Negative electrode active material, negative electrode sheet and battery

By covering the heterojunction MoSe2/MoS2 sheet layer in the intermediate layer of the carbon material, the MoSe2/MoS2@C composite material is formed, and the problem of poor sodium storage capacity and rate performance of the molybdenum diselenide negative electrode material is solved, and a higher Conductivity and cyclic stability.

CN118676351BActive Publication Date: 2024-12-03JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411127578.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-12-03
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

The existing molybdenum diselenide (MoSe2) negative electrode materials have poor performance in terms of sodium storage capacity, circulation performance and rate performance, mainly due to narrow layer spacing, low electronic conductivity and volume expansion problems.

Method used

Using MoSe2/MoS2@C composite material, the first and second sheets of heterojunction MoSe2/MoS2 are coated in the intermediate layer of carbon material to form a porous nanosheet structure, increase the layer spacing and reduce resistance, and improve conductivity. , the preparation method includes hydrothermal treatment and selenization/carbonization treatment.

Benefits of technology

It significantly improves the sodium storage capacity and cycle stability of the negative electrode active material, enhances the rate performance, reduces the resistance, and improves the electron transfer rate and electrochemical kinetics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118676351B_ABST
    Figure CN118676351B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of new energy batteries, and in particular to a negative electrode active material, a negative electrode sheet and a battery; the negative electrode active material comprises MoSe 2 / MoS 2 @C composite material; the MoSe 2 / MoS 2 The composite material has a flower-like structure formed by stacking a number of sheet structures; the sheet structure is formed by stacking a number of porous nanosheets; the porous nanosheet includes a carbon material middle layer, a heterojunction MoSe coated on one side of the carbon material middle layer 2 / MoS 2 The first sheet and the heterojunction MoSe coated on the other side of the carbon material intermediate layer 2 / MoS 2 The negative electrode active material of the present invention has excellent sodium storage capacity, cycle stability and rate performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of new energy batteries, and in particular to a negative electrode active material, a negative electrode sheet and a battery. Background Art

[0002] As market demand increases, the development of lithium-ion batteries may be constrained by lithium resources. Sodium-ion batteries are another type of energy storage battery with a similar working mechanism and battery structure to lithium-ion batteries. Recently, sodium-ion batteries have received increasing attention. With the continuous deepening of research, the potential advantages of sodium-ion batteries are constantly being explored, especially the excellent performance at high and low temperatures and high safety, which lays a good foundation for the application of sodium-ion batteries in the fields of energy storage and power.

[0003] In recent years, transition metal chalcogenides have attracted much attention due to their high theoretical capacity and high safety. 2 It shows excellent electrochemical activity. However, due to problems such as narrow interlayer spacing, low electronic conductivity, and volume expansion, its sodium storage capacity, cycle performance, and rate performance are poor.

[0004] Therefore, it is necessary to propose a simple preparation method to increase MoSe 2 interlayer spacing, improve conductivity, alleviate its volume expansion, and solve the problem of MoSe 2 Problems with poor sodium storage capacity, cycle performance and rate performance. Summary of the invention

[0005] In view of this, the present invention is committed to providing a negative electrode active material, a negative electrode plate and a battery to solve the problems of poor sodium storage capacity, cycle performance and rate performance of negative electrode materials containing molybdenum diselenide in the prior art.

[0006] A first aspect of the present invention provides a negative electrode active material, the negative electrode active material comprising MoSe 2 / MoS 2 @C composite material; the MoSe 2 / MoS 2 @C composite materials have a flower-like structure formed by the accumulation of several lamellar structures;

[0007] The sheet structure is formed by stacking a number of porous nanosheets;

[0008] The porous nanosheet includes a carbon material middle layer, a heterojunction MoSe coated on one side of the carbon material middle layer, and 2 / MoS 2 The first sheet and the heterojunction MoSe coated on the other side of the carbon material intermediate layer 2 / MoS 2 The second layer.

[0009] Optionally, the MoSe 2 / MoS 2 @C The specific surface area of ​​the composite material is 150~190m 2 / g.

[0010] Optionally, the diameter of the porous nanosheet is 1-3 μm; and / or the thickness of the porous nanosheet is 20-40 nm; and / or the pore diameter of the porous nanosheet is 20-30 nm; and / or the porosity of the porous nanosheet is 15-30%.

[0011] Optionally, the MoSe 2 / MoS 2 @C The total mass of the composite material is taken as the reference, the heterojunction MoSe 2 / MoS 2 The first sheet and the heterojunction MoSe 2 / MoS 2 The total content of the second sheet layer is 70-90wt%.

[0012] A second aspect of the present invention provides a method for preparing a negative electrode active material, the method comprising the following steps:

[0013] S1, adding molybdenum trioxide and a carbon-sulfur source into a solvent for mixing to obtain a first material; performing a hydrothermal treatment on the first material to obtain a second material;

[0014] S2, centrifuging the second material, collecting the precipitate, washing it, and drying it to obtain a precursor;

[0015] S3, mixing the precursor with selenium powder and performing selenization / carbonization treatment.

[0016] Optionally, the carbon-sulfur source is selected from at least one of alkyl sulfonate sodium salt, thiocyanate and diallyl sulfide.

[0017] Optionally, the carbon-sulfur source is sodium alkyl sulfonate; and / or the molar ratio of the molybdenum trioxide and the carbon-sulfur source is 1:1.5-6; and / or the solvent is water; and / or the mass ratio of the molybdenum trioxide to the solvent is 1:150-250.

