Preparation method of iron-based Prussian blue material and application of iron-based Prussian blue material in sodium battery electrode material
Through the high-speed mixing and sodium citrate control method of collision reactor, the initial capacity loss and cycle attenuation of iron-based Prussian blue material in sodium ion batteries was solved, and efficient and stable performance of the positive electrode material of sodium ion battery was achieved.
Patent Information
- Application Number
- CN202410985931.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-12-06
AI Technical Summary
The existing iron-based Prussian blue material has problems of initial capacity loss and long-cycle capacity attenuation in sodium ion batteries, and the preparation process is low, which is not conducive to industrial production.
High-speed mixing is adopted for collision reactor, and the high-speed shear force of microfluidics is reduced [Fe(CN)6]3-/4-defects and coordination water molecules are improved, and the crystallinity and structural stability of the material are used. Sodium acid is used as a chelating agent to control the nucleation and crystallization process.
It realizes an efficient, controllable synthetic iron Prussian blue material with uniform morphology and size, which significantly improves its sodium storage performance and structural stability, and can maintain good cycling stability under high current density.
Smart Images

Figure CN119080024A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of preparation of iron-based Prussian blue materials, and specifically to a method for preparing an iron-based Prussian blue material and its application in sodium ion battery electrode materials. Background Art
[0002] The limited reserves and high price of lithium restrict the sustainable large-scale application of lithium-ion batteries (LIBs). Sodium is an ideal resource to replace lithium because it is abundant, cheap, and in the same main group as lithium. Its physical and chemical properties are similar. In addition, sodium-ion batteries (SIBs) will not catch fire or explode under extreme conditions such as puncture, extrusion, and overcharging. They are safer and more suitable for large-scale energy storage systems. However, since the ionic radius of sodium is much larger than that of lithium, many cathode materials that perform well in LIBs cannot perform equally well in SIBs. Therefore, synthesizing new electrode materials based on the characteristics of SIBs is crucial for the development of SIBs.
[0003] Prussian blue analogs (PBAs) have an open three-dimensional framework structure, low cost, easy preparation, environmental friendliness, and high theoretical capacity advantages (such as Na2Fe[Fe(CN)6] is 170.7 mAh / g), making them the choice of commercial SIBs cathode materials. However, PBAs have problems of initial capacity loss and severe long-cycle capacity decay, which is due to the fact that [Fe(CN)6] 3- / 4- Defects, coordinated water molecules and dissolution of transition metals. Prussian blue compounds (PBAs) contain a large number of lattice water molecules and [Fe(CN)6] vacancies, which not only affect their electrochemical performance, but also cause initial capacity loss and serious long-cycle capacity decay problems, and lead to the collapse of the skeleton structure and lattice disorder during the cycle. As stated in "Research Progress of Prussian Blue and Prussian Blue Compound Materials in Sodium Ion Batteries" published by Li Huan et al. in Materials Guide, this defect limits the application of Prussian blue and its analogs.
[0004] In order to improve the cyclability and rate performance of PBAs, various adjustment strategies have been developed from the aspects of the bulk and interface of the materials in the existing means.
[0005] To date, many studies have focused on minimizing the concentration of [Fe(CN)6] vacancies and coordinated water in the PBAs lattice from four perspectives. First, the number of [Fe(CN)6] vacancies and coordinated water can be limited by the slow nucleation rate of the single iron source method. Second, additives such as polyvinylpyrrolidone (PVP) soluble polymers or surfactants can cover Prussian blue micronuclei or small particles during the nucleation process to reduce surface tension and temporarily maintain their stability in solution, ensuring the growth of high-quality, low-vacancy unit cells, and can act as a protective agent to prevent acid chemical etching. Third, chelating agents such as citrate, oxalate or ethylenediaminetetraethylene glycolate are added. These chelating agents can first complex metal ions to form a "chelator-metal ion" buffer pool, and then [Fe(CN)6] 4– When added to the solution, they can slowly capture metal ions from the buffer pool and then slowly nucleate and crystallize. Because they can significantly slow down crystallization, they effectively inhibit the formation of [Fe(CN)6] defects. However, the PBAs particles formed under the action of chelating agents are usually not standard cubic blocks, and the agglomeration between particles is more serious. Fourth, during the synthesis process, high concentrations of sodium salts (such as NaCl and sodium citrate) are added to increase the Na content in the lattice, thereby preventing Fe 2+ Or oxidation of FeII and maintaining high Na content to maintain charge balance. Huang et al. used sodium citrate as a chelating agent. During the reaction, citrate ions complexed with ferrous ions. When ferrocyanide ions were added to the solution, citrate ions slowly released ferrous ions. Ferrous ions and ferrocyanide ions slowly nucleated, crystallized, and grew, and finally obtained 2-micron-sized Prussian blue monodisperse particles; and coated the surface of Prussian blue with a layer of polypyrrole. Polypyrrole can be used as a protective layer to prevent the decomposition of the Prussian blue framework, and can also be used as a conductive layer to increase the conductivity of the material and effectively improve the rate performance of the material. However, this work only used a method to inhibit nucleation, and there are still a small amount of [Fe(CN)6] defects and coordinated water inside the material; and the subsequent surface coating of polypyrrole will make the reaction steps lengthy, which is not conducive to industrial production and increases production costs (Tang, Y.; Zhang, W.; Xue, L.; Ding, X.; Wang, T.; Liu, X.; Liu, J.; Li, X.; Huang, Y., Polypyrrole-Promoted Superior Cyclability and Rate Capability of NaxFe[Fe(CN)6] Cathodes for Sodium-Ion Batteries. J. Mater. Chem. A4 (2016) 6036–6041. http: / / dx.doi.org / 10.1039 / c6ta00876c.).
