An easily filled iron-based parahydrogen conversion catalyst, a preparation method thereof, and application in parahydrogen catalytic conversion

By preparing iron-based secondary hydrogen conversion catalyst, the problem of uneven particles and easy powderization of the catalyst at low temperature is solved, and the efficient filling and high conversion efficiency of the catalyst are achieved, and the pressure drop and bed flow resistance are reduced. The application requirements of hydrogen liquefaction systems.

CN118681604BActive Publication Date: 2024-11-12TECHNICAL INST OF PHYSICS & CHEMISTRY - CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411163618.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-12
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

The existing secondary hydrogen conversion catalysts have problems such as uneven particles, difficulty in filling, easy to wear, easy to powder, hinder gas flow, high pressure drop, and low heat transfer efficiency at low temperatures, and large catalyst size is not conducive to catalytic conversion.

Method used

Using a preparation method of an iron-based secondary hydrogen conversion catalyst, the pH is adjusted by adding alkali liquid to the iron salt solution under stirring to form a block catalyst precursor, and the particle size is 20-50 by spray granulation technology. Spherical catalyst, bonding binder to improve mechanical strength and catalytic activity.

Benefits of technology

The resulting catalyst has uniform particle size, easy to fill, high catalytic efficiency, reduced pressure, small bed flow resistance, high mechanical strength, and is not easy to powder. It is suitable for plate-fin heat exchangers, significantly meeting the actual application needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118681604B_ABST
    Figure CN118681604B_ABST
Patent Text Reader

Abstract

The invention discloses an easy-to-fill iron-based normal para-hydrogen conversion catalyst and its preparation method and application in normal para-hydrogen catalytic conversion. The preparation process of the iron-based normal para-hydrogen conversion catalyst is as follows: under stirring, alkali solution is added dropwise to an iron salt solution or an iron salt solution doped with other metal salts to adjust the pH to 8.5-10.5, and the solution is allowed to stand for aging. After aging, the pH is neutralized with a regulator to 6.5-7.5, and a bulk normal para-hydrogen conversion catalyst precursor is obtained by washing and drying; the bulk normal para-hydrogen conversion catalyst precursor is crushed into a fine powder, mixed with a binder, and then put into a granulator in batches for spray granulation, and dried and sieved to obtain a spherical or spherical catalyst with a particle size of 20-50 mesh; wherein the mass ratio of the fine powder to the binder is 1:0.03-0.35; the iron-based normal para-hydrogen conversion catalyst is a mixture of α-Fe2O3 and FeOOH doped or not doped with other metal elements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of hydrogen liquefaction, and more specifically, to an easily-filled iron-based para-hydrogen conversion catalyst, a preparation method thereof, and an application thereof in the catalytic conversion of para-hydrogen. Background Art

[0002] With the growing demand for new environmentally friendly energy, the field of hydrogen energy is developing rapidly. The large-scale transportation and storage of hydrogen energy has become an important challenge restricting the development of hydrogen energy. Liquid hydrogen is one of the main storage methods of hydrogen energy and is also an efficient liquid fuel. It is widely used in many fields such as chemical industry and aerospace. Molecular hydrogen exists in two forms: orthohydrogen with the same nuclear spin direction and parahydrogen with the opposite nuclear spin direction. At room temperature, the orthohydrogen content in hydrogen is 75% and the parahydrogen content is 25%. As the temperature decreases, the parahydrogen equilibrium content gradually increases. At liquid hydrogen temperature, the parahydrogen equilibrium content can reach 99.8%. The conversion of orthohydrogen to parahydrogen is an exothermic reaction, and it proceeds slowly and spontaneously. When orthohydrogen in liquid hydrogen is converted to parahydrogen, the liquid hydrogen evaporates due to heat release, which poses a great safety hazard to the storage and transportation of liquid hydrogen. Therefore, it is necessary to carry out catalytic conversion of orthohydrogen during the hydrogen liquefaction process.

[0003] Research on catalytic materials for the conversion of para-hydrogen at low temperatures has mostly focused on the conversion rate of para-hydrogen, while ignoring the problems of uneven particles in catalytic materials in practical applications, such as difficulty in filling well in the slender and narrow heat exchange channels of plate-fin heat exchangers, easy wear, easy pulverization, obstruction of gas flow, high pressure drop, low heat transfer efficiency, etc. Moreover, in the currently published reports on catalysts for the conversion of para-hydrogen, the catalyst size is relatively large, which is not conducive to the catalytic conversion of para-hydrogen. Even if smaller catalysts can be collected, the yield is usually low and the mechanical properties are low.

[0004] In order to realize the efficient application of normal parahydrogen catalyst, it is urgent to develop a preparation method of a normal parahydrogen conversion catalyst with high catalytic activity, stable catalytic activity, easy filling, high mechanical strength and not easy to pulverize, so as to meet the practical application requirements. At present, the method that is more effective to improve the above problems is to prepare a supported catalyst, and use a carrier with excellent mechanical properties to support the active catalyst to improve the problems of easy wear and easy pulverization, and the supported catalyst particles are uniform, which can also reduce the flow resistance of the catalyst bed, such as CN 112044457 A. However, the supported catalyst is limited by the pore size of the carrier, so that the supported catalyst particle size is required to be larger, which is not conducive to the improvement of catalytic activity.