[0018] Optionally, in step S1, the mixing treatment is magnetic stirring; the conditions of the magnetic stirring include: stirring time of 20~40min, stirring speed of 200~400 r / min; and / or, the hydrothermal treatment is carried out in a polytetrafluoroethylene reactor; and / or, the conditions of the hydrothermal treatment include: temperature of 160~200℃, time of 6~12h; and / or, in step S2, the washing liquid used for washing is selected from anhydrous ethanol and / or water; and / or, the conditions of the drying treatment include: temperature of 50~70℃, time of 18~36h; and / or, in step S3, the selenization / carbonization treatment includes: mixing selenium powder with the precursor and then performing high-temperature treatment; the high-temperature treatment is carried out under the protection of a protective atmosphere; the temperature of the high-temperature treatment is 400~600℃, and the time of the high-temperature treatment is 1~3h.

[0019] A third aspect of the present invention provides a negative electrode plate, comprising a current collector and a negative electrode material disposed on the surface of the current collector, wherein the negative electrode material comprises the above-mentioned negative electrode active material and / or the negative electrode active material prepared according to the above-mentioned method.

[0020] A fourth aspect of the present invention provides a battery, comprising the negative electrode plate described above.

[0021] Through the above technical solution, the beneficial technical effects of the present invention are:

[0022] (1) MoSe contained in the negative electrode active material provided by the present invention 2 / MoS 2 The composite material has a flower-like structure formed by stacking several sheet structures, which are formed by stacking several porous nanosheets, including a carbon material middle layer, which increases the MoSe 2 / MoS 2 The interlayer spacing enhances the sodium storage capacity of the negative electrode active material and alleviates the MoSe 2 / MoS 2 The volume expansion of the carbon material increases the cycle stability and rate performance. 2 / MoS 2 The first sheet and the heterojunction MoSe coated on the other side of the carbon material intermediate layer 2 / MoS 2 The second layer, heterojunction MoSe 2 / MoS 2 The presence of reduces the resistance of the negative electrode active material, and the coupled electric field increases the electron transfer rate, enhances the electrochemical kinetics, and improves the rate performance.

[0023] (2) The preparation method of the negative electrode active material of the present invention is to prepare molybdenum trioxide MoO 3 Mixed with carbon and sulfur sources, and hydrothermal sulfurization was performed to prepare flower-like carbon material intercalated MoS 2 Precursor, and then the precursor is carbonized / selenized to obtain MoSe 2 / MoS 2 @C flower-like composite material. The method of the present invention adds carbon and sulfur sources during the hydrothermal process to regulate the flower-like intercalated carbon structure MoS 2 / MoSe 2 @C flower-like composite materials, thereby significantly improving the ion diffusion rate.

[0024] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention, but do not constitute a limitation of the present invention.

[0026] Figure 1 Shown is an electron microscope scanning image of the negative electrode active material prepared in Example 1. DETAILED DESCRIPTION

[0027] The present invention discloses a negative electrode active material, a negative electrode plate and a battery. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve the same. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art and are deemed to be included in the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.

[0028] In the description of the present invention, a list of items connected by the term "at least one of" or other similar terms may mean any combination of the listed items. For example, if items A, B are listed, the phrase "at least one of A, B" means only A; only B; or A and B. In another example, if items A, B, C are listed, the phrase "at least one of A, B, C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.

[0029] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range or the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0030] If not otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form a new technical solution.

[0031] Unless otherwise specified, all technical features and optional technical features of the present invention can be combined with each other to form a new technical solution.

[0032] If there is no special explanation, the "include" and "comprising" mentioned in the present invention represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0033] In order to solve the problem that the negative electrode material containing molybdenum diselenide in the prior art has poor sodium storage capacity, cycle performance and rate performance, the present invention adopts the following technical solution:

[0034] A first aspect of the present invention provides a negative electrode active material, the negative electrode active material comprising MoSe 2 / MoS 2 @C composite material; the MoSe 2 / MoS 2 @C composite materials have a flower-like structure formed by the accumulation of several lamellar structures;

[0035] The sheet structure is formed by stacking a number of porous nanosheets;

[0036] The porous nanosheet includes a carbon material middle layer, a heterojunction MoSe coated on one side of the carbon material middle layer, and 2 / MoS 2 The first sheet and the heterojunction MoSe coated on the other side of the carbon material intermediate layer 2 / MoS 2 The second layer.

[0037] The MoSe contained in the negative electrode active material of the present invention 2 / MoS 2 The composite material has a flower-like structure formed by stacking several sheet structures, which are formed by stacking several porous nanosheets, including a carbon material middle layer, which increases the MoSe 2 / MoS2 The interlayer spacing enhances the sodium storage capacity of the negative electrode active material and alleviates the MoSe 2 / MoS 2 The volume expansion of the carbon material increases the cycle stability and rate performance. 2 / MoS 2 The first sheet and the heterojunction MoSe coated on the other side of the carbon material intermediate layer 2 / MoS 2 The second layer, heterojunction MoSe 2 / MoS 2 The presence of reduces the resistance of the negative electrode active material, and the coupled electric field increases the electron transfer rate, enhances the electrochemical kinetics, and improves the rate performance.

