particles again, these three points are extremely important, and the development of white ink must examine and evaluate these issues. Summary of the invention

[0003] The purpose of the present invention is to solve at least one of the above technical problems, focusing on how to prepare a white ink in a simple and low-cost way to solve the problem that titanium dioxide is easy to precipitate and stratify and is difficult to recover. To this end, the present invention provides a degradable coating for hot stamping and a preparation method thereof to solve this need in the art.

[0004] On the one hand, the present invention relates to a method for preparing a degradable coating for heat transfer, which comprises: mixing titanium dioxide, acrylic acid compound and organic solvent, resuspending in anhydrous ethanol after heating and heat preservation reaction, and drying to obtain modified titanium dioxide;

[0005] The water and the organic solvent are mixed, and then the MMA resin and the organosilicon-modified acrylic resin emulsion are added, and after mixing evenly, the surfactant and the modified titanium dioxide are added, and after fully mixing, the white ink is obtained by filtering.

[0006] Furthermore, in the method for preparing the degradable coating for heat transfer provided by the present invention, the acrylic compound is one of acrylic acid, methyl methacrylate and methacrylic acid.

[0007] Furthermore, in the method for preparing the degradable coating for heat transfer provided by the present invention, any of the organic solvents is one of methanol, ethanol and isopropanol.

[0008] Furthermore, in the method for preparing the degradable coating for hot stamping provided by the present invention, the surfactant is dodecyl betaine and / or dodecyl trimethyl ammonium chloride.

[0009] Furthermore, in the preparation method of the degradable coating for hot stamping provided by the present invention, the surfactant is dodecyl betaine and dodecyl trimethyl ammonium chloride, and the mass ratio of dodecyl betaine to dodecyl trimethyl ammonium chloride is 5:3.

[0010] Furthermore, in the method for preparing the degradable coating for heat transfer provided by the present invention, the temperature of the heating and heat preservation reaction is 30-40° C. and the time is 12-24 hours.

[0011] Furthermore, in the method for preparing the degradable coating for hot stamping provided by the present invention, the thermal weight loss of the modified titanium dioxide at 460-500° C. is 2-4%.

[0012] On the other hand, the present invention relates to a degradable coating for hot stamping, which is prepared by the preparation method.

[0013] Furthermore, in the biodegradable coating for hot stamping provided by the present invention, the raw materials for preparing the white ink are, by weight, 40 to 45 parts of MMA resin, 3 to 5 parts of silicone-modified acrylic resin emulsion, 1 to 3 parts of the surfactant, 30 to 35 parts of the modified titanium dioxide, 10 to 15 parts of organic solvent, and 10 to 15 parts of water.

[0014] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects or advantages:

[0015] The present invention obtains modified titanium dioxide by modifying the surface of titanium dioxide so that an acrylic compound forms a complex on the surface of titanium dioxide. The modified titanium dioxide exhibits good dispersibility in the preparation of a degradable coating using MMA resin as a raw material through surface modification, and in particular, maintains good dispersibility after long-term storage. The white ink obtained by the present invention has the advantage of being green and environmentally friendly because it uses MMA resin and the raw materials used are harmless and degradable substances. The modified titanium dioxide used in the white ink obtained by the present invention maintains good dispersibility in the system, thereby solving the problem that the white ink is prone to agglomeration and precipitation during inkjet printing, resulting in broken holes (broken needles), "ink dripping", "ink flying", "ink breaking", and nozzle clogging. DETAILED DESCRIPTION

[0016] The technical scheme of the present invention is described below in conjunction with the examples, but the present invention is not limited to the following examples. The experimental methods and detection methods described in each example are conventional methods unless otherwise specified; the reagents and materials are commercially available unless otherwise specified. The "%" indicates mass percentage unless otherwise specified.

[0017] Raw materials: Titanium dioxide was purchased from Henan Billions Chemical Co., Ltd., model R-896; MMA resin was purchased from Guangzhou Jushun Chemical Co., Ltd.; silicone-modified acrylic resin emulsion was purchased from Anhui Zhongen Chemical Co., Ltd., model SA-108, brand WC-SA108.

[0018] Example 1: This example provides a method for preparing a modified titanium dioxide.

[0019] Acrylic acid (92mL) and a small amount of water (8mL) were stirred and mixed in a container, and then titanium dioxide (5g) was added. The container was kept stirred while the water bath was heated to 35°C. After 12 hours, a milky white liquid was formed. The solid at the bottom of the tube was collected after centrifugation at 3000rpm for 5 minutes. The collected solid was resuspended in 20mL of anhydrous ethanol, and then dried at room temperature to obtain modified titanium dioxide. After thermogravimetric analysis (TGA), the curve at 460~500°C was observed (the thermal weight loss tended to be stable at this time). The thermal weight loss of the unmodified titanium dioxide at 480°C was 0.21%, and the thermal weight loss of the modified titanium dioxide was 2.18%.