[0005] Therefore, the development of a non-supported para-hydrogen conversion catalyst is very important in the field of para-hydrogen conversion. Summary of the invention

[0006] In order to solve the above problems, the first object of the present invention is to provide a method for preparing an iron-based para-hydrogen conversion catalyst. The preparation method is simple to operate, has a large output, and a high yield. The obtained iron-based para-hydrogen conversion catalyst has a uniform particle size and a small size. It is loaded in a plate-fin heat exchanger to carry out a para-hydrogen catalytic conversion reaction. It has the characteristics of easy filling, high para-hydrogen conversion efficiency, low pressure drop, small bed flow resistance, high mechanical strength, and not easy to pulverize, and can better meet the actual application needs.

[0007] The second object of the present invention is to provide a method for preparing an iron-based ortho-parahydrogen conversion catalyst.

[0008] The third object of the present invention is to provide the use of the iron-based para-hydrogen conversion catalyst as described above in the catalytic conversion of para-hydrogen.

[0009] In order to achieve the above first object, the present invention adopts the following technical scheme:

[0010] The present invention discloses a method for preparing an iron-based ortho-parahydrogen conversion catalyst, comprising the following steps:

[0011] 1) adding alkaline solution dropwise to an iron salt solution or an iron salt solution doped with other metal salts under stirring to adjust the pH to 8.5-10.5, and aging the solution. After aging, neutralizing the solution with a regulator to a pH of 6.5-7.5, and washing and drying the solution to obtain a blocky ortho-parahydrogen conversion catalyst precursor.

[0012] 2) crushing the blocky n-parahydrogen conversion catalyst precursor into fine powder, mixing it with a binder and then feeding it into a granulator in batches for spray granulation, drying and sieving to obtain a spherical or quasi-spherical catalyst with a particle size of 20-50 mesh;

[0013] Wherein, the mass ratio of the fine powder to the binder is 1:0.03-0.35;

[0014] The iron-based parahydrogen conversion catalyst is a mixture of α-Fe2O3 and FeOOH doped or not doped with other metal elements.

[0015] The invention provides a para-hydrogen conversion catalyst suitable for filling in a plate-fin heat exchanger of a hydrogen liquefaction system. After the catalyst is granulated by secondary molding, the catalyst has a more regular shape, a smoother surface, and a more uniform particle size, and is easy to roll, fill and stack in a narrow test tube. The particle size is smaller, 20-50 mesh, and the reaction activity is stronger. At the same time, the mechanical strength of the sphere can be ensured. Finally, the packing density of the iron-based para-hydrogen conversion catalyst is controlled at 0.9-1.4 g / cc, and the average crushing force value of a single particle is 5-7 N / particle. Such a catalyst is not easy to be pulverized at a high air velocity, and the bed flow resistance caused during the test is smaller, which can better meet the actual application needs.

[0016] Furthermore, the iron salt in the iron salt solution is selected from at least one of iron nitrate, iron chloride and iron sulfate;

[0017] The other metal salt is selected from at least one of cobalt salt, cerium salt, nickel salt and aluminum salt; for example, it can be cobalt nitrate, cobalt sulfate, cobalt acetate, cerium nitrate, cerium sulfate, cerium acetate, nickel nitrate, nickel sulfate, nickel acetate, aluminum nitrate, aluminum sulfate, aluminum acetate, etc. Depending on the doped metal, a mixture of cobalt-doped α-Fe2O3 and FeOOH, a mixture of cerium-doped α-Fe2O3 and FeOOH, a mixture of nickel-doped α-Fe2O3 and FeOOH, and a mixture of aluminum-doped α-Fe2O3 and FeOOH can be obtained in the end;

[0018] The alkali solution is selected from at least one of sodium hydroxide solution, ammonia solution and potassium hydroxide solution;

[0019] The regulator is selected from an iron salt solution with a mass fraction of 20-30wt%, and the iron salt solution can be selected from at least one of a ferric nitrate solution, a ferric chloride solution, and a ferric sulfate solution.

[0020] Further, the particle size of the bulk normal-parahydrogen conversion catalyst precursor is mainly affected by the alkali solution dripping speed and the concentration of the reaction solution. In order to ensure that the particle size of the obtained bulk normal-parahydrogen conversion catalyst precursor is within the specified range, the concentration of the alkali solution is controlled to be 3-19wt%, the dripping speed of the alkali solution is 3-6 L / min, and the concentration of the iron salt solution is 0.5-20mol / L; illustratively, the concentration of the iron salt solution can be 0.5mol / L, 1mol / L, 2mol / L, 3mol / L, 4mol / L, 5mol / L, 6mol / L, 7mol / L, 8mol / L, 9mol / L, 10mol / L, 11mol / L, 12mol / L, 13mol / L, 14mol / L, 15mol / L, 16mol / L, 17mol / L, 18mol / L, 19mol / L, 20mol / L, etc.

[0021] Further, when other metal salts are doped, the molar ratio of other metal elements and iron in the other metal salts and iron salt solutions is 0.05-0.3:1; illustratively, the molar ratio can be 0.05:1, 0.06:1, 0.07:1, 0.08:1, 0.09:1, 0.1:1, 0.11:1, 0.12:1, 0.13:1, 0.14:1, 0.15:1, 0.16:1, 0.17:1, 0.18:1, 0.19:1, 0.2:1, 0.21:1, 0.22:1, 0.23:1, 0.24:1, 0.25:1, 0.26:1, 0.27:1, 0.28:1, 0.29:1, 0.3:1, etc.

[0022] Furthermore, the solvent used in washing includes at least one of deionized water and anhydrous ethanol.