[0006] In addition, the existing research ideas for reducing the concentration of [Fe(CN)6] vacancies and coordinated water in the PBAs lattice are to inhibit the formation of [Fe(CN)6] defects and avoid PBAs crystal agglomeration through slow nucleation and crystallization, which has low industrial production efficiency and is not conducive to industrial application. Summary of the invention
[0007] The purpose of the present invention is to overcome the shortcomings and deficiencies of the prior art and to provide an iron-based Prussian blue material, a preparation method and an application thereof.
[0008] To achieve the above object, the first aspect of the present invention is to provide a method for preparing an iron-based Prussian blue material, comprising the following steps:
[0009] S1: preparing a ferrous sulfate solution and a sodium ferrocyanide solution, adding a chelating agent and a reducing agent to the ferrous sulfate solution to obtain a solution A, and adding a chelating agent to the sodium ferrocyanide solution to obtain a solution B;
[0010] Sodium citrate was selected as the chelating agent;
[0011] S2: A collision-type reactor is used for reaction, wherein the collision-type reactor includes two constant flow pumps, two raw material tanks, a "T"-shaped micro-mixing chamber, a product tank and a pipeline, wherein the "T"-shaped micro-mixing chamber includes two coaxially oppositely arranged inlets and an outlet, the two raw material tanks are respectively connected to the two inlets through pipelines provided with constant flow pumps, and the outlet is connected to the product tank;
[0012] Step S1: The prepared solution A and solution B are placed in two raw material tanks respectively, and two constant flow pumps are used to control the ferrous sulfate solution and the sodium ferrocyanide solution to enter the "T"-shaped micro-mixing chamber through two oppositely arranged inlets for high-speed impact mixing, and then flow from the outlet to the product tank to obtain a suspension;
[0013] S3: The suspension obtained in step S2 is first stirred under a nitrogen atmosphere, then aged, and finally washed and dried to obtain an iron-based Prussian blue material.
[0014] In the preparation method of iron-based Prussian blue of the present invention, in step S1, the concentration of ferrous sulfate solution is 0.02-0.1 mol / L, and the concentration of sodium ferrocyanide solution is 0.02-0.1 mol / L. For example, the concentrations of ferrous sulfate solution and sodium ferrocyanide solution can be set to 0.02 mol / L, 0.04 mol / L, 0.06 mol / L, 0.08 mol / L and 0.1 mol / L, wherein the optimal concentrations of ferrous sulfate solution and sodium ferrocyanide solution are 0.06 mol / L and 0.04 mol / L, respectively.
[0015] In the preparation method of iron-based Prussian blue of the present invention, in step S1, 5-10 g of chelating agent sodium citrate is added to every 100 mL of ferrous sulfate solution; 5-10 g of chelating agent sodium citrate is added to every 100 mL of sodium ferrocyanide solution. For example, the mass of sodium citrate added to each of the two raw material solutions can be set to 2.5 g, 5 g, 7.5 g and 10 g, wherein the optimal amount of sodium citrate added is 7.5 g.
[0016] In the preparation method of iron-based Prussian blue described in the present invention, in step S1, 1-5 g of ascorbic acid, a reducing agent, is added to every 100 mL of ferrous sulfate solution, for example, 1 g, 2 g, 3 g, 4 g and 5 g, wherein the optimal amount of ascorbic acid added is 2 g.
[0017] In the method for preparing iron-based Prussian blue of the present invention, in step S2, two constant flow pumps control the volume flow ratio of sulfur solution A and solution B to be 1:1, and the flow rate of a single constant flow pump is 25-200 mL / min. For example, the volume flow rate of a single constant flow pump can be set to 25 mL / min, 50 mL / min, 100 mL / min, 150 mL / min and 200 mL / min. The optimal volume flow rate of a single pump is 150 mL / min.
[0018] In the preparation method of the iron-based Prussian blue of the present invention, in step S3, the mixture is first stirred under nitrogen for 2-10 hours and then aged for 6-18 hours. For example, the stirring time under nitrogen protection can be 2 hours, 4 hours, 6 hours, 8 hours and 10 hours, wherein the optimal stirring time is 6 hours. The further aging time can be 6 hours, 9 hours, 12 hours, 15 hours and 18 hours, wherein the optimal aging time is 12 hours.
[0019] In step S3, after aging, the obtained solid is washed with water and ethanol three times each.
[0020] The second aspect of the present invention is to provide an iron-based Prussian blue material prepared by the preparation method as described above.
[0021] The particle size of the iron-based Prussian blue material is 1.0-1.5 μm.
[0022] The third aspect of the present invention is to provide an application of the iron-based Prussian blue material as described above as a positive electrode material for a sodium ion battery.