[0038] According to the present invention, the MoSe 2 / MoS 2 @C The specific surface area of ​​the composite material can be 150~190m 2 / g; For example, the MoSe 2 / MoS 2 @C The specific surface area of ​​the composite material can be 150 m 2 / g, 160 m 2 / g, 170 m 2 / g, 180 m 2 / g and 190 m 2 / g or any value in the range of values ​​formed by any two of the above values. If the specific surface area of ​​the negative electrode active material is too large, it will lead to excessive initial capacity loss, and the contact area between the negative electrode material and the electrolyte will increase, which may cause more irreversible reactions to occur; if the specific surface area of ​​the negative electrode active material is too small, the electrochemical reaction sites will be reduced, and the channels for lithium ion migration will be fewer, resulting in poor rate performance. Preferably, in order to further improve the channels for ion migration, shorten the migration path, and improve the rate performance of the battery, the MoSe 2 / MoS 2 @C The specific surface area of ​​the composite material is 170~180m 2 / g.

[0039] In the present invention, the appropriate diameter and thickness of the porous nanosheets are beneficial to controlling the particle uniformity of the negative electrode active material.

[0040] According to the present invention, the diameter of the porous nanosheet can be 1~3μm; in the present invention, "the diameter of the porous nanosheet" can be defined as the extension direction of the porous nanosheet as the radial direction, and the extension size of the porous nanosheet in the radial direction. Exemplarily, the diameter of the porous nanosheet can be any value among 1 μm, 1.5 μm, 2.0 μm, 2.5 μm and 3 μm, or any value within the range of values ​​composed of any two of the above values. Among them, a porous nanosheet with a diameter that is too small is not conducive to shortening the ion diffusion path, and a porous nanosheet with a diameter that is too large is not conducive to structural stability. Preferably, in order to further enhance the stability of the structure and shorten the ion diffusion path, the diameter of the porous nanosheet can be 1.5~2μm.

[0041] According to the present invention, the thickness of the porous nanosheet can be 20-40 nm; in the present invention, "the thickness of the porous nanosheet" can be defined as the dimension of the porous nanosheet perpendicular to the extension direction of the porous nanosheet as the radial direction. Exemplarily, the thickness of the porous nanosheet can be any value among 20 nm, 24 nm, 28 nm, 32 nm, 36 nm and 40 nm or any value within the range of values ​​composed of any two of the above values. Among them, too small a thickness of the porous nanosheet is not conducive to structural stability, and too large a thickness of the porous nanosheet is not conducive to shortening the ion diffusion path. Preferably, under the premise of ensuring structural stability, the ion diffusion path is further shortened, and the thickness of the porous nanosheet can be 25-35 nm.

[0042] The porous nanosheets in the present invention have abundant mesopores, and the reasonable pore size distribution in the porous nanosheets can balance the charge and discharge rate and the cycle life, and improve the overall performance of the battery. Optionally, the pore size of the porous nanosheet is 20-30 nm; illustratively, the pore size of the porous nanosheet can be any value among 20 nm, 22 nm, 24 nm, 26 nm, 28 nm and 30 nm, or any value within the range of any two of the above values. Among them, the pore size of the porous nanosheet is too small to ensure the transmission rate of ions and electrons, and the pore size of the porous nanosheet is too large to be conducive to structural stability. Preferably, the pore size of the porous nanosheet can be 23-27 nm.

[0043] According to the present invention, the porous nanosheet has a larger porosity to accommodate more active substances and electrolytes, thereby improving the energy density of the battery. Optionally, the porosity of the porous nanosheet may be 15-30%. Exemplarily, the porosity of the porous nanosheet may be any value among 15%, 20%, 25% and 30% or any value within the range of any two of the above values. Among them, the porosity of the porous nanosheet is too small to accommodate active substances and electrolytes, and the porosity of the porous nanosheet is too large to be conducive to structural stability. Preferably, the porosity of the porous nanosheet may be 20-25%.

[0044] According to the present invention, in order to improve the electrochemical activity of the battery, the negative electrode active material of the present invention contains a relatively high content of heterojunction MoSe 2 / MoS 2 The first sheet and the heterojunction MoSe 2 / MoS 2 The second layer is MoSe 2 / MoS 2 @C The total mass of the composite material is taken as the reference, the heterojunction MoSe 2 / MoS 2 The first sheet and the heterojunction MoSe 2 / MoS 2 The total content of the second layer is 70-90 wt%. In the present invention, the heterojunction MoSe 2 / MoS 2 The first sheet and the heterojunction MoSe 2 / MoS 2 The total content of the second layer is the heterojunction MoSe 2 / MoS 2 The first layer and the heterojunction MoSe 2 / MoS 2 The total mass of the second layer. 2 / MoS 2 The first sheet and the heterojunction MoSe 2 / MoS 2 The total content of the second sheet layer can be any value among 70 wt%, 75 wt%, 80 wt%, 85 wt% and 90 wt% or any value within the range of any two of the above values. Preferably, the presence of an appropriate amount of heterojunction can ensure sufficient capacity, and the presence of the remaining carbon materials can ensure structural stability, enhance electron transfer rate, and enhance rate performance. The heterojunction MoSe 2 / MoS 2 The first sheet and the heterojunction MoSe 2 / MoS 2 The total content of the second sheet layer can be 75-85wt%.

[0045] A second aspect of the present invention provides a method for preparing a negative electrode active material, the method comprising the following steps:

[0046] S1, adding molybdenum trioxide and a carbon-sulfur source into a solvent for mixing to obtain a first material; performing a hydrothermal treatment on the first material to obtain a second material;

[0047] S2, centrifuging the second material, collecting the precipitate, washing it, and drying it to obtain a precursor;

[0048] S3, mixing the precursor with selenium powder and performing selenization / carbonization treatment.