[0023] Furthermore, in step 1), the aging temperature is room temperature, and the aging time is 8-12 hours.

[0024] Furthermore, in step 1), the drying process mainly affects the crystal form, moisture and specific surface area of ​​the catalyst. In a specific embodiment, the drying process is drying at 40-60°C for 4-6 hours, and then drying at 100-200°C for 10-12 hours. When drying, first dry at low temperature so that most of the moisture is slowly lost, and then dry it thoroughly at high temperature to increase the strength. If it is dried directly at high temperature, the moisture will be lost quickly, causing the filter cake to shrink sharply, which is not conducive to the catalyst's adsorption of hydrogen, thereby directly affecting the catalytic activity.

[0025] Furthermore, during the process of adding the alkali solution, stirring is utilized to quickly disperse the alkali solution in the iron salt solution or the iron salt solution doped with other metal salts, and the stirring speed is 300-700 rpm.

[0026] Secondary molding granulation has a huge impact on improving the mechanical strength, stability and catalytic ability of the catalyst. The study found that by reasonably controlling the rotation speed of the granulator, the type of binder, the ratio of binder to fine powder, and the surface wetting state of the material affected by the spray in the granulator, the average crushing force value of a single catalyst particle and the sphere growth rate can be effectively affected.

[0027] The specific operation of secondary molding granulation is: mix the fine powder and the binder in proportion. The mixing process can be carried out in the granulator, or the mixing operation can be completed in advance outside the granulator. Then adjust the granulator speed to 30-40r / min, put the evenly mixed materials into the granulator in batches, and spray mist water droplets into the granulator intermittently to ensure that a very thin water film can be formed on the surface of the rolling material particles, which is in an infiltrated state, and the water content is not too high to become muddy and unable to roll. In this way, the material can be adsorbed during rolling to make the spheres gradually grow slowly to form regular small balls. Under the rolling action, the density of the balls is gradually increased, so that the balls have a certain mechanical strength. This cycle is repeated until raw balls that meet the requirements are formed.

[0028] In order to increase the pelletizing speed, a small amount of regular or irregular catalyst masterbatch with a mesh size of 70-100 can be directly added to the pelletizer. These catalyst masterbatch can be derived from the catalyst with the required mesh size obtained by granulation under the same material formula in a small-scale experiment, or can be the finished catalyst with a mesh size in this range from the previous batch.

[0029] Further, the binder plays a bonding role in the secondary molding granulation process, and the fine powder is bonded into a whole with the fine powder, so as to maintain the stability and integrity of the catalyst shape. In addition, the binder can also increase the mechanical strength of the catalyst, so that the catalyst particles are closely connected, thereby improving the durability and stability of the catalyst. In a specific embodiment, the binder is selected from at least one of the inorganic binders such as bentonite, attapulgite, hydroxypropyl methylcellulose, and hydroxyethyl methylcellulose. At the same time, it is also necessary to control the mass ratio relationship of the fine powder and the binder. If the binder ratio is too low, the spherical particles cannot grow to the required size or even if they grow to the strength is not high. If the ratio of the binder is too high, the material is easy to agglomerate, and the balling rate is not high. In a specific embodiment, the mass ratio of the fine powder to the binder is 1:0.03-0.35; illustratively, the mass ratio of the fine powder to the binder can be 1:0.03, 1:0.04, 1:0.05, 1:0.06, 1:0.07, 1:0.08, 1:0.09, 1:0.10, 1:0.11, 1:0.12, 1:0.13, 1:0.14, 1:0. 1:0.29, 1:0.30, 1:0.31, 1:0.32, 1:0.33, 1:0.34, 1:0.35, etc.

[0030] Furthermore, when the binder is selected from inorganic binders such as bentonite and attapulgite, the mass ratio of the fine powder to the binder is 1:0.1-0.30; when the binder is selected from organic binders such as hydroxypropyl methylcellulose and hydroxyethyl methylcellulose, the mass ratio of the fine powder to the binder is 1:0.03-0.08.

[0031] Furthermore, the mesh size of the fine powder is 100-300 meshes.

[0032] Furthermore, in step 2), a drying process is also included after secondary molding, which affects the mechanical strength and stability of the catalyst to a certain extent. The appropriate drying temperature and time are controlled to avoid damage to the catalyst activity or cracking of the sphere. The drying conditions are a drying temperature of 40-110°C and a drying time of 3-12 h.

[0033] Further, the mass ratio of the fine powder to the catalyst masterbatch is 1:0.03-0.1; illustratively, the mass ratio of the fine powder to the catalyst masterbatch can be 1:0.03, 1:0.04, 1:0.05, 1:0.06, 1:0.07, 1:0.08, 1:0.09, 1:0.1, etc.

[0034] Furthermore, the particle size of the iron-based para-hydrogen conversion catalyst is preferably 30-50 mesh.

[0035] Furthermore, the granulation is to mix the fine powder with the binder and then add the mixture into a pot-type granulator for granulation.

[0036] Furthermore, the bulk density of the iron-based parahydrogen conversion catalyst is 0.9-1.4 g / cc.

[0037] In order to achieve the above second purpose, the present invention adopts the following technical solutions:

[0038] The invention discloses an iron-based ortho-parahydrogen conversion catalyst prepared by the preparation method as described above.

[0039] Furthermore, the average crushing force of a single iron-based para-hydrogen conversion catalyst is 5-7 N / particle.

