A kind of carbon mineralized inorganic artificial stone and preparation method thereof
Through compounding modified powder and process adjustment, combined with the use of carbon dioxide gas, the problem of insufficient mechanical properties and permeability of inorganic artificial stones was solved, and high-performance carbon mineralized inorganic artificial stones was prepared, achieving the goal of green building And improve the overall performance of the product.
Patent Information
- Application Number
- CN202411182637.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The existing inorganic artificial stone has shortcomings in terms of mechanical properties and permeability resistance, and the addition of high-carbon emission cement to its raw materials is not conducive to the promotion of green buildings.
Through the combination and process adjustment of modified powders, auxiliary materials, inorganic fillers, solid waste aggregates, fibers, water repellents, and water reducing agents, carbon mineralized inorganic stones with high mechanical strength and good permeability resistance are prepared. The mineralization reaction is carried out using carbon dioxide-containing gas to generate phenol salts and complexes to fill and seal the pores and cracks of solid waste powder, and improve density and permeability.
Carbon mineralized inorganic artificial stone has been achieved with high mechanical strength, high carbon fixation rate, low water absorption rate and good gloss, optimized the various properties of the product, and promoted the utilization of carbon dioxide resources.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and in particular to a carbon mineralized inorganic artificial stone and a preparation method thereof. Background Art
[0002] Artificial stone is one of the commonly used building materials, which is divided into organic negative carbon stone board and inorganic negative carbon stone board. Most of the organic artificial boards use adhesives such as phenolic enhancers and urea-formaldehyde enhancers, which may have adverse effects on the human body; while inorganic boards are made of cement as the main binder and various natural aggregates. They are better than resin-type artificial stones in high temperature resistance and fire resistance, and are non-toxic and pollution-free. They can be used in the field of decoration, but the raw materials they use are some high-carbon emission raw materials, which is not conducive to the promotion of green buildings.
[0003] Inorganic artificial stone has certain defects in inorganic materials, such as low strength, poor toughness and impermeability. For example, Chinese patent application CN117645439A discloses a high-strength inorganic artificial travertine and its preparation method. Its main raw materials include artificial stone aggregate, cement, auxiliary cementitious materials, and fillers. The compressive strength of the obtained product reaches more than 110MPa and the flexural strength reaches more than 22MPa. Although relatively excellent mechanical properties can be obtained, the addition of high-carbon raw material cement in its raw materials is not conducive to carbon reduction. The preparation of a carbon-negative, green, superior performance, and high-gloss solid waste-based carbon mineralized inorganic artificial stone is still full of challenges. Summary of the invention
[0004] In order to overcome the above-mentioned shortcomings, one of the purposes of the present invention is to prepare a solid waste-based carbon mineralized inorganic artificial stone with high mechanical strength, good impermeability and gloss through further raw material compounding and process adjustment.
[0005] In order to achieve the above purpose, the technical solution adopted by the present invention is: the raw materials for preparing carbon mineralized inorganic artificial stone include modified powder, auxiliary materials, inorganic filler, solid waste aggregate, fiber, water repellent, and water reducing agent;
[0006] Furthermore, by mass, the raw materials for preparing carbon mineralized inorganic artificial stone include 15-70 parts of modified powder, 3-25 parts of auxiliary materials, 5-28 parts of inorganic fillers, 20-120 parts of solid waste aggregates, 1-7 parts of fibers, 0.2-2.0 parts of water repellents, and 0.2-1.5 parts of water reducing agents.