[0023] The present invention aims to reduce the [Fe(CN)6] 3- / 4-In order to solve the problems of defects, coordinated water molecules and morphology that cannot be accurately controlled, by adding a chelating agent and using a collision reactor for reaction, which is completely different from the idea of controlling slow nucleation and crystallization in the prior art, the present invention allows the raw materials to be mixed by high-speed collision in a "T"-shaped micro-mixing chamber, and for the first time uses the high-speed shear force of microfluids to improve the crystallinity of iron-based Prussian blue, reduce the content of crystal water and vacancy, and very cleverly reduce various defects in the material.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. The present invention uses a collision reactor to coaxially collide two reaction liquids at high speed to enhance the phase transfer and micro-mixing of the fluids, thereby achieving efficient and controllable synthesis of an iron-based Prussian blue material with uniform morphology and size and excellent electrochemical performance.
[0026] 2. The present invention is the first to use the high-speed shear force of microfluids to increase the crystallinity of iron-based Prussian blue and reduce the content of crystal water and vacancy, thereby significantly improving the sodium storage performance and structural stability of the material.
[0027] 3. The present invention strengthens fluid micromixing through high-speed collision, thereby achieving the regulation of the Prussian blue phase. It is found for the first time that high impact velocity can promote the synthesis of cubic iron-based Prussian blue, while low-speed impact (conventional stirring reaction) can only synthesize monoclinic iron-based Prussian blue with poor structural stability.
[0028] 4. The high-speed collision synthesis of iron-based Prussian blue of the present invention is a controllable and efficient technology capable of large-scale production. A single reactor can produce 10 tons of products at the beginning of the year, and by scaling up the quantity, it can achieve an annual output of 100 tons of iron-based Prussian blue powder.
[0029] 5. The iron-based Prussian blue material obtained in the present invention can be directly used as a positive electrode material for SI Bs. The iron-based Prussian blue material prepared in one embodiment of the present invention has a specific capacity of up to 125 mAh / g at a current density of 0.1C (1C=170 mA / g). When the current density is increased to a high current density of 20C, the specific capacity is still 96.7 mAh / g. After 5000 cycles at 10C, the capacity attenuation rate is 75%, showing good cycle stability performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, without paying creative labor, other drawings obtained based on these drawings still belong to the scope of the present invention.
[0031] Figure 1 : A schematic diagram of a collision reactor used in a laboratory in some embodiments of the present invention;
[0032] Figure 2 : XRD patterns of the iron-based Prussian blue materials prepared in Examples 1 and 2;
[0033] Figure 3 : TGA graph of the iron-based Prussian blue material prepared in Examples 1 and 2;
[0034] Figure 4 : SEM images and TEM images of the iron-based Prussian blue materials prepared in Examples 1 and 2; (a) is the SEM image of MISR-25, (b) MISR-50, (c) MISR-100, (d) MISR-200, (e) is the SEM image of MISR-150; (f) TEM of MISR-150;
[0035] Figure 5 : XPS and FTIR images of the iron-based Prussian blue material prepared in Example 1; (a) is the XPS total spectrum; (b) is the C spectrum; (c) is the Fe spectrum; (d) is the FTIR spectrum;
[0036] Figure 6 : Electrochemical impedance diagrams of the iron-based Prussian blue materials prepared in Examples 1 and 2; (a) is the initial impedance diagram of the synthesized materials at different volume flow rates; (b) is the impedance diagram after 1000 cycles;
[0037] Figure 7 : The battery performance of the iron-based Prussian blue material prepared in Examples 1 and 2, wherein:
[0038] (a) The first cycle charge and discharge curve of the iron-based Prussian blue material at a current density of 0.1C
[0039] (b) Rate performance diagram of iron-based Prussian blue material at different current densities;
[0040] (c) Cyclic stability performance diagram of iron-based Prussian blue material at 1C current density;
[0041] (d) Cyclic stability performance diagram of iron-based Prussian blue material at 10C current density;
[0042] Figure 8 :(a) is a charge-discharge curve diagram of different current densities of the iron-based Prussian blue material prepared in Example 1; (b) is a charge-discharge curve diagram of different cycles of the iron-based Prussian blue material prepared in Example 1; (c) capacitance contribution of the iron-based Prussian blue material prepared in Example 1; (d) XRD diagram of the iron-based Prussian blue material prepared in Example 1 after different cycles;
[0043] Fig. 9 : SEM images of the iron-based Prussian blue material prepared in Example 1 after different cycles; (a) and (b) are the morphology images of the material after 3000 cycles; (c) and (d) are the morphology images of the material after 5000 cycles;
[0044] Fig.10 : The battery performance of the iron-based Prussian blue material prepared in Example 3, wherein:
[0045] (a) The first cycle charge and discharge curve of the iron-based Prussian blue material at a current density of 0.1C
[0046] (b) Rate performance diagram of iron-based Prussian blue material at different current densities;
[0047] (c) Cyclic stability performance diagram of iron-based Prussian blue material at 1C current density;
[0048] (d) Cyclic stability performance diagram of iron-based Prussian blue material at 10C current density;
[0049] Fig.11 : The battery performance of the iron-based Prussian blue material prepared in Example 4, wherein:
[0050] (a) The first cycle charge and discharge curve of the iron-based Prussian blue material at a current density of 0.1C
[0051] (b) Rate performance diagram of iron-based Prussian blue material at different current densities;
[0052] (c) Cyclic stability performance diagram of iron-based Prussian blue material at 1C current density;
[0053] (d) Cyclic stability performance diagram of iron-based Prussian blue material at 10C current density
[0054] Fig.12 : XRD patterns of the iron-based Prussian blue materials prepared in Comparative Examples 1 and 2;
[0055] Fig.13 : SEM images of the iron-based Prussian blue materials prepared in Comparative Examples 1 and 2; (a) STR-5; (b) STR-10; (c) STR-20; (d) STR-30; (e) STR-50; (f) is the SEM image of the STR-20 material enlarged to 1um
[0056] Fig.14 : Battery performance of the iron-based Prussian blue material prepared in Comparative Examples 1 and 2, wherein:
[0057] (a) Rate performance diagram of iron-based Prussian blue material at different current densities;
[0058] (b) Cyclic stability performance diagram of iron-based Prussian blue material at 10C current density;
[0059] Fig.15 : The electrochemical properties and battery performance of the iron-based Prussian blue materials prepared in Example 1 and Comparative Example 1, wherein:
[0060] (a) CV graphs of the iron-based Prussian blue materials prepared in Example 1 and Comparative Example 1;
[0061] (b) The first cycle charge and discharge curves of the iron-based Prussian blue materials prepared in Example 1 and Comparative Example 1;
[0062] (c) Rate performance diagram of the iron-based Prussian blue material prepared in Example 1 and Comparative Example 1;
[0063] (d) Cycling of the iron-based Prussian blue materials prepared in Example 1 and Comparative Example 1 at a current density of 10C. DETAILED DESCRIPTION
[0064] In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention will be further described in detail below with reference to the accompanying drawings.
