A kind of ultraviolet light-cured thermoplastic polyurethane elastomer solvent adhesive and preparation method thereof

By introducing acrylic groups and photoinitiators into the thermoplastic polyurethane elastomer solvent glue, the ultraviolet curable thermoplastic polyurethane elastomer solvent glue is solved, and the problem of insufficient bonding strength and production efficiency in the prior art is achieved, and high viscosity is achieved Connect strength and simplify construction steps.

CN118667502BActive Publication Date: 2024-11-29HUADA CHEM GRP CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411169976.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-29
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

The existing ultraviolet curing adhesives have shortcomings in terms of bonding strength and production efficiency, and the construction steps are cumbersome, which cannot meet the needs of high bonding strength and production efficiency.

Method used

By making homemade polyester diol, acrylic groups are introduced into the molecular chain of thermoplastic polyurethane elastomer solvent glue, combined with a photoinitiator, forming a thermoplastic polyurethane elastomer solvent glue that can be cured by UV, increasing the crosslinking point and induction through UV light Rapid crosslinking to form a network molecular structure and improve bonding strength.

Benefits of technology

High bonding strength and high temperature resistance are achieved, construction steps are simplified, production efficiency is improved, and the bonding strength is further cured after the solvent evaporates.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of thermoplastic polyurethane elastomers, and relates to a UV-cured thermoplastic polyurethane elastomer solvent adhesive and a preparation method, wherein the solvent adhesive comprises the following components in parts by weight: diisocyanate: 20-40 parts, self-made polyester diol: 45-75 parts, chain extender: 4.5-13 parts, photoinitiator: 2-5 parts, auxiliary agent: 0.5-3.0 parts, catalyst: 0.005-0.02 parts. The present invention introduces acrylic acid groups into the molecular chain of thermoplastic polyurethane elastomer solvent adhesive through self-made polyester diol, and matches the photoinitiator to obtain solvent adhesive; after ultraviolet light induction, the macromolecules can be further cross-linked, which greatly improves the bonding strength, and as the solvent evaporates, the properties of the thermoplastic polyurethane elastomer hard segment crystallization make the adhesive further solidify, and the bonding strength is greatly improved; and the production process is simple and the production efficiency is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermoplastic polyurethane elastomers, and in particular relates to an ultraviolet light-cured thermoplastic polyurethane elastomer solvent adhesive and a preparation method thereof. Background Art

[0002] Solvent-based adhesives refer to adhesives containing volatile organic solvents. Thermoplastic polyurethane elastomer solvent adhesives are made by dissolving thermoplastic polyurethane elastomers in solvents to give the adhesive fluidity. After the solvent is completely evaporated, the polyurethane molecular chains crystallize and the adhesive solidifies, thus bonding the adherends together. It has the characteristics of fast dissolution speed, strong crystallinity, high initial bonding strength and final bonding strength, and is mainly used in the fields of fabric coating, shoe glue, hot melt adhesive film, etc.

[0003] Chinese invention patent CN109181619A discloses a UV light-curing adhesive, which is prepared by grafting monohydroxy acrylic monomers such as hydroxyethyl methacrylate into a polyurethane prepolymer to obtain an acrylic modified polyurethane resin with double bonds, and then combining it with an acrylic diluent, a photoinitiator, a filler, etc. to obtain an adhesive that can be rapidly cross-linked under ultraviolet light induction. However, the amount of cross-linkable acrylic monomers introduced is relatively small, and a large number of cross-linking points cannot be formed after ultraviolet light induction, resulting in low bonding strength.

[0004] Chinese invention patent CN107201180A discloses a method for preparing a UV-curable acrylic hot melt pressure-sensitive adhesive, which uses solution polymerization to chemically bond the photoinitiator component to the main chain of the acrylic polymer, then adds a tackifying resin to adjust the initial viscosity, and removes the solvent to obtain the target product. The invention is characterized by adjustable initial viscosity and high bonding strength; however, its production cycle is long and the production process is cumbersome. After the photoinitiator is introduced into the main chain of the polymer, its reaction site is limited after ultraviolet light induction, and it cannot fully induce the polymerization reaction of acrylic acid, and cannot fully crosslink, thereby reducing the bonding strength of the adhesive.