[0049] The preparation method of the negative electrode active material of the present invention is to prepare molybdenum trioxide MoO 3 Mixed with carbon and sulfur sources, during the hydrothermal process, the carbon and sulfur sources enter the interlayer of molybdenum trioxide through molecular motion, and then MoO 3 React with the sulfur source between the layers to form MoS 2 , MoS intercalated with flower-like carbon materials was prepared 2 Precursor, and then the precursor is carbonized / selenized to obtain MoSe 2 / MoS 2 @C flower-like composite material. The method of the present invention adds carbon and sulfur sources during the hydrothermal process to regulate the flower-like intercalated carbon structure MoS 2 / MoSe 2 @C flower-like composite materials, thereby significantly improving the ion diffusion rate.

[0050] In the present invention, the carbon-sulfur source can be selected from at least one of alkyl sulfonate sodium salt, thiocyanate and diallyl sulfide.

[0051] As a preferred embodiment of the present invention, the carbon-sulfur source is sodium alkyl sulfonate. In the embodiment of the present invention, molybdenum trioxide and sodium alkyl sulfonate are mixed and hydrothermally heated. During the hydrothermal process, the sulfur source contained in the sodium alkyl sulfonate present between the molybdenum trioxide layers will sulfidize the molybdenum trioxide to form a precursor, which is a mixture of molybdenum disulfide and its interlayer carbonaceous material, and has a flower-like shape; after the precursor is carbonized and selenized, the interlayer carbon source becomes a carbon skeleton supporting the overall structure, and part of the molybdenum sulfide is selenized into molybdenum diselenide to obtain MoSe 2 / MoS 2 @CFlower-like composite material.

[0052] While providing carbon and sulfur sources, sodium alkyl sulfonate can supplement additional sodium sources, thereby reducing the loss of sodium ions during the first cycle of charge and discharge and improving the first cycle coulombic efficiency. Furthermore, sodium alkyl sulfonate can also play the role of a surface modifier, which is conducive to promoting the formation of curved flakes during the hydrothermal process. The flower-like structure of the curved flake combination has more surface area and increases more reaction sites, which is conducive to improving the sodium storage performance.

[0053] Optionally, the structural formula of the sodium salt of alkyl sulfonate of the present invention is as shown in formula (1), wherein R is a straight-chain aliphatic alkyl group:

[0054] ;

[0055] Formula (1)

[0056] Exemplarily, the sodium salt of alkyl sulfonate is selected from at least one of sodium dodecyl sulfonate, sodium pentadecyl sulfonate, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, sodium octadecylbenzene sulfonate, sodium dodecyl ether sulfate, sodium dodecyl diphenyl ether disulfonate, disodium octadecyl succinamide sulfonate, sodium 1-pentane sulfonate, sodium secondary alkyl sulfonate, sodium fatty alcohol alkyl sulfonate, sodium alkyl naphthalene sulfonate and sodium alkylbenzene sulfonate.

[0057] In the present invention, too much carbon-sulfur source will affect the hydrothermal nucleation of molybdenum disulfide, and too little sulfurization is not easy to succeed and the improvement of the cycle is not obvious. Optionally, the molar ratio of the molybdenum trioxide and the carbon-sulfur source is 1:1.5-6, preferably 1:2-4; more preferably 1:3.

[0058] The solvent in the present invention is water; optionally, the mass ratio of the molybdenum trioxide to the solvent is 1:150-250; illustratively, the mass ratio of the molybdenum trioxide to the solvent can be any value among 1:150, 1:175, 1:200, 1:225 and 1:250 or any value within the range of any two of the above values. Preferably, the mass ratio of the molybdenum trioxide to the solvent can be 1:180-220.

[0059] In an optional embodiment of the present invention, in step S1, the mixing treatment is magnetic stirring; the conditions of the magnetic stirring may include: a stirring time of 20 to 40 minutes and a stirring speed of 200 to 400 r / min. In the present invention, the hydrothermal treatment enables the carbon source to be intercalated between the layers of molybdenum trioxide, and the molybdenum trioxide is sulfided. Preferably, the hydrothermal treatment is carried out in a polytetrafluoroethylene reactor; and / or, the conditions of the hydrothermal treatment include: a temperature of 160 to 200°C, preferably 180 to 200°C; a time of 6 to 12 hours, preferably 8 to 12 hours.

[0060] In an optional embodiment of the present invention, in step S2, the washing liquid used in the washing is selected from anhydrous ethanol and / or water. Exemplarily, the washing of the present invention can be washing three times with water and ethanol respectively to remove excess growth and unstable impurities. Preferably, the conditions of the drying treatment include: a temperature of 50-70°C and a time of 18-36 hours.

[0061] In an optional embodiment of the present invention, in step S3, the "selenization / carbonization treatment" in the present invention specifically refers to the step including selenization treatment and carbonization treatment, and the selenization treatment and carbonization treatment are carried out simultaneously. Exemplarily, the step of the selenization / carbonization treatment includes: mixing the selenium powder with the precursor and then performing a high-temperature treatment, wherein the high-temperature treatment in the present invention is carried out under the protection of a protective atmosphere to prevent air from entering, wherein the protective atmosphere can be one of nitrogen, argon, neon, helium, xenon and krypton. In the present invention, high-temperature carbonization can cause the carbon alkyl to lose hydrogen and oxygen and polymerize into carbides, and high-temperature selenization can convert selenium powder into hydrogen selenide gas, and hydrogen selenide gas selenizes molybdenum disulfide into molybdenum diselenide. Optionally, the temperature of the high-temperature treatment is 400~600℃, and the time of the high-temperature treatment is 1~3h. Preferably, the temperature of the high-temperature treatment is 450~550℃, and this temperature range can produce uniform amorphous carbon.