[0065] The present invention provides a method for preparing an iron-based Prussian blue material, which comprises the following steps:
[0066] S1: preparing a ferrous sulfate solution and a sodium ferrocyanide solution, adding a chelating agent and a reducing agent to the ferrous sulfate solution to obtain a solution A, and adding a chelating agent to the sodium ferrocyanide solution to obtain a solution B;
[0067] Sodium citrate was selected as the chelating agent;
[0068] S2: A collision-type reactor is used for reaction, wherein the collision-type reactor includes two constant flow pumps, two raw material tanks, a "T"-shaped micro-mixing chamber, a product tank and a pipeline, wherein the "T"-shaped micro-mixing chamber includes two coaxially oppositely arranged inlets and an outlet, the two raw material tanks are respectively connected to the two inlets through pipelines provided with constant flow pumps, and the outlet is connected to the product tank;
[0069] Step S1: The prepared solution A and solution B are placed in two raw material tanks respectively, and two constant flow pumps are used to control the ferrous sulfate solution and the sodium ferrocyanide solution to enter the "T"-shaped micro-mixing chamber through two oppositely arranged inlets for high-speed impact mixing, and then flow from the outlet to the product tank to obtain a suspension;
[0070] S3: The suspension obtained in step S2 is first stirred under a nitrogen atmosphere, then aged, and finally washed and dried to obtain an iron-based Prussian blue material.
[0071] In some embodiments of the present invention, the following methods are used in the laboratory: Figure 1 The collision reactor shown is carried out, the raw material tank directly adopts a quantitative bottle or a beaker, the "T"-shaped micro-mixing chamber adopts a T-shaped micro-tee with a caliber of 1.2mm, the pipeline adopts a stainless steel capillary with an inner diameter of 0.6mm, and the product tank adopts a beaker equipped with a stirring device. The stirring and aging treatment of step S3 are directly carried out in the product tank. In other embodiments of the present invention, the reaction is amplified by an order of magnitude, the raw material tank adopts a stirring device or other holding container for industrial production, the "T"-shaped micro-mixing chamber adopts a device with an appropriately enlarged size that can realize the high-speed collision of two solutions, the pipeline adopts a pipe fitting with an appropriately enlarged inner diameter, and the product tank adopts a holding container for industrial production to hold the suspension after the reaction. The stirring and aging treatment of step S3 can be directly carried out in the product tank, or transferred to a stirring device for industrial production.
[0072] The present invention controls the flow rates of solution A and solution B respectively by means of a constant flow pump, so as to realize high-speed collision of solution A and solution B in a "T"-shaped micro-mixing chamber. The flow rates of solution A and solution B under the control of the constant flow pump are Q A and Q B The inner cross-sectional area of the stainless steel capillary is A, and the formula The flow rate v of solution A and solution B entering the "T"-shaped micro-mixing chamber can be calculated. A and ν B , the theoretical collision velocity is (ν A +ν B ).
[0073] In the following embodiments, the Figure 1 The collision reactor shown is carried out. In step S2, two constant flow pumps control the volume flow ratio of solution A and solution B to be 1:1, and the flow rate of a single constant flow pump is 25-200 mL / min. Since the inner diameter of the stainless steel capillary used is 0.6 mm, the corresponding impact velocity of the single fluid is 1.48-11.84 m / s, and the relative velocity range of the two fluids is 2.96-23.68 m / s, which can form a high-speed collision.
[0074] Example 1
[0075] (1) First, prepare 100 mL of a 0.06 mol / L ferrous sulfate solution, and then add 7.5 g of sodium citrate and 2 g of ascorbic acid thereto to obtain a mixed solution "A"; prepare 100 mL of a 0.04 mol / L sodium ferrocyanide solution, and also add 7.5 g of sodium citrate thereto;
[0076] (2) The two solutions were transferred to the corresponding two raw material solutions respectively, and the flow rates of the two constant flow pumps were set to 150 mL / min. The two solutions were subjected to high-speed collision and microscopic mixing in the "T"-shaped tee of the collision reactor to obtain a suspension at the tee outlet.