[0005] Therefore, there is a need for a UV-curable thermoplastic polyurethane elastomer solvent adhesive with bonding strength, high production efficiency, and simple and convenient construction steps. Summary of the invention

[0006] In view of the deficiencies of the above-mentioned prior art, the present invention provides a UV-curable thermoplastic polyurethane elastomer solvent adhesive and a preparation method thereof. The specific technical scheme is as follows:

[0007] The first object of the present invention is to provide a UV-curable thermoplastic polyurethane elastomer solvent adhesive, comprising the following components in parts by weight:

[0008] Diisocyanate: 20-40 parts, self-made polyester diol: 45-75 parts, chain extender: 4.5-13 parts, photoinitiator: 2-5 parts, auxiliary agent: 0.5-3.0 parts, catalyst: 0.005-0.02 parts;

[0009] The preparation method of the self-made polyester diol is as follows: under nitrogen protection, a small molecule dibasic acid, a small molecule diol A, a small molecule diol B and a polyester synthesis catalyst are mixed, the temperature is raised to 140-180° C., and the reaction is carried out at a constant temperature for 1-5 hours; then the temperature is further raised to 190-220° C. within 0.5-2 hours, and the vacuum is turned on when the acid value is lower than 5 mgKOH / g, the moisture and the small molecule diol A and the small molecule diol B in the system are removed, and the reaction is continued until the hydroxyl value is 20-200 mg KOH / g and the acid value is 0.15-0.35 mg KOH / g; the molar ratio of the small molecule dibasic acid, the small molecule diol A and the small molecule diol B is 2:(0-1):(1-2), and the small molecule diol B is a small molecule diol containing an acrylic acid group.

[0010] The invention prepares polyester diol with small molecule diol containing acrylic acid group, introduces acrylic acid group into the molecular chain of thermoplastic polyurethane elastomer solvent adhesive, and matches with photoinitiator to obtain ultraviolet light-cured thermoplastic polyurethane elastomer solvent adhesive; multiple crosslinking points are added to the long-chain thermoplastic polyurethane elastomer molecules of solvent adhesive, and the molecules are rapidly crosslinked after ultraviolet light induction to form a network molecular structure, thereby improving the bonding strength; and as the solvent evaporates, the crystallization property of the hard segment of the thermoplastic polyurethane elastomer causes the adhesive to be further cured, thereby greatly improving the bonding strength.

[0011] Furthermore, the molecular weight of the self-made polyester diol is 1000-4000.

[0012] Furthermore, the polyester synthesis catalyst is tetraisopropoxytitanium or tetrabutyl titanate.

[0013] Furthermore, the small molecule dibasic acid is one or two or more of succinic acid (SA), glutaric acid (GA), adipic acid (AA), hexahydrophthalic anhydride (HHPA), 1,4-cyclohexanedicarboxylic acid (1,4-CHDA), azelaic acid (AzA), isophthalic acid (IPA), phthalic acid (PA), and terephthalic acid (PTA).

[0014] Further, the small molecule diol A is one or two or more of ethylene glycol (EG), propylene glycol (PG), butanediol (BG), hexanediol (HDO), diethylene glycol (DEG), 2-methyl-1,3-propanediol (MPO), neopentyl glycol (NPG), 2,2,4-trimethyl-1,3-pentanediol (TMPD), 2-ethyl-2-butyl-1,3-propanediol (BEPG), and 1,4-cyclohexanedimethanol (1,4-CHDM);

[0015] The small molecule diol B is one or both of pentaerythritol diacrylate and trimethylolpropane monoallyl ether.

[0016] Further, the diisocyanate is an aromatic diisocyanate or an aliphatic diisocyanate;

[0017] The aromatic diisocyanate is one or two or more of diphenylmethane diisocyanate (MDI), xylylene diisocyanate (XDI), p-phenylene diisocyanate (PPDI), 1,5-naphthalene diisocyanate (NDI), toluene diisocyanate (TDI), and 1,3-bis(1-isocyanato-2-propyl)benzene (TMXDI);

[0018] The aliphatic diisocyanate is one or two or more of hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), 4,4'-dicyclohexylmethane diisocyanate (HMDI), 1,4-cyclohexane diisocyanate (CHDI), and trimethylhexamethylene diisocyanate (TMDI).