[0040] In order to achieve the third object, the present invention adopts the following technical solutions:

[0041] The present invention discloses an application of the above-mentioned iron-based para-hydrogen conversion catalyst in the catalytic conversion of para-hydrogen. The iron-based para-hydrogen conversion catalyst is filled in a plate-fin heat exchanger of a hydrogen liquefaction system to carry out a para-hydrogen conversion reaction.

[0042] Furthermore, the iron-based para-hydrogen conversion catalyst is filled in a test tube with a diameter of 6-8 mm and a length of 150-250 mm in a plate-fin heat exchanger. When the flow rate is not higher than 1.12 L / min / cc, the pressure drop of the iron-based para-hydrogen conversion catalyst is not greater than 950 Pa, indicating that the use of the iron-based para-hydrogen conversion catalyst provided by the present invention for the para-hydrogen conversion reaction can significantly reduce the pressure drop during the reaction.

[0043] The beneficial effects of the present invention are as follows:

[0044] The invention controls the preparation process parameters of the blocky para-hydrogen conversion catalyst precursor, including the alkali solution addition speed, the reaction solution concentration, and the drying conditions, so as to ensure that a catalyst precursor material with a suitable particle size and a stable crystal form is obtained, and then further controls the ratio of fine powder to binder, the type of binder, the selection of a granulator, and the particle size of the target catalyst, and finally obtains an iron-based para-hydrogen conversion catalyst with uniform particles, smaller particle size, regular surface, high mechanical strength, and good catalytic effect. The entire preparation process requires less equipment and materials, has less environmental pollution, and can be mass-produced.

[0045] The iron-based para-hydrogen conversion catalyst prepared by the present invention is used in a plate-fin heat exchanger of a hydrogen liquefaction system, and it is found that the bed flow resistance during the reaction can be significantly reduced, and a lower pressure drop is achieved. At the same time, the integrity of the catalyst is ensured, and pulverization is not likely to occur. It also has a higher para-hydrogen conversion efficiency, and can better meet the needs of practical applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] The specific implementation modes of the present invention will be further described in detail below in conjunction with the accompanying drawings.

[0047] Figure 1 A photograph of the iron-based para-hydrogen conversion catalyst of Example 1 is shown.

[0048] Figure 2 An optical microscope photograph of the iron-based para-hydrogen conversion catalyst (30-50 mesh) of Example 2 is shown.

[0049] Figure 3 An optical microscope photograph of the iron-based para-hydrogen conversion catalyst (20-30 mesh) of Example 5 is shown. DETAILED DESCRIPTION

[0050] In order to more clearly illustrate the present invention, the present invention is further described below in conjunction with preferred embodiments and accompanying drawings. Similar components in the accompanying drawings are represented by the same reference numerals. It should be understood by those skilled in the art that the content specifically described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.

[0051] Example 1

[0052] This embodiment provides a method for preparing an iron-based ortho-parahydrogen conversion catalyst, comprising the following steps:

[0053] 1) Take 50 kg of Fe(NO3)3·9H2O and add it to 150 L of deionized water, stir evenly to obtain ferric nitrate solution;

[0054] 2) Take 15.5 kg of NaOH and add it into 200 L of deionized water, stir evenly to obtain alkaline solution;

[0055] 3) adding alkali solution to the ferric nitrate solution under stirring at 300-700 rpm, detecting the pH in real time, and stopping the dropping when the pH of the system reaches 9, with a dropping rate of 3 L / min, then stopping the stirring, and standing and aging at room temperature for 10 hours. After the aging, adjusting the pH of the system to 7 with a 25% by mass ferric nitrate solution;

[0056] 4) Filter, wash the precipitate with deionized water, dry the precipitate at 40°C for 6 hours, and then keep it at 110°C for 12 hours. The sample is naturally cooled to room temperature to obtain a bulk normal-parahydrogen conversion catalyst precursor;

[0057] 5) The blocky ortho-parahydrogen conversion catalyst precursor is crushed into fine powder with a mesh size of 120-300 meshes, and attapulgite is added according to the mass ratio of fine powder to the attapulgite of 1:0.10. After mixing evenly, it is added to the pot granulator in batches for granulation, and the 70-100 mesh catalyst masterbatch collected in the previous batch under the same formula amount is added at the same time. The mass ratio of fine powder to catalyst masterbatch is 1:0.05, and the pot body speed is 30 rpm. During the granulation process, mist water droplets are sprayed on the material intermittently to control the humidity of the material, and the material is kept in a state of not dripping water when it is grabbed, similar to the state of damp wet soil. As the material is continuously added, the sphere gradually grows slowly to form a regular raw material ball with a size of about 0.8 mm, and stops rolling. The obtained spherical particles are dried in an industrial hot air oven at 60°C for 12 hours, sieved, and spherical particles with a particle size of 30-50 mesh are collected, and the yield is 85%.

[0058] XRD analysis showed that the crystal form of the catalyst was a mixture of α-Fe2O3 and FeOOH.