[0077] (3) The obtained suspension was then placed in a stirred tank reactor for stirring for 6 h, then aged at room temperature for 12 h, centrifuged, washed with water 3 times, washed with alcohol 3 times, and then vacuum dried at 120 °C for 12 h to obtain an iron-based Prussian blue material (sample labeled "MISR-150").
[0078] Example 2
[0079] In this implementation case, we investigated the effect of the volume flow rate of a horizontal flow pump on the properties of an iron-based Prussian blue material.
[0080] Except for replacing the volume flow rates of the two constant flow pumps in Implementation Example 1 to 25 mL / min and 25 mL / min (the sample is labeled "MISR-25"); or setting them to 50 mL / min and 50 mL / min (the sample is labeled "MISR-50"), or setting them to 100 mL / min and 100 mL / min (the sample is labeled "MISR-100"), or setting them to 200 mL / min and 200 mL / min (the sample is labeled "MISR-200"), the other operating conditions remain unchanged, thereby obtaining iron-based Prussian blue materials prepared at different flow rates.
[0081] Example 3
[0082] In this embodiment, we investigated the effect of the addition amount of sodium citrate on the properties of iron-based Prussian blue material.
[0083] (1) First, prepare 100 mL of a 0.06 mol / L ferrous sulfate solution, and then add 2.5 g, 5.0 g, 7.5 g, or 10.0 g of sodium citrate and 2 g of ascorbic acid thereto to obtain a mixed solution "A"; prepare 100 mL of a 0.04 mol / L sodium ferrocyanide solution, and add 2.5 g, 5.0 g, 7.5 g, or 10.0 g of sodium citrate thereto respectively;
[0084] (2) The two solutions were transferred to the corresponding two raw material solutions respectively, and the flow rates of the two constant flow pumps were set to 150 mL / min. The two solutions were subjected to high-speed collision and microscopic mixing in the "T"-shaped tee of the collision reactor to obtain a suspension at the tee outlet.
[0085] (3) The obtained suspension was then placed in a stirred tank reactor for stirring for 6 h, then aged at room temperature for 12 h, centrifuged, washed with water 3 times, washed with alcohol 3 times, and then vacuum dried at 120°C for 12 h to obtain an iron-based Prussian blue material. Among them, samples in which 2.5 g, 5.0 g, 7.5 g, and 10.0 g of sodium citrate were added to ferrous sulfate solution and sodium ferrocyanide solution, respectively, were labeled "SC-2.5", "SC-5.0", "SC-7.5", and "SC-10.0", respectively.
[0086] Example 4
[0087] In this implementation case, we investigated the effect of aging temperature on the properties of iron-based Prussian blue materials.
[0088] (1) First, prepare 100 mL of a 0.06 mol / L ferrous sulfate solution, and then add 7.5 g of sodium citrate and 2 g of ascorbic acid thereto to obtain a mixed solution "A"; prepare 100 mL of a 0.04 mol / L sodium ferrocyanide solution, and also add 7.5 g of sodium citrate thereto;
[0089] (2) The two solutions were transferred to the corresponding two raw material solutions respectively, and the flow rates of the two constant flow pumps were set to 150 mL / min. The two solutions were subjected to high-speed collision and microscopic mixing in the "T"-shaped tee of the collision reactor to obtain a suspension at the tee outlet.
[0090] (3) The obtained suspension was then placed in a stirred tank reactor for stirring for 6 h, and then aged at 25°C, 60°C, and 80°C for 12 h, respectively. It was then centrifuged, washed with water 3 times, washed with alcohol 3 times, and then vacuum dried at 120°C for 12 h to obtain an iron-based Prussian blue material (the samples were labeled "AT-25", "AT-60", and "AT-80").
[0091] Comparative Example 1: Iron-based Prussian blue material prepared in a stirred tank reactor
[0092] (1) First, prepare 100 mL of a 0.06 mol / L ferrous sulfate solution, and then add 7.5 g of sodium citrate and 2 g of ascorbic acid thereto to obtain a mixed solution "A"; prepare 100 mL of a 0.04 mol / L sodium ferrocyanide solution, and add 7.5 g of sodium citrate thereto;
[0093] (2) The two solutions were transferred to the two corresponding raw material tanks respectively, and the flow rates of the two constant flow pumps were set to 20 mL / min. The solutions flowed directly into the stirred tank reactor through the stainless steel pipe.
[0094] (3) The suspension was stirred in a stirred tank reactor for 6 h, then aged at room temperature for 12 h, centrifuged, washed with water 3 times, washed with alcohol 3 times, and then vacuum dried at 120 °C for 12 h to obtain an iron-based Prussian blue material (sample labeled "STR-20").
[0095] Comparative Example 2
[0096] In this implementation case, we investigated the effect of changing the volume flow rate of a constant flow pump on the properties of an iron-based Prussian blue material.
[0097] Except that the volume flow rates of the two constant flow pumps in Comparative Example 1 were replaced with 5 mL / min and 5 mL / min respectively (the sample was labeled as "STR-5"); or were set to 10 mL / min and 10 mL / min respectively (the sample was labeled as "STR-10"), or were set to 30 mL / min and 30 mL / min respectively (the sample was labeled as "STR-30"), or were set to 50 mL / min and 50 mL / min respectively (the sample was labeled as "STR-50"), the other operating conditions remained unchanged, thereby obtaining iron-based Prussian blue materials prepared at different flow rates.