[0019] Furthermore, the chain extender is one or two or more of ethylene glycol (EG), propylene glycol (PG), 1,4-butanediol (BG), 1,6-hexanediol (HDO), 1,4-cyclohexanediol, neopentyl glycol, hydroquinone bis(β-hydroxyethyl) ether (HQEE), hydrogenated bisphenol A, dihydroxyethyl terephthalate (BHET), resorcinol dihydroxyethyl ether (HER), glycerol α-allyl ether, TMP monoallyl ether, 3,3-dichloro-4,4-diaminodiphenylmethane (MOCA), 3,5-diamino-p-chlorobenzoic acid isobutyl ester, diethyltoluenediamine, 3,5-dimethylthiotoluenediamine, 4,4-methylenebis(3-chloro-2,6-diethylaniline), and 1,3-propylene glycol-bis(4-aminobenzoate).

[0020] Furthermore, the photoinitiator is one or two or more of benzophenone, 4-methylbenzophenone, methyl o-benzoylbenzoate, 4-hydroxybenzophenone, 2,4-dihydroxybenzophenone, Michler's ketone, 4-fluoro-4'-hydroxybenzophenone, photoinitiator 819 (BAPO), triphenyl phosphite (TPO), ethyl 2,4,6-trimethylbenzoylphenylphosphonate (TPO-L), 2-dimethylamino-2-benzyl-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, thiopropoxythioxanthone, isopropylthioxanthone, ethyl dimethylaminobenzoate (EDB), triarylsulfonium salts, and isopropylferrocenium hexafluorophosphate (Irgacure 261).

[0021] Furthermore, the auxiliary agent is one or two or more of an antioxidant and a hydrolysis stabilizer; the antioxidant is any one or two or more of 2,6-di-tert-butyl-4-methylphenol (antioxidant 264), pentaerythritol ester (antioxidant 1010), and 3,5-di-tert-butyl-4-hydroxyphenylpropionic acid octadecyl (antioxidant 1076); the hydrolysis stabilizer is any one or two or more of carbodiimide, 4-tert-butylcatechol, and hexamethylenetetramine.

[0022] Furthermore, the catalyst is one or two or more of an amine catalyst, an organic bismuth catalyst, an organic tin catalyst, an organic zinc catalyst, an organic lead catalyst, an organic cobalt catalyst, and an organic mercury catalyst.

[0023] The second object of the present invention is to provide a method for preparing the above-mentioned UV-curable thermoplastic polyurethane elastomer solvent adhesive, comprising the following steps:

[0024] S1: Heat and melt the self-made polyester diol, remove water by vacuum for 1 to 3 hours, add the auxiliary agent, stir evenly, and stir for no less than 3 hours to obtain component A;

[0025] S2: Heat and melt the diisocyanate, then add component A and the catalyst, stir for 5 to 10 minutes, and wait until the viscosity rises to 10,000 to 20,000 mPa·s to obtain a polyurethane prepolymer;

[0026] S3: Add a chain extender to the polyurethane prepolymer obtained in S2 to further extend the chain reaction, stir for 1 to 2 minutes, the melt viscosity further increases, pour into a tray for solidification, and mature at 90 to 95°C for 3 to 5 hours. After maturation, crush the sample into particles;

[0027] S4: The crushed particles in S3 are dried in an oven, fully mixed with a photoinitiator, and then extruded into granules through an extruder.

[0028] When the UV-curable thermoplastic polyurethane elastomer solvent adhesive of the present invention is used, the product is prepared into a solvent adhesive according to the required solid content and the solvent, and is directly coated. After being induced by ultraviolet light, it is rapidly cross-linked, and as the solvent evaporates, the crystallization property of the hard segment of the thermoplastic polyurethane elastomer causes the adhesive to be further cured, and the bonding strength is greatly improved. When used, the solvent that can be used in the UV-curable thermoplastic polyurethane elastomer solvent adhesive of the present invention is any one or two or more of acetone, butanone, and tetrahydrofuran.