[0062] A third aspect of the present invention provides a negative electrode plate, comprising a current collector and a negative electrode material disposed on the surface of the current collector, wherein the negative electrode material comprises the above-mentioned negative electrode active material and / or the negative electrode active material prepared according to the above-mentioned method.

[0063] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode active material layer is disposed on the side in contact with the separator so that the negative electrode active material reacts with ions released from the positive electrode to reduce the ion diffusion rate.

[0064] The present application has no particular restrictions on the material of the negative electrode current collector, as long as the purpose of the present application can be achieved, and it can be selected according to actual needs. For example, in some embodiments, the negative electrode current collector includes common copper foil (the copper foil can be modified, such as the setting of a carbon coating layer, screen-printed copper foil, porous copper foil, copper mesh, etc.), or the negative electrode current collector can adopt a composite current collector structure (such as a composite current collector structure containing a polymer layer and a metal layer), and those skilled in the art can make adaptive selections according to actual needs.

[0065] In some embodiments, the negative electrode active material layer includes the aforementioned negative electrode active material and also includes a basic negative electrode material, that is, the negative electrode active material of the negative electrode active material layer may be composed of the negative electrode active material of this embodiment and a conventional negative electrode material. Optionally, the basic negative electrode material (conventional negative electrode material) may be a carbon material. As an example, the basic negative electrode material may be conventional negative electrode materials such as artificial graphite, natural graphite, soft carbon, and hard carbon.

[0066] In some embodiments, the negative electrode active material layer also includes a conductive agent, a binder and a solvent. The present application has no particular restrictions on the type of conductive agent, which can also be selected by conventional technology. As an example, the conductive agent includes but is not limited to a combination of one or more of superconducting carbon, conductive graphite, conductive carbon black (including acetylene black, Ketjen black, etc.), carbon nanotubes (including single-walled carbon nanotubes and / or multi-walled carbon nanotubes), graphene or carbon fiber. The present application has no particular restrictions on the type of conductive agent, which can also be selected by conventional technology. As an example, the binder includes but is not limited to a combination of one or more of polyvinylidene fluoride (PVDF), styrene-butadiene rubber (SBR), sodium carboxymethyl cellulose (CMC), polyacrylate (LA), polyacrylic acid binder (PAA), etc. The present application has no particular restrictions on the type of negative electrode solvent, which can also be selected by conventional technology. As an example, the negative electrode solvent can be N-methylpyrrolidone (NMP).

[0067] In a preferred embodiment of the present invention, the preparation method of the negative electrode sheet may include: pouring the negative electrode active material, the binder, and the conductive agent into an agate mortar in a certain proportion in sequence, mixing and grinding until the powder is evenly mixed and fine. Then pour it into a small weighing bottle, and drop the negative electrode solvent while stirring magnetically until the powder is evenly infiltrated and the drop is stopped. Then magnetic stirring and ultrasonic treatment are performed, and this process is repeated 1 to 3 times. The mixed slurry is evenly coated and flattened on the current collector aluminum foil with a coater, and then placed in a drying oven for drying. Then the electrode sheet is cut into circular electrode sheets with a slicer, and the circular electrode sheets are compacted with a tablet press and weighed to obtain the negative electrode sheet. Exemplarily, the mixing mass ratio of the negative electrode active material, the binder, and the conductive agent can be (6 to 10): (0.8 to 1.2): 1, for example, it can be 8: 1: 1.

[0068] A fourth aspect of the present invention provides a battery, comprising the negative electrode plate described above.

[0069] In the embodiment of the present invention, the battery structure includes but is not limited to button batteries, soft-pack batteries, cylindrical batteries, etc.

[0070] The present invention is further described in detail by way of examples. The raw materials used in the examples can be obtained through commercial sources. The binder used in the examples and comparative examples is polyvinylidene fluoride (PVDF), and the conductive agent is conductive carbon black (Super P).

[0071] Example 1

[0072] (1) Weigh 0.07 mol of molybdenum trioxide and 0.21 mol of sodium dodecyl sulfate into a beaker with a magnet and distilled water. The mass ratio of molybdenum trioxide to distilled water is 1:200. Stir for 30 min at a stirring speed of 350 r / min. Then add the stirred solution to a polytetrafluoroethylene reactor for hydrothermal treatment. Place the reactor in an oven for hydrothermal reaction. The hydrothermal treatment temperature is 200 °C and the hydrothermal treatment time is 10 h.

[0073] (2) Collect the sample with a high-speed centrifuge, wash the sample three times with water and ethanol to obtain a washed material, dry the washed material in a drying oven at a constant temperature of 60°C for 24 hours to obtain a precursor sample.

[0074] (3) The precursor and selenium powder were mixed in a mass ratio of 1:3, and the magnetic boat containing the mixed powder was placed in the middle of a tube furnace. The selenization / carbonization treatment was performed at 500°C for 2 hours in a nitrogen protective atmosphere, and finally the MoSe of this embodiment was obtained. 2 / MoS 2 @CComposite materials.

[0075] (4) Preparation of negative electrode sheet: The prepared composite material, binder and conductive agent are poured into an agate mortar in a mass ratio of 8:1:1, and mixed and ground for 30 min until the powder is evenly mixed and fine. Then pour it into a small weighing bottle, and add NMP solvent while stirring magnetically until the powder is evenly soaked and then stop adding. Then stir magnetically for 20 min and then ultrasonically treat for 15 min, and repeat this process 3 times. The mixed slurry is evenly coated and scraped on the current collector aluminum foil with a coater, and then placed in a drying oven, set to a constant temperature of 80°C, and taken out after drying for 12 h. Then use a slicer to cut the electrode sheet into a circular electrode sheet with a radius of 6 mm, and the circular electrode sheet is compacted with a tablet press and weighed to obtain the negative electrode sheet.