[0059] Example 2

[0060] 1) Take 100 kg of Fe(NO3)3·9H2O and add it to 150 L of deionized water, stir evenly to obtain ferric nitrate solution;

[0061] 2) Take 30.5 kg of NaOH and add it into 200 L of deionized water, stir evenly to obtain alkaline solution;

[0062] 3) adding alkali solution to the ferric nitrate solution under stirring at 300-700 rpm, detecting the pH in real time, and stopping the addition when the pH of the system reaches 9, with a dropping rate of 4 L / min, then stopping the stirring, and allowing the solution to stand for aging at room temperature for 11 hours. After the aging, adjusting the pH of the system to 7 with a 25% by mass ferric nitrate solution;

[0063] 4) Filter, wash the precipitate with deionized water, dry the precipitate at 50°C for 8 hours, and then keep it at 120°C for 12 hours. The sample is naturally cooled to room temperature to obtain a bulk normal-parahydrogen conversion catalyst precursor;

[0064] 5) The blocky ortho-parahydrogen conversion catalyst precursor is crushed into fine powder with a mesh size of 120-300 meshes, and attapulgite is added according to a mass ratio of fine powder to the attapulgite of 1:0.20. After mixing evenly, it is added to a pot-type granulator in batches for granulation, and the 70-100 mesh catalyst masterbatch collected in the previous batch with the same formula amount is added at the same time. The mass ratio of fine powder to catalyst masterbatch is 1:0.05, and the pot body speed is 30 rpm. During the granulation process, mist water droplets are sprayed on the material intermittently to control the humidity of the material, and the material is kept in a state of not dripping water when it is grabbed, similar to the state of damp wet soil. As the material is continuously added, the sphere gradually grows slowly to form a regular raw material ball with a size of about 0.8 mm, and stops rolling. The obtained spherical particles are dried in an industrial hot air oven at 70°C for 12 hours, sieved, and spherical particles with a particle size of 30-50 mesh are collected, and the yield is 80%.

[0065] XRD analysis showed that the crystal form of the catalyst was a mixture of α-Fe2O3 and FeOOH.

[0066] Example 3

[0067] This embodiment provides a method for preparing an iron-based ortho-parahydrogen conversion catalyst, comprising the following steps:

[0068] 1) Take 50 kg of Fe(NO3)3·9H2O and add it to 150 L of deionized water, stir evenly to obtain ferric nitrate solution;

[0069] 2) Take 15.5 kg of NaOH and add it into 200 L of deionized water, stir evenly to obtain alkaline solution;

[0070] 3) adding alkali solution to the ferric nitrate solution under stirring at 300-700 rpm, detecting the pH in real time, and stopping the addition when the pH of the system reaches 9, with a dropping rate of 5 L / min, then stopping the stirring, and allowing the solution to stand and age at room temperature for 12 hours. After the aging, adjusting the pH of the system to 7 with a 25% by mass ferric nitrate solution;

[0071] 4) Filter, wash the precipitate with deionized water, dry the precipitate at 40°C for 6 hours, then keep it at 110°C for 12 hours, and cool the sample naturally to room temperature to obtain a bulk normal-parahydrogen conversion catalyst precursor;

[0072] 5) The blocky ortho-parahydrogen conversion catalyst precursor is crushed into fine powder with a mesh size of 120-300 meshes, and bentonite is added according to a mass ratio of fine powder to the bentonite of 1:0.30. After mixing evenly, it is added to a pot-type granulator in batches for granulation, and the 70-100 mesh catalyst masterbatch collected in the previous batch with the same formula amount is added at the same time. The mass ratio of fine powder to catalyst masterbatch is 1:0.05, and the pot body speed is 35 rpm. During the granulation process, mist water droplets are sprayed on the material intermittently to control the humidity of the material, and the material is kept in a state of not dripping water when it is grabbed, similar to the state of damp wet soil. As the material is continuously added, the sphere gradually grows slowly to form a regular raw material ball with a size of about 0.8 mm, and stops rolling. The obtained spherical particles are dried in an industrial hot air oven at 80°C for 12 hours, sieved, and spherical particles with a particle size of 30-50 mesh are collected, and the yield is 75%.

[0073] XRD analysis showed that the crystal form of the catalyst was a mixture of α-Fe2O3 and FeOOH.

[0074] Example 4

[0075] This embodiment provides a method for preparing an iron-based ortho-parahydrogen conversion catalyst, comprising the following steps:

[0076] 1) Take 50 kg Fe(NO3)3·9H2O and 9.28 kg Al(NO3)3·9H2O and add them into 150 L deionized water, stir evenly to obtain Al-doped ferric nitrate solution;

[0077] 2) Take 19.8 kg of NaOH and add it into 200 L of deionized water, stir evenly to obtain alkaline solution;

[0078] 3) adding a sodium hydroxide solution to the Al-doped ferric nitrate solution under stirring at 300-700 rpm, detecting the pH in real time, and stopping the dropping when the pH of the system reaches 9 at a dropping rate of 6 L / min, then stopping the stirring, and allowing the solution to stand for aging at room temperature for 10 hours. After the aging, adjusting the pH of the system to 7 with a 25% by mass ferric nitrate solution;

[0079] 4) Filter, wash the precipitate with deionized water, dry the precipitate at 40°C for 6 hours, and then keep it at 110°C for 12 hours. The sample is naturally cooled to room temperature to obtain a bulk normal-parahydrogen conversion catalyst precursor;

[0080] 5) The blocky ortho-parahydrogen conversion catalyst precursor is crushed into fine powder with a mesh size of 120-300 meshes, and attapulgite is added according to the mass ratio of fine powder to the attapulgite of 1:0.10. After mixing evenly, it is added to the pot granulator in batches for granulation, and the 70-100 mesh catalyst masterbatch collected in the previous batch under the same formula amount is added at the same time. The mass ratio of fine powder to catalyst masterbatch is 1:0.05, and the pot body speed is 30 rpm. During the granulation process, mist water droplets are sprayed on the material intermittently to control the humidity of the material, and the material is kept in a state of not dripping water when it is grabbed, similar to the state of damp wet soil. As the material is continuously added, the sphere gradually grows slowly to form a regular raw material ball with a size of about 0.8 mm, and stops rolling. The obtained spherical particles are dried in an industrial hot air oven at 110°C for 12 hours, sieved, and spherical particles with a particle size of 30-50 mesh are collected, and the yield is 85%.