[0029] The beneficial effects of the present invention are:

[0030] The invention introduces acrylic acid groups into the molecular chains of thermoplastic polyurethane elastomer solvent adhesive by using self-made polyester diol to directly prepare thermoplastic polyurethane elastomer; then, a photoinitiator is compounded and granulated by an extruder to obtain ultraviolet light-curable thermoplastic polyurethane elastomer solvent adhesive; the production process is simple and the production efficiency is high.

[0031] The UV-curable thermoplastic polyurethane elastomer solvent adhesive of the present invention can further cross-link macromolecules after being induced by UV light, thereby greatly improving the bonding strength. As the solvent evaporates, the crystallization property of the hard segment of the thermoplastic polyurethane elastomer causes the adhesive to further solidify, thereby greatly improving the bonding strength. Compared with traditional UV-curable adhesives, the adhesive has the characteristics of high bonding strength and good high temperature resistance, and the curing time is controllable, and the construction steps are simple and convenient. DETAILED DESCRIPTION

[0032] The principles and features of the present invention are described below in conjunction with embodiments. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0033] Embodiment 1:

[0034] Preparation of Homemade Polyester Diols:

[0035] Under nitrogen protection, 2000g of adipic acid, 308g of butanediol, 2506g of pentaerythritol diacrylate and 1g of tetrabutyl titanate were mixed, the temperature was raised to 150°C, and the reaction was carried out at a constant temperature for 4h; then the temperature was continued to be raised to 200°C within 1h, and the vacuum was turned on when the acid value was lower than 5mgKOH / g to remove the moisture and butanediol and pentaerythritol diacrylate in the system, and the reaction was continued until the hydroxyl value was 54-57mg KOH / g and the acid value was 0.15-0.35mg KOH / g to obtain a homemade polyester diol.

[0036] Preparation of UV-curable thermoplastic polyurethane elastomer solvent adhesive:

[0037] (1) 2000 g of self-made polyester diol was heated to 75°C, dehydrated for 2 hours under a vacuum degree of less than 20 kPa, and then heated to 85°C. Auxiliary agents: 6 g of antioxidant 1010, 6 g of antioxidant 1076, and 4 g of hydrolysis stabilizer carbodiimide were added, and stirred for 3 hours under nitrogen protection to obtain component A;

[0038] (2) 1325 g of diphenylmethane diisocyanate (MDI) was heated to 65° C., component A and 0.5 g of dibutyltin dilaurate were added under stirring, and the mixture was stirred for 5 to 10 minutes until the viscosity of the system increased to 10,000 to 20,000 mPa·s to obtain a polyurethane prepolymer;

[0039] (3) Add 380 g of 1,4-butanediol (melted at 45°C in advance) and stir for 1 to 2 minutes. The viscosity of the system will further increase. Quickly pour the melt into a tray to cool and solidify. Place the solidified material in a 90°C oven for 4 hours and crush the cured material into particles.

[0040] (4) The crushed particles in (3) were placed in an oven at 90°C and dried for 3 hours. The crushed particles were mixed with 50 g of benzophenone and 50 g of 4-methylbenzophenone and then granulated by a twin-screw extruder.

[0041] Embodiment 2:

[0042] Preparation of Homemade Polyester Diols:

[0043] Under nitrogen protection, 2000g of adipic acid, 246g of butanediol, 1906g of trimethylolpropane monoallyl ether and 1g of tetrabutyl titanate were mixed, the temperature was raised to 150°C, and the reaction was carried out at a constant temperature for 4h; then the temperature was continued to be raised to 200°C within 1h, and the vacuum was turned on when the acid value was lower than 5mgKOH / g to remove the moisture and butanediol and trimethylolpropane monoallyl ether in the system, and the reaction was continued until the hydroxyl value was 54-57mg KOH / g and the acid value was 0.15-0.35mg KOH / g to obtain a homemade polyester diol.

[0044] The preparation of the UV-curable thermoplastic polyurethane elastomer solvent adhesive is the same as that in Example 1 and will not be described in detail here.