[0007] Exemplarily, the modified powder is in the range of 15 parts, 20 parts, 25 parts, 30 parts, 40 parts, 50 parts, 60 parts, 70 parts or any two of them; the auxiliary material is in the range of 3 parts, 5 parts, 10 parts, 15 parts, 20 parts, 25 parts or any two of them; the inorganic filler is in the range of 5 parts, 10 parts, 15 parts, 20 parts, 25 parts, 28 parts or any two of them; the solid waste aggregate is in the range of 20 parts, 40 parts, 60 parts, 80 parts, 100 parts, 120 parts or any two of them; the fiber is in the range of 1 part, 3 parts, 5 parts, 7 parts or any two of them; the water repellent is in the range of 0.2 parts, 0.5 parts, 1.0 parts, 1.5 parts, 2.0 parts or any two of them; the water reducer is in the range of 0.2 parts, 0.5 parts, 0.7 parts, 1.0 parts, 1.2 parts, 1.5 parts or any two of them.
[0008] Preferably, by mass, the raw materials for preparing carbon mineralized inorganic artificial stone include 20-51 parts of modified powder, 6-16 parts of auxiliary materials, 7-20 parts of inorganic fillers, 35-90 parts of solid waste aggregates, 2-5 parts of fibers, 0.3-0.8 parts of water repellents, and 0.3-0.8 parts of water reducing agents.
[0009] Furthermore, the auxiliary material is selected from any one or both of quartz powder and granite.
[0010] Further, the average particle size of the auxiliary material is 150-400 mesh;
[0011] Preferably, the average particle size of the auxiliary material is 200-300 mesh.
[0012] Further, the inorganic filler is selected from any one or more of slag, fly ash, and fine tailings;
[0013] Preferably, the inorganic filler is selected from any one or more of slag and fly ash.
[0014] Further, the average particle size of the inorganic filler is 50-300 mesh;
[0015] Preferably, the average particle size of the inorganic filler is 60-240 mesh.
[0016] Further, the solid waste aggregate is selected from any one or more of steel slag particles, magnesium slag particles, sawdust, coarse tailings, and waste concrete particles;
[0017] Preferably, the solid waste aggregate is selected from any one or more of steel slag particles and magnesium slag particles.
[0018] Further, the average particle size of the solid waste aggregate is 0.01-8 mm;
[0019] Preferably, the average particle size of the solid waste aggregate is 0.01-5 mm.
[0020] Further, the fiber is selected from any one or more of basalt fiber, polypropylene fiber, and glass fiber;
[0021] Preferably, the fiber is selected from any one or more of basalt fiber and polypropylene fiber.
[0022] Furthermore, the average diameter of the fibers is 10-20 μm and the length is 8-19 mm.
[0023] Further, the water repellent is selected from any one or more of octyltriethoxysilane, calcium stearate, and methyl calcium silicate;
[0024] Preferably, the hydrophobic agent is selected from any one or more of octyltriethoxysilane and calcium stearate.
[0025] Furthermore, the water reducer is selected from any one or more of polycarboxylate water reducer and naphthalene water reducer;
[0026] Preferably, the water reducer is a polycarboxylate water reducer.
[0027] Furthermore, the raw materials for preparing the modified powder include solid waste powder, phenolic compounds and a reinforcing agent;
[0028] Furthermore, the raw materials for preparing the modified powder include, by mass, 30-70 parts of solid waste powder, 3-20 parts of phenolic compounds and 1-18 parts of enhancer.
[0029] Exemplarily, the solid waste powder is in the range of 30 parts, 40 parts, 50 parts, 60 parts, 70 parts or any two thereof; the phenol compound is in the range of 3 parts, 5 parts, 10 parts, 12 parts, 15 parts, 18 parts, 20 parts or any two thereof; the enhancer is in the range of 1 part, 2 parts, 5 parts, 8 parts, 10 parts, 12 parts, 15 parts, 18 parts or any two thereof.
[0030] Furthermore, the solid waste raw material used to prepare the solid waste powder is at least one of steel slag, magnesium slag, calcium silicate slag, blast furnace slag, coal gangue, carbide slag, alkali slag, zero slag, and thiourea slag;
[0031] Preferably, the solid waste raw material used to prepare the solid waste powder is at least one of steel slag, magnesium slag, calcium-silicon slag and blast furnace slag.