[0081] XRD analysis showed that the crystal form of the obtained catalyst was a mixture of Al-doped α-Fe2O3 and FeOOH.

[0082] Example 5

[0083] This embodiment provides a method for preparing an iron-based ortho-parahydrogen conversion catalyst, comprising the following steps:

[0084] 1) Take 50 kg of Fe(NO3)3·9H2O and add it to 150 L of deionized water, stir evenly to obtain ferric nitrate solution;

[0085] 2) Take 15.5 kg of NaOH and add it into 200 L of deionized water, stir evenly to obtain alkaline solution;

[0086] 3) adding alkali solution to the ferric nitrate solution under stirring at 300-700 rpm, detecting the pH in real time, and stopping the addition when the pH of the system reaches 9, with a dropping rate of 4 L / min, then stopping the stirring, and allowing the solution to stand for aging at room temperature for 8 hours. After the aging, adjusting the pH of the system to 7 with a 25% by mass ferric nitrate solution;

[0087] 4) Filter, wash the precipitate with deionized water, dry the precipitate at 40°C for 6 hours, and then keep it at 160°C for 12 hours. The sample is naturally cooled to room temperature to obtain a bulk normal-parahydrogen conversion catalyst precursor;

[0088] 5) The blocky ortho-parahydrogen conversion catalyst precursor is crushed into fine powder with a mesh size of 120-300 mesh, and hydroxyethyl methyl cellulose is added according to the mass ratio of fine powder to the hydroxyethyl methyl cellulose of 1:0.043. After mixing evenly, it is added to the pot granulator in batches for granulation, and the 70-100 mesh catalyst masterbatch collected in the previous batch with the same formula amount is added at the same time. The mass ratio of fine powder to catalyst masterbatch is 1:0.05, and the pot body speed is 35 rpm. During the granulation process, mist water droplets are sprayed on the material intermittently to control the humidity of the material, and the material is kept in a state of not dripping water when it is grabbed, similar to the state of damp wet soil. As the material is continuously added, the sphere gradually grows slowly to form a regular raw material ball with a size of about 0.8 mm, and stops rolling. The obtained spherical particles are dried in an industrial hot air oven at 110°C for 12 hours, sieved, and spherical particles with a particle size of 20-30 mesh are collected, and the yield is 78%.

[0089] XRD analysis showed that the crystal form of the catalyst was a mixture of α-Fe2O3 and FeOOH.

[0090] Comparative Example 1

[0091] This comparative example provides a method for preparing an iron-based ortho-parahydrogen conversion catalyst, comprising the following steps:

[0092] 1) Take 50 kg of Fe(NO3)3·9H2O and add it to 150 L of deionized water, stir evenly to obtain ferric nitrate solution;

[0093] 2) Take 15.5 kg of NaOH and add it into 200 L of deionized water, stir evenly to obtain alkaline solution;

[0094] 3) Under stirring at 300-700 rpm, add sodium hydroxide solution to the ferric nitrate solution, monitor the pH in real time, and stop adding when the pH of the system reaches 9. The drop rate is 3 L / min, and then stop stirring. Let it stand at room temperature for 10 hours. After the aging, adjust the pH of the system to 7 with a 25% ferric nitrate solution;

[0095] 4) Filter, wash the precipitate with deionized water, dry the precipitate at 40°C for 6 hours, then keep it at 110°C for 12 hours, and cool the sample naturally to room temperature to obtain a bulk normal-parahydrogen conversion catalyst precursor;

[0096] 5) The blocky n-parahydrogen conversion catalyst precursor is crushed into fine powder, and particles with a particle size of 30-50 mesh are sieved out.

[0097] XRD analysis showed that the crystal form of the catalyst was a mixture of α-Fe2O3 and FeOOH.

[0098] Comparative Example 2

[0099] This embodiment provides a method for preparing an iron-based ortho-parahydrogen conversion catalyst, comprising the following steps:

[0100] 1) Take 50 kg of Fe(NO3)3·9H2O and add it to 150 L of deionized water, stir evenly to obtain ferric nitrate solution;

[0101] 2) Take 30.5 kg of NaOH and add it into 200 L of deionized water, stir evenly to obtain alkaline solution;

[0102] 3) adding alkali solution to the ferric nitrate solution under stirring at 300-700 rpm, detecting the pH in real time, and stopping the dropping when the pH of the system reaches 9, with a dropping rate of 3 L / min, then stopping the stirring, and standing and aging at room temperature for 10 hours. After the aging, adjusting the pH of the system to 7 with a 25% by mass ferric nitrate solution;

[0103] 4) Filter, wash the precipitate with deionized water, dry the precipitate at 40°C for 6 hours, then keep it at 110°C for 12 hours, and cool the sample naturally to room temperature to obtain a bulk normal-parahydrogen conversion catalyst precursor;