[0045] Embodiment 3:

[0046] Preparation of Homemade Polyester Diols:

[0047] Under nitrogen protection, 2000g of adipic acid, 246g of butanediol, 1336g of pentaerythritol diacrylate, 953g of trimethylolpropane monoallyl ether and 1g of tetrabutyl titanate were mixed, the temperature was raised to 150°C, and the reaction was carried out at a constant temperature for 4h; then the temperature was continued to be raised to 200°C within 1h, and the vacuum was turned on when the acid value was lower than 5mgKOH / g, the water and butanediol, pentaerythritol diacrylate and trimethylolpropane monoallyl ether in the system were removed, and the reaction was continued until the hydroxyl value was 54-57mg KOH / g and the acid value was 0.15-0.35mg KOH / g, to obtain a homemade polyester diol with a molecular weight of 2000.

[0048] The preparation of the UV-curable thermoplastic polyurethane elastomer solvent adhesive is the same as that in Example 1 and will not be described in detail here.

[0049] Embodiment 4:

[0050] The preparation of the homemade polyester diol is the same as that in Example 1 and will not be repeated here.

[0051] Preparation of UV-curable thermoplastic polyurethane elastomer solvent adhesive:

[0052] Steps (1), (2), and (3) are the same as those in Example 1 and will not be repeated here.

[0053] (4) The crushed particles in (3) were placed in an oven at 90°C and dried for 3 hours. The crushed particles were mixed with 50 g of photoinitiator 819 (BAPO) and 50 g of triphenyl phosphite (TPO) and stirred until uniformly mixed, and then granulated by a twin-screw extruder.

[0054] Embodiment 5:

[0055] The preparation of the homemade polyester diol is the same as that in Example 1 and will not be repeated here.

[0056] Preparation of UV-curable thermoplastic polyurethane elastomer solvent adhesive:

[0057] Steps (1), (2), and (3) are the same as those in Example 1 and will not be repeated here.

[0058] (4) The crushed particles in (3) were placed in an oven at 90°C and dried for 3 hours. The crushed particles were mixed with 50 g of Michler's ketone and 50 g of isopropylthioxanthone and then granulated by a twin-screw extruder.

[0059] Comparative Example 1:

[0060] (1) 2000 g of polyester diol with a molecular weight of 2000 synthesized from adipic acid and butanediol was heated to 75°C, vacuum dehydrated for 2 hours, heated to 85°C, and added with additives: 6 g of antioxidant 1010, 6 g of antioxidant 1076, and 4 g of hydrolysis stabilizer carbodiimide. The mixture was stirred for 3 hours under nitrogen protection to obtain component A;

[0061] (2) Heat 1325 g of diphenylmethane diisocyanate (MDI) to 65°C, add component A and 0.5 g of dibutyltin dilaurate while stirring, and stir for 5 to 10 minutes until the viscosity of the system increases to obtain a prepolymer;

[0062] (3) Add 380 g of 1,4-butanediol (melted at 45°C in advance) and stir for 1 to 2 minutes. The viscosity of the system will further increase. Quickly pour the melt into a tray to cool and solidify. Place the solidified material in a 90°C oven for 4 hours and crush the cured material into particles.

[0063] (4) The pulverized particles in (3) were placed in an oven at 90°C and dried for 3 hours, and then granulated using a twin-screw extruder.

[0064] The properties of the solvent adhesive in Examples 1 to 5 and Comparative Example 1 are shown in Table 1:

[0065] Table 1 Solvent adhesive properties of the embodiments and comparative examples

[0066] project Testing standards unit Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 1 hardness ASTM D2240 shore A 90 90 90 90 90 91 Tensile Strength ASTM D412 (Die C) MPa 37 38 36 37 38 38 Elongation at break ASTM D412 (Die C) % 610 623 663 612 623 603 Initial flow temperature - ℃ 60 60 60 60 60 60 Dry time - min 5 6 7 6 6 6 Viscosity (15% solid content 25°C) ISO3219 mPa·S 800-1500 800-1500 800-1500 800-1500 800-1500 800-1500 Minimum activation temperature - ℃ 55-65 55-65 55-65 55-65 55-65 55-65 Peel strength after light curing (25℃) GB / T 2791-1995 KN / m 2.2 2.1 2.5 2.2 2.2 0.3 Peel strength after solvent evaporation (25°C) GB / T 2791-1995 KN / m 5.3 5.4 5.6 5.2 5.4 3.6