[0098] Example 5: Preparation of Iron-based Prussian Blue Electrode
[0099] The iron-based Prussian blue powder, Ketjen black and polytetrafluoroethylene (PVDF) prepared by the method of Example 1-2 and Comparative Example 1-2 are put into a mortar in a mass ratio of 70:20:10, and after repeated sufficient grinding, an appropriate amount of N-methylpyrrolidone (NMP) is added, and then sufficient grinding is performed for 30 minutes to obtain a viscous slurry. The slurry is evenly coated on aluminum foil, dried at 80°C for 12 hours, and finally the electrode sheet is obtained by pressing. The electrode sheet is placed in a glove box (H2O<0.5ppm, O2<0.5ppm) to assemble the battery, and the electrode sheet coated with iron-based Prussian blue powder is used as the positive electrode, the sodium sheet is used as the counter electrode, the glass fiber is used as the diaphragm, and NaPF6 is used as the electrolyte for battery assembly. After the assembly is completed, the battery is left to stand for more than 10 hours to allow the electrolyte to fully infiltrate, and then the performance of the sodium ion battery is tested using the Xinwei battery system.
[0100] The following are the microscopic characterizations of iron-based Prussian blue materials by different means:
[0101] Figure 2 3 and 4. The XRD diagram of the iron-based Prussian blue material prepared in Examples 1 and 2 shows that in the "T"-shaped mixing chamber, as the flow rate of the constant flow pump increases, the iron-based Prussian blue material synthesized in the chamber gradually transforms from a monoclinic phase to a cubic phase, and the synthesized material has relatively good crystallinity on the (200), (220), and (400) crystal planes.
[0102] Figure 3This is the TGA graph of the iron-based Prussian blue material prepared in Examples 1 and 2. It can be seen from the figure that the elimination of water in the material is mainly in the three temperature ranges of 100°C, 200°C and 270°C, which correspond to adsorbed water, interstitial water and coordinated water, respectively. Among them, the MISR-150 material has less mass loss at the coordinated water at 270°C compared with other materials, indicating that there are fewer vacancy defects in the material.
[0103] Figure 4 ae are SEM images of the iron-based Prussian blue materials prepared in Examples 1 and 2. It can be seen from the figure that in the mixing chamber, as the volume flow rate of the constant flow pump is changed, the iron-based Prussian blue material synthesized changes from the initial agglomeration phenomenon and irregular morphology to Figure 4 a(MISR-25) gradually changes to a uniformly dispersed and regular cubic morphology Figure 4 e(MISR-150) and the grain size is 1 to 1.5um; in addition Figure 4 f is the TEM image of MISR-150 material, from which it can be seen that the grain size of the material is about 200nm.
[0104] Figure 5 The XPS graph of the iron-based Prussian blue material prepared in Example 1 is shown in the XPS total spectrum ( Figure 5 It can be seen from a) that the iron-based Prussian blue material is composed of five elements: Na, Fe, C, N, and O. Figure 5 b) shows that 284.8eV, 285.9eV, and 288.8eV correspond to CC bond, C≡N bond, and C=O bond, respectively; in the Fe spectrum ( Figure 5 c) It can be seen that 708.4eV, 721.0eV, 710.6eV, 723.4eV, 712.5eV, and 726.6eV correspond to Fe Ⅱ 2p 3 / 2 , Fe Ⅱ 2p 1 / 2 , Fe Ⅲ 2p 3 / 2 , Fe Ⅲ 2p 1 / 2 , Fe Ⅱ and Fe Ⅲ Satellite peaks. Figure 5 d is the FTIR graph of the iron-based Prussian blue material prepared in Example 1. It can be seen from the figure that the peaks at 451.3, 589.5, 1616.8, 2068.4, 3549.6, and 3617.8 cm -1 The corresponding positions are Fe-O, Fe-C≡N, OH, C≡N and OH bonds respectively.
[0105] Figure 61 and 2 are electrochemical impedance spectroscopy diagrams of the iron-based Prussian blue materials prepared in Examples 1 and 2. Figure 6 a is the initial impedance diagram of synthetic materials with different volume flow rates. In the Nernst diagram, it is usually low resistance at high frequency. The semicircle in the medium frequency region can correspond to the charge transfer resistance of Na ions, and the oblique line in the low frequency region can correspond to the diffusion of sodium ions in the electrode. It can be seen that no matter what volume flow rate the material has, the impedance in the medium and high frequency region is large. Figure 6 b is the impedance diagram of synthetic materials with different volume flow rates after 1000 cycles. It can be seen that the impedance has been significantly reduced compared to when there is no cycle; and the material with a higher synthetic volume flow rate has a smaller impedance after the cycle.
[0106] Figure 7 The battery performance of the iron-based Prussian blue material prepared in Examples 1 and 2. Figure 7 It can be seen from the graph that in the first charge-discharge curve at 0.1C, since MISR-25 is a monoclinic phase material, it has the highest initial discharge capacity (148 mAh / g). As the volume flow rate increases and the material gradually transforms to the cubic phase, the initial discharge capacity decreases, and MISR-150 still has a discharge capacity of 127.5 mAh / g. Figure 7 b is the rate performance diagram of the iron-based Prussian blue material at different current densities. It can be seen from the figure that although MISR-25 has a high specific capacity, the capacity decays quickly and cannot be maintained well, while MISR-150 still has a specific capacity of 96.7mAh / g at 20C, and can return to a small current density well after completing a high current density, showing good rate performance. Figure 7 cd are the charge and discharge curves of 1C and 10C current density respectively. It can be seen that the capacity decay of MISR-25 is very fast at both low and high current density, while the cubic phase material (STR-150) has excellent capacity retention rate at both high and low current density, and still has a capacity retention rate of 75% even after 5000 cycles at 10C.