[0104] 5) The blocky ortho-parahydrogen conversion catalyst precursor is crushed into fine powder with a mesh size of 120-300 meshes, and the attapulgite is added in a mass ratio of fine powder to the attapulgite of 1:0.10. After mixing evenly, it is added to the pot granulator in batches for granulation, and the 70-100 mesh catalyst masterbatch collected in the previous batch with the same formula amount is added at the same time. The mass ratio of fine powder to catalyst masterbatch is 1:0.05, and the pot body speed is 30 rpm. During the granulation process, mist water droplets are sprayed on the material intermittently to control the humidity of the material, and the material is kept in a state of not dripping water when it is grabbed, similar to the state of damp wet soil. As the material is continuously added, the sphere gradually grows slowly to form a regular raw material ball with a size of about 0.8 mm, and stops rolling. The obtained spherical particles are dried in an industrial hot air oven at 60°C for 12 hours, sieved, and spherical particles with a particle size of 30-50 mesh are collected, and the yield is 70%.

[0105] XRD analysis showed that the crystal form of the catalyst was a mixture of α-Fe2O3 and FeOOH.

[0106] Comparative Example 3

[0107] This comparative example provides a method for preparing an iron-based ortho-parahydrogen conversion catalyst, comprising the following steps:

[0108] 1) Take 50 kg of Fe(NO3)3·9H2O and add it to 150 L of deionized water, stir evenly to obtain ferric nitrate solution;

[0109] 2) Take 15.5 kg of NaOH and add it into 200 L of deionized water, stir evenly to obtain alkaline solution;

[0110] 3) adding alkali solution to the ferric nitrate solution under stirring at 300-700 rpm, detecting the pH in real time, and stopping the dropping when the pH of the system reaches 9, with a dropping rate of 3 L / min, then stopping the stirring, and standing and aging at room temperature for 10 hours. After the aging, adjusting the pH of the system to 7 with a 25% by mass ferric nitrate solution;

[0111] 4) Filter, wash the precipitate with deionized water, dry the precipitate at 150° C. for 12 h, and cool the sample naturally to room temperature to obtain a bulk n-parahydrogen conversion catalyst precursor;

[0112] 5) The blocky ortho-parahydrogen conversion catalyst precursor is crushed into fine powder with a mesh size of 120-300 meshes, and attapulgite is added according to a mass ratio of fine powder to the attapulgite of 1:0.10. After mixing evenly, it is added to a pot-type granulator in batches for granulation, and the 70-100 mesh catalyst masterbatch collected in the previous batch under the same formula amount is added at the same time. The mass ratio of fine powder to catalyst masterbatch is 1:0.05, and the pot body speed is 30 rpm. During the granulation process, mist water droplets are sprayed on the material intermittently to control the humidity of the material, and the material is kept in a state of not dripping water when it is grabbed, similar to the state of damp wet soil. As the material is continuously added, the sphere gradually grows slowly to form a regular raw material ball with a size of about 0.8 mm, and stops rolling. The obtained spherical particles are dried in an industrial hot air oven at 60°C for 12 hours, sieved, and spherical particles with a particle size of 30-50 mesh are collected, and the yield is 55%.

[0113] XRD analysis showed that the crystal form of the catalyst was α-Fe2O3.

[0114] Comparative Example 4

[0115] This embodiment provides a method for preparing an iron-based ortho-parahydrogen conversion catalyst, comprising the following steps:

[0116] 1) Take 50 kg of Fe(NO3)3·9H2O and add it to 150 L of deionized water, stir evenly to obtain ferric nitrate solution;

[0117] 2) Take 15.5 kg of NaOH and add it into 200 L of deionized water, stir evenly to obtain alkaline solution;

[0118] 3) adding alkali solution to the ferric nitrate solution under stirring at 300-700 rpm, detecting the pH in real time, and stopping the dropping when the pH of the system reaches 9, with a dropping rate of 3 L / min, then stopping the stirring, and standing and aging at room temperature for 10 hours. After the aging, adjusting the pH of the system to 7 with a 25% by mass ferric nitrate solution;

[0119] 4) Filter, wash the precipitate with deionized water, dry the precipitate at 40°C for 6 hours, and then keep it at 110°C for 12 hours. The sample is naturally cooled to room temperature to obtain a bulk normal-parahydrogen conversion catalyst precursor;

[0120] 5) The blocky ortho-parahydrogen conversion catalyst precursor is crushed into fine powder with a mesh size of 120-300 meshes, and attapulgite is added according to the mass ratio of fine powder to the attapulgite of 1:0.40. After mixing evenly, it is added to the pot granulator in batches for granulation, and the 70-100 mesh catalyst masterbatch collected in the previous batch under the same formula amount is added at the same time. The mass ratio of fine powder to catalyst masterbatch is 1:0.05, and the pot body speed is 30 rpm. During the granulation process, mist water droplets are sprayed on the material intermittently to control the humidity of the material, and the material is kept in a state of not dripping water when it is grabbed, similar to the state of damp wet soil. As the material is continuously added, the sphere gradually grows slowly to form a regular raw material ball with a size of about 0.8 mm, and stops rolling. The obtained spherical particles are dried in an industrial hot air oven at 60°C for 12 hours, sieved, and spherical particles with a particle size of 30-50 mesh are collected, and the yield is 50%.

[0121] XRD analysis showed that the crystal form of the catalyst was a mixture of α-Fe2O3 and FeOOH.