[0076] (5) Preparation of sodium ion button half-cell: The prepared negative electrode material was used as the working electrode, the metal sodium sheet was used as the reference electrode, Whatman GF / D glass fiber was used as the separator, nickel foam was used as the spacer, and 1 mol·L -1 NeA 6 The diethylene glycol methyl ether solution was used as the sodium ion battery electrolyte and added several times. The half-cell was assembled in the order of positive electrode shell, negative electrode material, separator, sodium sheet, nickel foam and negative electrode shell. The assembled half-cell was clamped on the packaging machine with insulating tweezers for sealing. Finally, the packaged battery was taken out of the glove box and left to stand for 24 hours to allow the electrolyte to fully infiltrate before conducting relevant electrochemical tests.

[0077] Example 2

[0078] (1) Weigh 0.07 mol of molybdenum trioxide and 0.14 mol of sodium dodecylbenzene sulfonate and add them into a beaker with a magnet and distilled water. The mass ratio of molybdenum trioxide to distilled water is 1:200. Stir for 30 min at a stirring speed of 300 r / min. Then add the stirred solution into a polytetrafluoroethylene reactor and place the reactor in an oven for hydrothermal reaction. The hydrothermal treatment temperature is 200 °C and the hydrothermal treatment time is 12 h.

[0079] (2) Collecting the sample with a high-speed centrifuge, washing the sample with water and ethanol three times to obtain a washed material, and drying the washed material in a drying oven at a constant temperature of 60°C for 24 hours to obtain a precursor sample;

[0080] (3) The precursor and selenium powder were mixed in a mass ratio of 1:3, and the magnetic boat containing the mixed powder was placed in the middle of a tube furnace. The selenization / carbonization treatment was performed at 400°C for 1.5 hours in a nitrogen protective atmosphere. Finally, the MoSe 2 / MoS 2 @CComposite materials.

[0081] The manufacturing method of the negative electrode sheet and the sodium ion button half-cell of this embodiment is the same as that of Embodiment 1.

[0082] Example 3

[0083] (1) Weigh 0.07 mol of molybdenum trioxide and 0.28 mol of sodium dodecyl sulfate into a beaker with a magnet and distilled water. The mass ratio of molybdenum trioxide to distilled water is 1:200. Stir for 30 min at a speed of 350 r / min. Add the stirred solution into a polytetrafluoroethylene reactor and place the reactor in an oven for hydrothermal reaction. The hydrothermal treatment temperature is 180 °C and the hydrothermal treatment time is 12 h.

[0084] (2) Collecting the sample with a high-speed centrifuge, washing the sample with water and ethanol three times to obtain a washed material, and drying the washed material in a drying oven at a constant temperature of 60°C for 24 hours to obtain a precursor sample;

[0085] (3) The precursor and selenium powder were mixed in a mass ratio of 1:3, and the magnetic boat containing the mixed powder was placed in the middle of a tube furnace. The selenization / carbonization treatment was performed at 600°C for 2 hours in a nitrogen protective atmosphere. Finally, the MoSe 2 / MoS 2 @CComposite materials.

[0086] The manufacturing method of the negative electrode sheet and the sodium ion button half-cell of this embodiment is the same as that of Embodiment 1.

[0087] Example 4

[0088] (1) Weigh 0.07 mol of molybdenum trioxide and 0.35 mol of sodium dodecyl sulfate into a beaker with a magnet and distilled water. The mass ratio of molybdenum trioxide to distilled water is 1:200. Stir for 30 min at a stirring speed of 300 r / min. Then add the stirred solution into a polytetrafluoroethylene reactor. Place the reactor in an oven for hydrothermal reaction at a temperature of 180 °C and a time of 12 h.

[0089] (2) Collecting the sample with a high-speed centrifuge, washing the sample with water and ethanol three times to obtain a washed material, and drying the washed material in a drying oven at a constant temperature of 60°C for 24 hours to obtain a precursor sample;

[0090] (3) The precursor and selenium powder were mixed in a mass ratio of 1:3, and the magnetic boat containing the mixed powder was placed in the middle of a tube furnace. The selenization / carbonization treatment was performed at 600°C for 2 hours in a nitrogen protective atmosphere. Finally, the MoSe 2 / MoS 2 @CComposite materials.

[0091] The manufacturing method of the negative electrode sheet and the sodium ion button half-cell of this embodiment is the same as that of Embodiment 1.

[0092] Example 5

[0093] (1) Weigh 0.07 mol of molybdenum trioxide and 0.07 mol of sodium dodecyl sulfate into a beaker with a magnet and distilled water. The mass ratio of molybdenum trioxide to distilled water is 1:200. Stir for 30 min at a stirring speed of 200 r / min. Then add the stirred solution into a polytetrafluoroethylene reactor. Place the reactor in an oven for hydrothermal reaction. The hydrothermal treatment temperature is 180°C and the hydrothermal treatment time is 12 h.

[0094] (2) Collect the sample with a high-speed centrifuge, wash the sample three times with water and ethanol to obtain a washed material, dry the washed material in a drying oven at a constant temperature of 60°C for 24 hours to obtain a precursor sample.

[0095] (3) The precursor and selenium powder were mixed in a mass ratio of 1:3, and the magnetic boat containing the mixed powder was placed in the middle of a tube furnace. The selenization / carbonization treatment was performed at 400°C for 2 hours in a nitrogen protective atmosphere. Finally, the MoSe 2 / MoS 2 @CComposite materials.