[0020] Example 2: This example provides a method for preparing a modified titanium dioxide.

[0021] Methyl methacrylate (92 mL) and a small amount of water (8 mL) were stirred and mixed in a container, and then titanium dioxide (5 g) was added. The container was kept stirred while the water bath was heated to 35 ° C. After 18 hours, a milky white liquid was formed. After centrifugation at 3000 rpm for 5 minutes, the solid at the bottom of the tube was collected. The collected solid was resuspended in 20 mL of anhydrous ethanol, and then dried at room temperature to obtain modified titanium dioxide. After thermogravimetric analysis (TGA), the curve at 460-500 ° C was observed (the thermal weight loss tended to be stable at this time). The thermal weight loss of the unmodified titanium dioxide at 480 ° C was 0.20%, and the thermal weight loss of the modified titanium dioxide was 3.84%.

[0022] Example 3: This example provides a method for preparing a modified titanium dioxide.

[0023] Methyl acrylic acid (92 mL) and a small amount of water (8 mL) were stirred and mixed in a container, and then titanium dioxide (5 g) was added. The container was kept stirred while the water bath was heated to 35 ° C. After 24 hours, a milky white liquid was formed. The solid at the bottom of the tube was collected after centrifugation at 3000 rpm for 5 minutes. The collected solid was resuspended in 20 mL of anhydrous ethanol, and then dried at room temperature to obtain modified titanium dioxide. After thermogravimetric analysis (TGA), the curve at 460-500 ° C was observed (the thermal weight loss tended to be stable at this time). The thermal weight loss of the unmodified titanium dioxide at 480 ° C was 0.22%, and the thermal weight loss of the modified titanium dioxide was 2.68%.

[0024] Example 4: This example provides white inks of different compositions and performance test results thereof.

[0025] The parts in the following formulas are all parts by mass.

[0026] Formula 1: 40 parts of MMA resin, 3 parts of silicone-modified acrylic resin emulsion, 1 part of surfactant, 30 parts of modified titanium dioxide prepared in Example 1, 10 parts of methanol, and 10 parts of water, wherein the surfactant is dodecyl betaine and dodecyl trimethyl ammonium chloride in a mass ratio of 5:3.

[0027] Formula 2: 42 parts of MMA resin, 4 parts of silicone-modified acrylic resin emulsion, 2 parts of surfactant, 32 parts of modified titanium dioxide prepared in Example 2, 12 parts of ethanol, and 12 parts of water, wherein the surfactant is dodecyl betaine and dodecyl trimethyl ammonium chloride in a mass ratio of 5:3.

[0028] Formula 3: 45 parts of MMA resin, 5 parts of silicone-modified acrylic resin emulsion, 3 parts of surfactant, 35 parts of modified titanium dioxide prepared in Example 3, 15 parts of isopropanol, and 15 parts of water, wherein the surfactant is dodecyl betaine and dodecyl trimethyl ammonium chloride in a mass ratio of 5:3.

[0029] Formula 4: 45 parts of MMA resin, 5 parts of silicone-modified acrylic resin emulsion, 3 parts of surfactant, 35 parts of modified titanium dioxide prepared in Example 3, 15 parts of isopropanol, and 15 parts of water, wherein the surfactant is dodecyl betaine.

[0030] Formula 5: 45 parts of MMA resin, 5 parts of silicone-modified acrylic resin emulsion, 3 parts of surfactant, 35 parts of modified titanium dioxide prepared in Example 3, 15 parts of isopropanol, and 15 parts of water, wherein the surfactant is dodecyltrimethylammonium chloride.

[0031] Formula 6: 45 parts of MMA resin, 5 parts of silicone-modified acrylic resin emulsion, 3 parts of surfactant, 35 parts of modified titanium dioxide prepared in Example 3, 15 parts of isopropanol, and 15 parts of water, wherein the surfactant is dodecyl betaine and sodium lignin sulfonate in a mass ratio of 5:3.

[0032] Formula 7: 45 parts of MMA resin, 5 parts of silicone-modified acrylic resin emulsion, 3 parts of surfactant, 35 parts of unmodified modified titanium dioxide in Example 3, 15 parts of isopropanol, and 15 parts of water, wherein the surfactant is dodecyl betaine and dodecyl trimethyl ammonium chloride in a mass ratio of 5:3.

[0033] Preparation steps: according to the amount, water and organic solvent are fully mixed, and then MMA resin is added to heat and dissolve. After cooling to room temperature, the mixture is stirred at 300 rpm for 1 hour, and then silicone-modified acrylic resin emulsion is added, and stirring is continued for 1 hour; surfactants, modified or unmodified titanium dioxide are added while stirring, and finally stirring at 600 rpm for 1 hour; filter with a 1.0 μm filter membrane, and finally add deionized water to adjust the viscosity to 4~5.5 mP·s.