[0122] Test Example 1: Voltage Drop Test

[0123] In the low temperature range, the inertial resistance of hydrogen passing through the packed bed cannot be ignored. The bed pressure drop is mainly affected by the combined effect of viscous resistance and inertial resistance, and is quadratically related to the speed. The catalyst has a significant effect on the bed pressure drop. The present invention tests the pressure drop of hydrogen before and after passing through a 3 / 8 British stainless steel tube with an inner diameter of 7.75mm and a length of 200mm under 77K and 2Mpa conditions. The test results are shown in Table 1. The experiment found that with the increase of flow rate, the pressure drop gradually increased. The pressure drop values ​​of powder particle catalysts are generally higher than those of spherical ones. When the flow rate is 1.166 L / min / cc catalyst, the pressure drop of the spherical catalyst is 943.1 Pa, while the pressure drop of the powder particles is 3701.1 Pa, which is about 4 times that of the spherical catalyst. The pressure drop of the spherical catalyst is much smaller than that of the powder particle catalyst, indicating that the spherical catalyst can effectively reduce the flow resistance of the catalyst bed and has higher practicality.

[0124] Table 1

[0125]

[0126] The catalyst to be tested was fully activated, and 1 mL of the activated catalyst (bulk density of 1.3 g / cc) was taken for reaction in a normal-parahydrogen conversion device at 77K and a hydrogen flow rate of 1200 mL / min / cc catalyst. The data was collected by gas chromatograph to determine the catalyst activity at a certain space velocity.

[0127] The catalyst to be tested is tested for its single particle crushing strength using a particle strength tester. The test process is: take the same catalyst particles to test their mechanical strength three times in total, taking 20-30 catalysts each time. When the data is counted, remove the highest and lowest values ​​of each group of data, and then calculate the average value.

[0128] The conversion rate of normal and para hydrogen and the single particle strength of different catalysts are shown in Table 2.

[0129] Table 2

[0130]

[0131] It can be seen from Table 2 that the catalytic activity and average crushing force of the catalyst after secondary molding are higher than those of the catalyst without secondary molding. In addition, doping with Al is beneficial to improving the strength of the catalyst.

[0132] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. A method for preparing an iron-based ortho-parahydrogen conversion catalyst, characterized in that: The steps include: 1) adding alkaline solution dropwise to an iron salt solution or an iron salt solution doped with other metal salts under stirring to adjust the pH to 8.5-10.5, and aging the solution. After aging, neutralizing the solution with a regulator to a pH of 6.5-7.5, and washing and drying the solution to obtain a blocky ortho-parahydrogen conversion catalyst precursor. 2) crushing the blocky n-parahydrogen conversion catalyst precursor into fine powder, mixing it with a binder and then feeding it into a granulator in batches for spray granulation, drying and sieving to obtain a spherical or quasi-spherical catalyst with a particle size of 20-50 mesh; The iron-based parahydrogen conversion catalyst is a mixture of α-Fe2O3 and FeOOH doped or undoped with other metal elements; The binder is selected from at least one of bentonite and attapulgite, and the mass ratio of the fine powder to the binder is 1:0.1-0.30; or the binder is selected from at least one of hydroxypropyl methylcellulose and hydroxyethyl methylcellulose, and the mass ratio of the fine powder to the binder is 1:0.03-0.

08.

2. The preparation method according to claim 1, characterized in that: The iron salt in the iron salt solution is selected from at least one of iron nitrate, iron chloride and iron sulfate; The other metal salt is selected from at least one of cobalt salt, cerium salt, nickel salt and aluminum salt; The alkali solution is selected from at least one of sodium hydroxide solution, ammonia solution and potassium hydroxide solution; The regulator is selected from an iron salt solution with a mass fraction of 20-30wt%.

3. The preparation method according to claim 1, characterized in that: The concentration of the iron salt solution is 0.5-20 mol / L; When other metal salts are doped, the molar ratio of other metal elements to iron in the other metal salt and iron salt solution is 0.05-0.3:

1.

4. The preparation method according to claim 1, characterized in that: The mesh size of the fine powder is 100-300 meshes; the granulator is selected from a pot-type granulator, and its rotation speed is 30-40r / min.

5. The preparation method according to claim 1, characterized in that: The bulk density of the iron-based parahydrogen conversion catalyst is controlled at 0.9-1.4 g / cc.

6. The preparation method according to claim 1, characterized in that: In step 1), the aging temperature is room temperature, and the aging time is 8-12 hours; the drying conditions are drying at 40-60° C. for 4-6 hours, and then drying at 100-200° C. for 10-12 hours.

7. An iron-based parahydrogen conversion catalyst, characterized in that: The preparation is obtained by the preparation method according to any one of claims 1 to 6.

8. The iron-based ortho-parahydrogen conversion catalyst according to claim 7, characterized in that The average crushing force of a single iron-based para-hydrogen conversion catalyst is 5-7 N / particle.

9. Use of the iron-based para-hydrogen conversion catalyst according to any one of claims 7 to 8 in catalytic conversion of para-hydrogen, characterized in that: The iron-based para-hydrogen conversion catalyst is filled in a plate-fin heat exchanger of a hydrogen liquefaction system to carry out a para-hydrogen conversion reaction.

10. The use according to claim 9, characterized in that: The iron-based para-hydrogen conversion catalyst is filled in a test tube of a plate-fin heat exchanger with a diameter of 6-8 mm and a length of 150-250 mm. When the flow rate is not higher than 1.12 L / min / cc, the pressure drop of the iron-based para-hydrogen conversion catalyst is not greater than 950 Pa.