[0107] Figure 8 a is a charge and discharge curve of the iron-based Prussian blue material prepared in Example 1 at different current densities, wherein the discharge specific capacities at current densities of 0.1C, 0.2C, 0.5C, 1C, 2C, 5C, 10C, 20C, and 30C are 127.5mAh / g, 118.2mAh / g, 113.7mAh / g, 110.5mAh / g, 108.2mAh / g, 104.6mAh / g, 101.0mAh / g, 96.7mAh / g, and 93.4mAh / g, respectively; Figure 8b is the charge-discharge curve of the iron-based Prussian blue material prepared in Example 1 at different cycles at 10C. It can be seen from the figure that as the number of cycles increases, the discharge specific capacity gradually decreases and polarization occurs; Figure 8 c is the capacitance contribution rate of the iron-based Prussian blue material prepared in Example 1. It can be seen that at 0.1 mv / s, the material has shown a relatively high capacitance contribution. As the scan rate continues to increase, the capacitance contribution also gradually increases. At 1 mv / s, the material reaches a capacitance contribution of 97.4%. In addition, Figure 8 d is the XRD pattern of the iron-based Prussian blue material prepared in Example 1 after 3000 and 5000 cycles. It can be seen that the material still has good crystallinity after multiple cycles, and the (200) and (400) crystal planes are well maintained.
[0108] Fig. 9 The SEM images of the iron-based Prussian blue material prepared in Example 1 at different cycle numbers are shown in FIG. Fig. 9 ab are the material morphology images after 3000 cycles; Fig. 9 cd is the material morphology after 5000 cycles; it can be seen that the material still maintains the cubic morphology after multiple cycles, and the morphological damage is not serious, which further shows that this material has excellent cycle stability.
[0109] Fig.10 The battery performance of the iron-based Prussian blue material prepared in Example 3 is shown in FIG. Fig.10 It can be seen from a that with the gradual addition of sodium citrate, the sodium storage capacity of the material is gradually increased. When it is increased to 7.5g, the material has the highest discharge capacity. When it is added to 10.0g, the specific capacity of the material decreases. This may be due to excessive chelation of the material caused by excessive sodium citrate, resulting in the material not showing excellent specific capacity. Fig.10 b is the rate performance diagram with different chelating agents added. It can be seen from the figure that when a small amount of sodium citrate is added (SC-2.5), the material decays quickly at different current densities and does not return to the specific capacity of small current density. Later, with the increase of chelating agent, the rate performance of the material is also greatly improved, and the optimal value is achieved when 7.5g of sodium citrate is added. Fig.10 cd are the cycle diagrams at 1C and 10C current densities respectively. It can be seen from the figure that the capacity of SC-2.5 material decays very rapidly regardless of whether it is cycled at a small current or a large current density. By further increasing the dosage of sodium citrate, the cycle stability of the material is also improved. The SC-7.5 material has a discharge specific capacity of 106.8mAh / g after 500 cycles at 1C, and also shows good cycle stability after 5000 cycles at a high current density of 10C.
[0110] Fig.11 The battery performance of the iron-based Prussian blue material prepared in Example 4 is shown in FIG. Fig.11 It can be seen from a that as the aging temperature gradually increases, the sodium storage capacity of the material has increased. The material aged at 80°C (AT-80) has the highest discharge capacity. Fig.11 As can be seen from the rate performance diagram b, with the increase of aging temperature, although the discharge specific capacity of the material has increased, its stability at different current densities decays too quickly, among which AT-80 has the worst rate performance. Fig.11 cd are the cycle diagrams of materials with different aging temperatures at current densities of 1C and 10C, respectively. It can be seen from the figure that with the increase of the aging temperature, the capacity decay of the material is very obvious regardless of whether it is cycled at large or small current density. This may be due to the change in temperature gradient, which causes the synthesized material to transform from a cubic monoclinic phase. The phase change experienced during the cycle is different, resulting in differences in cycle stability.
[0111] Fig.12 2 is the XRD diagram of the iron-based Prussian blue material prepared in Comparative Examples 1 and 2. It can be seen from the figure that no matter how the volume flow rate of the constant flow pump changes, the material synthesized by the stirred tank reactor appears as a monoclinic phase.
[0112] Fig.13 : SEM images of the iron-based Prussian blue materials prepared in Comparative Examples 1 and 2, Fig.13 ae are the SEM images of STR-5 to STR-50 respectively. It can be seen from the figures that no matter what volume flow rate is used, the material morphology after synthesis in the stirred tank reactor has obvious agglomeration phenomenon, and the morphology and size are not uniform. Fig.13 f is the SEM image of the STR-20 material magnified to 1um. It can be seen that the surface of the material presents a layered gradient. This may be due to the uneven chelation of sodium citrate, which leads to serious clustering. There is no regular cubic morphology of the material and the distribution is uneven.
[0113] Fig.14 : Battery performance of the iron-based Prussian blue material prepared in Comparative Examples 1 and 2, wherein: Fig.14 a is the rate performance diagram of the iron-based Prussian blue material at different current densities. It can be seen from the figure that the materials synthesized by various volume flow rates have a higher discharge specific capacity at a small current density. With the increase of volume flow rate, the specific capacity of the material has a certain improvement; but in terms of cycling at a current density of 10C (such as Fig.14 (b) The material synthesized by the STR method has a faster capacity decay in cycle performance.