[0034] White ink (samples numbered 1 to 7) was prepared using formulations 1 to 7. After measuring the surface tension, the ink was loaded into oil barrels (diameter 12.3 cm, height 13.2 cm, volume 1 L). After canning, the viscosity at the top (1 cm depth) and bottom (1 cm depth) was measured respectively. After standing for 30 days, the viscosity was measured again after stirring at 300 rpm for 5 minutes. After standing for 180 days, the viscosity was measured again after stirring at 300 rpm for 5 minutes. The measurement results are shown in Table 1.

[0035] Table 1: Performance results of the white ink obtained

[0036]

[0037] Based on the test results in Table 1, in terms of surface tension performance, it can be seen from sample 6 that an inappropriate combination of surfactants will lead to too low surface tension, which may make the elasticity of the heat transfer film transfer ink too low, and then lead to the problem of infinite extension; the white ink prepared by samples 1~5 has moderate surface tension and viscosity, and will not be tight and brittle or infinitely extended. After storage, the ink shows that the upper part of the container is thin, the viscosity is low, and the color and concentration are also relatively poor; the lower part is thicker, the viscosity is high, and the color and concentration are also relatively good. In severe cases, there is even a phenomenon of bottom agglomeration. This is because the binder of this type of ink is a thin and low-viscosity fluid, which is prone to poor dispersion in the pigment system. The purpose of stirring at 300rpm for 5 minutes during the above test process is to fully mix the ink again so that the pigment and the binder are fully and evenly mixed again. After standing for 180 days, the white inks made from samples 1 to 5 still maintain a viscosity within the range, and the viscosity difference between the top and the bottom is small; the white inks made from samples 6 to 7 cannot achieve the purpose after sufficient mixing, so the inks are no longer usable and new inks should be considered. The inks made from samples 1 to 7 (without standing) were placed in the ink cartridge of a four-nozzle white ink heat transfer fully automatic all-in-one machine, and printed continuously for 30 meters, and the state of the nozzles before and after printing was observed; samples 1 to 5 and sample 7 can be seen to have no broken holes after printing for 30 meters, and the nozzles are in good condition, with no broken holes, no slanted spraying, no hollowing, no obvious ink droplets flowing down, no obvious fine lines, and no cracks; sample 6 had 3 broken holes after printing for 30 meters, and slanted spraying occurred.

[0038] As described above, the basic principle, main features and advantages of the present invention are well described. The above embodiments and descriptions are only descriptions of the preferred implementation modes of the present invention, and the present invention is not limited by the above embodiments. Without departing from the spirit and scope of the present invention, various changes and improvements made by ordinary technicians in this field to the technical solution of the present invention should fall within the protection scope determined by the present invention.

Claims

1. A method for preparing a degradable coating for heat transfer, It is characterized in that include: The titanium dioxide, acrylic compound and organic solvent are mixed, heated and kept for reaction, then resuspended in anhydrous ethanol, and dried to obtain modified titanium dioxide; Mix water and an organic solvent, then add MMA resin and organosilicon-modified acrylic resin emulsion, mix well, add surfactant and the modified titanium dioxide, mix well and filter to obtain white ink; The acrylic compound is one of acrylic acid, methyl methacrylate and methacrylic acid; The heating and heat preservation reaction temperature is 30-40°C and the time is 12-24h; In parts by mass, the raw materials for preparing the white ink are 40-45 parts of MMA resin, 3-5 parts of silicone-modified acrylic resin emulsion, 1-3 parts of the surfactant, 30-35 parts of the modified titanium dioxide, 10-15 parts of organic solvent and 10-15 parts of water.

2. The method for preparing the degradable coating for heat transfer according to claim 1, It is characterized in that Any of the organic solvents is one of methanol, ethanol and isopropanol.

3. The method for preparing the degradable coating for heat transfer according to claim 1, It is characterized in that The surfactant is dodecyl betaine and / or dodecyl trimethyl ammonium chloride.

4. The method for preparing the degradable coating for heat transfer according to claim 3, It is characterized in that The surfactant is dodecyl betaine and dodecyl trimethyl ammonium chloride, and the mass ratio of dodecyl betaine to dodecyl trimethyl ammonium chloride is 5:

3.

5. The method for preparing the degradable coating for heat transfer according to claim 1, It is characterized in that The thermal weight loss of the modified titanium dioxide at 460-500° C. is 2-4%.

6. A degradable coating for heat transfer, It is characterized in that The method is prepared by the preparation method according to any one of claims 1 to 5.