[0096] The manufacturing method of the negative electrode sheet and the sodium ion button half-cell of this embodiment is the same as that of Embodiment 1.

[0097] Comparative Example 1

[0098] (1) Weigh 0.07 mol of molybdenum trioxide and 0.21 mol of selenium powder and add them to a beaker with a magnet and distilled water. The mass ratio of molybdenum trioxide to distilled water is 1:200. Stir for 30 min at a stirring speed of 300 r / min. Then add the stirred solution to a polytetrafluoroethylene reactor and place the reactor in an oven for hydrothermal reaction. The hydrothermal treatment temperature is 200 °C and the hydrothermal treatment time is 12 h.

[0099] (2) Collect the sample with a high-speed centrifuge, wash the sample with water and ethanol three times to obtain the washed material, and dry the washed material in a drying oven at a constant temperature of 60°C for 24 hours to obtain MoSe 2 The powder material is the negative electrode active material of this comparative example.

[0100] The manufacturing method of the negative electrode sheet and the sodium ion button half-cell of this comparative example is the same as that of Example 1.

[0101] Test Example 1

[0102] First-cycle capacity test: Take the sodium ion button half-cells prepared in the embodiment and the comparative example respectively, and carry out the first-cycle capacity test under the test conditions of 0.2 C rate, charging cut-off voltage 3.0 V, and discharging cut-off voltage 0 V at 25°C. The specific measurement method of the first-cycle discharge capacity is: after the battery is charged to 3.0V, it is discharged to 0V at a rate of 0.2C, and the capacity discharged is divided by the amount of active material to be the first-cycle discharge capacity. The specific measurement method of the first-cycle coulomb efficiency is: first-cycle discharge capacity / first-cycle charge capacity.

[0103] 1C / 1C cycle life test: Take the sodium ion button half-cells prepared in the embodiment and the comparative example respectively, and carry out 1C / 1C cycle test at 25°C (charge cut-off voltage 3.0V, discharge cut-off voltage 0V). The specific measurement method of the discharge specific capacity after 200 cycles of 1C / 1C is as follows: after the battery has been cycled to 199 cycles, it is charged to 3.0V again and discharged to 0V at a rate of 0.2C. The discharged capacity divided by the amount of active material is the 200th cycle discharge specific capacity. The specific measurement method of the capacity retention rate after 200 cycles of 1C / 1C cycle is as follows: 200th cycle discharge specific capacity / first cycle discharge specific capacity.

[0104] The measurement method of the charge transfer resistance of the new battery is: use the Autolab electrochemical workstation to test the charge transfer resistance of the half-cell, and the test frequency is 0.01Hz~100kHz.

[0105] The specific measurement method of the sodium ion diffusion coefficient of the new battery is: use the CT2001A blue battery system to perform a constant current intermittent titration test on the half-cell with a voltage range of 0.01~3.0 V.

[0106] The specific measurement method of the rate discharge ratio of a half-cell is as follows: after the battery is charged to 3.0V, it is discharged to 0V at rates of 0.5C, 1C, 2C, and 5C respectively. The discharged capacity divided by the amount of active material is the discharge specific capacity at different rates.

[0107] Among them, the first charge and discharge capacity, coulomb efficiency, discharge capacity after 200 cycles of 1C / 1C and charge transfer resistance of the new battery of the half-cell are shown in Table 1. The rate discharge capacity of the half-cell is shown in Table 2.

[0108] Table 1

[0109]

[0110] Table 2

[0111]

[0112] It can be seen from the data in Table 1 and Table 2 that the molybdenum disulfide / molybdenum diselenide heterojunction composite carbon flower-like material (MoSe 2 / MoS 2 @C composite material) is used for the negative electrode of sodium ion batteries, which enhances the sodium storage capacity of the material and alleviates the MoSe 2 / MoS 2 The volume expansion is reduced, and the charging and discharging internal resistances are lower, and the battery exhibits better rate performance and cycle performance.

[0113] also, Figure 1 The MoSe prepared in Example 1 2 / MoS 2 @C composite material scanning electron microscope image, from Figure 1 It can be seen that the MoSe prepared in Example 1 2 / MoS 2 @C The composite material is a flower-like structure formed by the stacking of several lamellar structures.

[0114] Specifically, it can be seen from Table 1 and Table 2 that the negative electrode active materials prepared in Examples 1 to 5 are applied to sodium ion button half-cells, and the first charge and discharge capacity, coulomb efficiency, discharge capacity at different rates, and discharge capacity after 200 cycles of 1C / 1C are significantly improved, the charge transfer resistance of the new battery is significantly reduced, and the sodium ion diffusion coefficient of the new battery is significantly increased. By comparing Example 3 with Example 4, it can be seen that when the molar ratio of molybdenum trioxide and sodium dodecyl sulfate is adjusted from 1:4 to 1:5, the first charge and discharge capacity, coulomb efficiency, discharge capacity at different rates, and discharge capacity after 200 cycles of 1C / 1C are reduced to a certain extent, so too much alkyl sulfonic acid sodium salt will affect the hydrothermal nucleation of molybdenum disulfide, which is not conducive to long-term circulation. By comparing Example 2 with Example 5, it can be seen that when the molar ratio of molybdenum trioxide and sodium dodecyl sulfate is adjusted from 1:2 to 1:1, and the hydrothermal treatment temperature is adjusted from 200°C to 180°C, the initial charge and discharge capacity, coulomb efficiency, discharge capacity at different rates, and discharge capacity after 200 cycles of 1C / 1C will also decrease, the charge transfer resistance of the new battery will increase, and the ion diffusion rate will decrease, indicating that too little alkyl sulfonic acid sodium salt will affect the vulcanization and ion diffusion rate, thereby affecting the cycle performance. 2 When the powder material is used as the negative electrode active material, the initial charge and discharge capacity, coulombic efficiency, discharge specific capacity at different rates and discharge specific capacity after 200 cycles of 1C / 1C are significantly reduced. At the same time, the charge transfer resistance of the new battery is significantly improved.