[0114] Fig.15a is the CV graph of the iron-based Prussian blue material prepared in Example 1 and Comparative Example 1. It can be seen that there are a pair of redox peaks at voltages of 3.12V / 2.75V and 3.65V / 3.30V, respectively, corresponding to the high-spin iron (Fe HS ) and low-spin iron (Fe LS ). Fig.15 b is the first cycle charge and discharge curve of the iron-based Prussian blue material prepared in Example 1 and Comparative Example 1 at a current density of 0.1C. It can be seen from the figure that the discharge specific capacity of the STR-20 material is 138.7 mAh / g, and the discharge specific capacity of the MISR-150 material is 127.6 mAh / g. As for the rate performance diagrams of the two materials (such as Fig.15 c), although the discharge specific capacity of MISR-150 material is slightly worse than that of STR-20, it has less attenuation when cycling under different current densities, and can still return to low current after cycling at high current, while STR-20 cannot return to low current very well. In comparison, MISR-150 material is more excellent. Fig.15 d is the cycle performance diagram of the iron-based Prussian blue materials prepared in Example 1 and Comparative Example 1 at a current density of 10C. It can be seen from the figure that after 5000 cycles, the MISR-150 material still has a relatively high discharge specific capacity (80.15 mAh / g), while the capacity of the STR-20 material decays rapidly, with only 47.46 mAh / g after 5000 cycles.
[0115] The above disclosure is only the preferred embodiment of the present invention, which certainly cannot be used to limit the scope of the present invention. Therefore, equivalent changes made according to the claims of the present invention are still within the scope of the present invention.
Claims
1. A method for preparing an iron-based Prussian blue material, characterized in that The following steps are involved: S1: preparing a ferrous sulfate solution and a sodium ferrocyanide solution, adding a chelating agent and a reducing agent to the ferrous sulfate solution to obtain a solution A, and adding a chelating agent to the sodium ferrocyanide solution to obtain a solution B; Sodium citrate was selected as the chelating agent; S2: A collision reactor is used for the reaction, wherein the collision reactor includes two constant flow pumps, two raw material tanks, a "T"-shaped micro-mixing chamber, a product tank and a capillary tube, wherein the "T"-shaped micro-mixing chamber includes two coaxially oppositely arranged inlets and an outlet, the two raw material tanks are respectively connected to the two inlets through a capillary tube provided with a constant flow pump, and the outlet is connected to the product tank; Step S1: The prepared solution A and solution B are placed in two raw material tanks respectively, and two constant flow pumps are used to control the ferrous sulfate solution and the sodium ferrocyanide solution to enter the "T"-shaped micro-mixing chamber through two oppositely arranged inlets for high-speed impact mixing, and then flow from the outlet to the product tank to obtain a suspension; S3: The suspension obtained in step S2 is first stirred under a nitrogen atmosphere, then aged, and finally washed and dried to obtain an iron-based Prussian blue material.
2. The method for preparing an iron-based Prussian blue material according to claim 1, characterized in that: In step S1, the concentration of the ferrous sulfate solution is 0.02-0.1 mol / L, and the concentration of the sodium ferrocyanide solution is 0.02-0.1 mol / L.
3. The method for preparing an iron-based Prussian blue material according to claim 1, characterized in that: In step S1, 5-10 g of chelating agent sodium citrate is added to every 100 mL of ferrous sulfate solution; 5-10 g of chelating agent sodium citrate is added to every 100 mL of sodium ferrocyanide solution.
4. The method for preparing an iron-based Prussian blue material according to claim 1, characterized in that: In step S1, ascorbic acid is selected as a reducing agent; 1-5 g of ascorbic acid is added to every 100 mL of ferrous sulfate solution.
5. The method for preparing an iron-based Prussian blue material according to claim 1, characterized in that: In step S2, two constant flow pumps control the volume flow ratio of solution A and solution B to be 1:1, and the flow rate of a single constant flow pump is 25-200 mL / min.
6. The method for preparing an iron-based Prussian blue material according to claim 1, characterized in that: In step S3, the mixture is first stirred under nitrogen for 2-10 hours and then aged for 6-18 hours.
7. The method for preparing an iron-based Prussian blue material according to claim 1, characterized in that: In step S3, after aging, the obtained solid is washed with water and ethanol three times each.
8. An iron-based Prussian blue material obtained by the preparation method according to any one of claims 1 to 7.
9. The iron-based Prussian blue material according to claim 8, characterized in that: The particle size of the iron-based Prussian blue material is 1.0-1.5 μm.
10. Use of the iron-based Prussian blue material as claimed in claim 8 as a positive electrode material for a sodium ion battery.
Citation Information
Patent Citations
Method for quickly preparing Prussian blue analog with monoclinic structure
CN110451525A
Method for preparing Prussian blue analogue by microchannel reactor
CN113145040A
Preparation method of long-life iron-based Prussian blue positive electrode material
CN115108566A
Sodium-rich and low-water-content Prussian blue positive electrode material, preparation method thereof and sodium ion battery
CN117534088A
Method for regulating and controlling defect number and sodium content of manganese-based Prussian blue sodium ion battery positive electrode material
CN118125470A