[0067] Examples 1 to 3 of the present invention use different homemade polyester diols and the same photoinitiator; Examples 1, 4, and 5 use the same homemade polyester diol and different combinations of photoinitiators; Comparative Example 1 uses conventional polyester polyols and uses the same process to prepare thermoplastic polyurethane elastomer. As shown in the data in Table 1, the hardness, tensile strength and other physical properties of the samples of Examples 1 to 5 and Comparative Example 1 are similar, indicating that after the acrylic acid group is introduced into the thermoplastic polyurethane elastomer of the present invention, it can still have the same performance as the ordinary thermoplastic polyurethane elastomer of Comparative Example 1; Solvent glue is prepared and tested according to the same solid content. After ultraviolet light induction, the molecules of Examples 1 to 5 are rapidly cross-linked and have a certain peel strength, while the solvent glue in Comparative Example 1 has a very weak peel strength after ultraviolet light induction; after the solvent evaporates, the peel strength of Examples 1 to 5 and Comparative Example 1 is greatly improved, but the peel strength of Examples 1 to 3 is significantly higher than that of Comparative Example 1. The ultraviolet light-curable thermoplastic polyurethane elastomer solvent glue of the present invention is significantly better than the ordinary thermoplastic polyurethane elastomer solvent glue in terms of bonding strength.

[0068] It can be seen that the homemade polyester diol of the present invention introduces acrylic acid groups into the molecular chains of thermoplastic polyurethane elastomer solvent adhesive, and matches the photoinitiator to obtain ultraviolet-cured thermoplastic polyurethane elastomer solvent adhesive; multiple cross-linking points are added to the long-chain thermoplastic polyurethane elastomer molecules of the solvent adhesive, and the molecules are rapidly cross-linked after being induced by ultraviolet light to form a network molecular structure, thereby improving the bonding strength; and as the solvent evaporates, the crystallization property of the hard segment of the thermoplastic polyurethane elastomer causes the adhesive to further solidify, and the bonding strength is greatly improved.

[0069] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A UV-curable thermoplastic polyurethane elastomer solvent adhesive, characterized in that: The composition comprises the following components in parts by weight: Diisocyanate: 20-40 parts, self-made polyester diol: 45-75 parts, chain extender: 4.5-13 parts, photoinitiator: 2-5 parts, auxiliary agent: 0.5-3.0 parts, catalyst: 0.005-0.02 parts; The preparation method of the self-made polyester diol is as follows: under nitrogen protection, a small molecule dibasic acid, a small molecule diol A, a small molecule diol B and a polyester synthesis catalyst are mixed, the temperature is raised to 140-180° C., and the reaction is carried out at a constant temperature for 1-5 hours; then the temperature is further raised to 190-220° C. within 0.5-2 hours, and the vacuum is turned on when the acid value is lower than 5 mgKOH / g, the water and the small molecule diol A and the small molecule diol B in the system are removed, and the reaction is continued until the hydroxyl value is 20-200 mg KOH / g and the acid value is 0.15-0.35 mg KOH / g; the molar ratio of the small molecule dibasic acid, the small molecule diol A and the small molecule diol B is 2:(0-1):(1-2); The small molecule diol A is one or two or more of ethylene glycol, propylene glycol, butylene glycol, hexylene glycol, diethylene glycol, 2-methyl-1,3-propanediol, neopentyl glycol, 2,2,4-trimethyl-1,3-pentanediol, 2-ethyl-2-butyl-1,3-propanediol, and 1,4-cyclohexanedimethanol; The small molecule diol B is a small molecule diol containing an acrylic acid group, and the small molecule diol containing an acrylic acid group is one or both of pentaerythritol diacrylate and trimethylolpropane monoallyl ether.