[0115] Test Example 2

[0116] The negative electrode active materials prepared in the examples and comparative examples were measured, among which MoSe 2 / MoS 2 The specific surface area, pore size and porosity of the porous nanosheets of the composite material were determined by nitrogen adsorption-desorption isothermal test, and the diameter and thickness of the porous nanosheets were calibrated by SEM phase images. 2 / MoS 2 The first layer and heterojunction MoSe 2 / MoS 2 The total content of the second layer was measured using an energy dispersive X-ray spectrometer (EDS). The test results are shown in Table 3.

[0117] Table 3

[0118]

[0119] It can be seen from the data in Table 3 that the MoSe prepared in Examples 1 to 5 2 / MoS 2 @C The specific surface area of ​​the composite material is 170~180m 2 / g, the porous nanosheet has a sheet diameter of 1.5-2.0 μm, a thickness of 25-35 nm, a pore diameter of 23-27 nm, and a porosity of 20-25%; the composite material prepared in Comparative Example 1 does not contain MoSe 2 / MoS 2 Combining the data in Tables 1 and 2, it can be seen that compared with Comparative Example 1, the MoSe prepared in Examples 1 to 5 2 / MoS 2 The charge transfer resistance of the @C composite material is significantly reduced and the sodium ion diffusion coefficient is significantly increased, indicating that the electrochemical reaction kinetics is significantly improved, which is beneficial to the improvement of electrical performance.

[0120] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a negative electrode active material, characterized in that: The method comprises the following steps: S1, adding molybdenum trioxide and a carbon-sulfur source into a solvent for mixing to obtain a first material; performing a hydrothermal treatment on the first material to obtain a second material; S2, centrifuging the second material, collecting the precipitate, washing it, and drying it to obtain a precursor; S3, mixing the precursor with selenium powder and performing selenization / carbonization treatment.

2. The preparation method according to claim 1, characterized in that: The carbon-sulfur source is selected from at least one of alkyl sulfonate sodium salt, thiocyanate and diallyl sulfide.

3. The preparation method according to claim 1 or 2, characterized in that: The carbon-sulfur source is sodium alkyl sulfonate; and / or the molar ratio of the molybdenum trioxide to the carbon-sulfur source is 1:1.5-6; And / or, the solvent is water; and / or, the mass ratio of the molybdenum trioxide to the solvent is 1:150-250.

4. The preparation method according to claim 1, characterized in that: In step S1, the mixing process is magnetic stirring; the conditions of the magnetic stirring include: a stirring time of 20 to 40 minutes and a stirring speed of 200 to 400 r / min; and / or, the hydrothermal treatment is carried out in a polytetrafluoroethylene reactor; and / or, the conditions of the hydrothermal treatment include: a temperature of 160-200° C. and a time of 6-12 h; And / or, in step S2, the washing liquid used for washing is selected from anhydrous ethanol and / or water; And / or, the drying conditions include: temperature of 50-70°C and time of 18-36h; And / or, in step S3, the selenization / carbonization treatment includes: mixing selenium powder with the precursor and then subjecting the mixture to high temperature treatment; the high temperature treatment is carried out under a protective atmosphere; the temperature of the high temperature treatment is 400-600°C, and the time of the high temperature treatment is 1-3 hours.

5. A negative electrode active material, characterized in that: The negative electrode active material is prepared according to the method according to any one of claims 1 to 4.

6. The negative electrode active material according to claim 5, characterized in that The negative electrode active material comprises a MoSe2 / MoS2@C composite material; the MoSe2 / MoS2@C composite material has a flower-like structure formed by stacking a plurality of lamellar structures; The sheet structure is formed by stacking a number of porous nanosheets; The porous nanosheet includes a carbon material middle layer, a first heterojunction MoSe2 / MoS2 layer coated on one side of the carbon material middle layer, and a second heterojunction MoSe2 / MoS2 layer coated on the other side of the carbon material middle layer.

7. The negative electrode active material according to claim 6, characterized in that: The specific surface area of ​​the MoSe2 / MoS2@C composite material is 150~190m 2 / g.

8. The negative electrode active material according to claim 6, characterized in that The porous nanosheet has a sheet diameter of 1 to 3 μm; And / or, the thickness of the porous nanosheet is 20-40 nm; And / or, the pore size of the porous nanosheet is 20-30 nm; And / or, the porosity of the porous nanosheet is 15-30%.

9. The negative electrode active material according to claim 6, characterized in that: Based on the total mass of the MoSe2 / MoS2@C composite material, the total content of the heterojunction MoSe2 / MoS2 first layer and the heterojunction MoSe2 / MoS2 second layer is 70-90wt%.

10. A negative electrode plate, characterized in that: The negative electrode sheet comprises a current collector and a negative electrode material disposed on a surface of the current collector, wherein the negative electrode material comprises the negative electrode active material according to any one of claims 5 to 9.

11. A battery, characterized in that: The battery comprises the negative electrode sheet according to claim 10.