2. The UV-curable thermoplastic polyurethane elastomer solvent adhesive according to claim 1, characterized in that: The molecular weight of the self-made polyester diol is 1000-4000.

3. The UV-curable thermoplastic polyurethane elastomer solvent adhesive according to claim 1, characterized in that: The small molecule dibasic acid is one or two or more of succinic acid, glutaric acid, adipic acid, hexahydrophthalic anhydride, 1,4-cyclohexanedicarboxylic acid, azelaic acid, isophthalic acid, phthalic acid, and terephthalic acid.

4. The ultraviolet light-cured thermoplastic polyurethane elastomer solvent adhesive according to claim 1, characterized in that: The diisocyanate is an aromatic diisocyanate or an aliphatic diisocyanate.

5. The UV-curable thermoplastic polyurethane elastomer solvent adhesive according to claim 1, characterized in that: The chain extender is one or two or more of ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,4-cyclohexanediol, neopentyl glycol, hydroquinone bis(β-hydroxyethyl) ether, hydrogenated bisphenol A, dihydroxyethyl terephthalate, resorcinol dihydroxyethyl ether, glycerol α-allyl ether, TMP monoallyl ether, 3,3-dichloro-4,4-diaminodiphenylmethane, 3,5-diamino-p-chlorobenzoic acid isobutyl ester, diethyltoluenediamine, 3,5-dimethylthiotoluenediamine, 4,4-methylenebis(3-chloro-2,6-diethylaniline), and 1,3-propylene glycol-bis(4-aminobenzoate).

6. The ultraviolet light-cured thermoplastic polyurethane elastomer solvent adhesive according to claim 1, characterized in that: The photoinitiator is one or two or more of benzophenone, 4-methylbenzophenone, methyl o-benzoylbenzoate, 4-hydroxybenzophenone, 2,4-dihydroxybenzophenone, Michler's ketone, 4-fluoro-4'-hydroxybenzophenone, photoinitiator 819, triphenyl phosphite, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 2-dimethylamino-2-benzyl-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, thiopropoxythioxanthone, isopropylthioxanthone, ethyl dimethylaminobenzoate, triarylsulfonium salts, and isopropylferrocenium hexafluorophosphate.

7. The ultraviolet light-cured thermoplastic polyurethane elastomer solvent adhesive according to claim 1, characterized in that: The auxiliary agent is one or two of an antioxidant and a hydrolysis stabilizer.

8. The ultraviolet light-cured thermoplastic polyurethane elastomer solvent adhesive according to claim 1, characterized in that: The catalyst is one or two or more of an amine catalyst, an organic bismuth catalyst, an organic tin catalyst, an organic zinc catalyst, an organic lead catalyst, an organic cobalt catalyst, and an organic mercury catalyst.

9. A method for preparing the ultraviolet light-cured thermoplastic polyurethane elastomer solvent adhesive according to any one of claims 1 to 8, characterized in that: The steps include: S1: Heat and melt the self-made polyester diol, remove water by vacuum for 1 to 3 hours, add the auxiliary agent, stir evenly, and stir for no less than 3 hours to obtain component A; S2: Heat and melt the diisocyanate, then add component A and the catalyst, stir for 5 to 10 minutes, and wait until the viscosity rises to 10,000 to 20,000 mPa·s to obtain a polyurethane prepolymer; S3: Add a chain extender to the polyurethane prepolymer obtained in S2 to further extend the chain reaction, stir for 1 to 2 minutes, the melt viscosity further increases, pour into a tray for solidification, and mature at 90 to 95°C for 3 to 5 hours. After maturation, crush the sample into particles; S4: The crushed particles in S3 are dried in an oven, fully mixed with a photoinitiator, and then extruded into granules through an extruder.

Citation Information

Patent Citations

  • Ultraviolet-cured acrylic ester hot-melt pressure-sensitive adhesive and preparation method thereof

    CN107201180A

  • UV curable adhesive

    CN109181619A

  • Polyurethane acrylate adhesive containing ionic groups and preparation method thereof

    CN101974307A

  • Dual-curing reaction type polyurethane hot melt adhesive and preparation method thereof

    CN113736414A