[0032] Among them, the calcium-silicon slag is the calcium-silicon slag after aluminum extraction treatment.
[0033] Furthermore, the solid waste powder is obtained by wet grinding the solid waste raw materials.
[0034] Furthermore, the specific steps of wet grinding treatment are: at room temperature, keep the moisture content of the solid waste raw material at 30-70%, wet grind for 0.5-2h, and then dry at 40-60°C to a moisture content of 5-10%. The obtained solid waste powder has alkali metal salts distributed on it after wet grinding.
[0035] Furthermore, the average particle size of the solid waste powder is 100-300 meshes.
[0036] Furthermore, the phenol compound is at least one of resorcinol, m-aminophenol, 4-methylcatechol, 4-isopropylphenol and 2-sec-butylphenol.
[0037] Furthermore, the reinforcing agent is at least one of polyacrylic acid and chloroacetic acid resin;
[0038] Preferably, the reinforcing agent is polyacrylic acid.
[0039] Further, the mass ratio of the solid waste powder to the phenol compound is 1:(0.05-0.5);
[0040] Exemplarily, the mass ratio of the solid waste powder to the phenol compound is 1:0.05, 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5 or a range consisting of any two thereof;
[0041] Preferably, the mass ratio of solid waste powder to phenolic compounds is 1:(0.1-0.3).
[0042] Further, the mass ratio of the phenolic compound to the enhancer is 1:(0.1-1.2);
[0043] Illustratively, the mass ratio of the phenol compound to the enhancer is 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2 or a range consisting of any two of them.
[0044] Preferably, the mass ratio of the phenol compound to the enhancer is 1:(0.3-0.9).
[0045] Furthermore, the modified powder preparation method comprises the following steps:
[0046] (1) Take solid waste powder, add phenol compound and enhancer in sequence, stir evenly, and obtain a mixed material;
[0047] (2) The mixed material is placed in a mineralization reactor, and after the air is replaced by a gas containing carbon dioxide, the pressure is increased to 0.1-1 MPa, the temperature is raised to 60-100°C, and the reaction is kept at this temperature for 1-8 hours. After the reaction is completed, the product is ground to obtain a modified powder.
[0048] Preferably, the preparation steps of the modified powder include:
[0049] (1) Take 30-70 parts of wet-grinded solid waste powder (100-300 mesh), add 3-20 parts of phenolic compounds and 1-18 parts of enhancer in sequence, and stir for 5-10 minutes to obtain a mixture;
[0050] (2) The mixed material is placed in a mineralization reactor, and after the air is replaced by a gas containing carbon dioxide, the mixture is pressurized to 0.1-0.5 MPa, and the temperature is raised to 80-100°C. The mixture is kept warm for 2-6 hours. After the reaction is completed, the product is ground into 200-500 mesh to obtain a modified powder.
[0051] Under the conditions of pressure and temperature, phenol compounds react with alkali metal salts in the solid waste powder after wet grinding to form phenol salts, and the ortho-carbon of the phenolic hydroxyl group is activated, reacting with carbon dioxide for a nucleophilic addition reaction, which not only consumes more carbon dioxide, but the reaction products can also synergize the carboxyl groups in the enhancer structure with the metal ions on the surface of the solid waste powder to form a stable coordination relationship, forming a complex, which effectively fills and seals the pores and cracks in the solid waste powder.
[0052] Further, the mass concentration of carbon dioxide in the carbon dioxide-containing gas is 8-100%;
[0053] Preferably, the mass concentration of carbon dioxide in the carbon dioxide-containing gas is 50-100%.
[0054] Furthermore, the gas containing carbon dioxide also contains gases such as nitrogen, oxygen, and water vapor.
[0055] The second aspect of the present invention provides a method for preparing a carbon mineralized inorganic artificial stone, comprising the following steps:
[0056] S1. Take the modified powder, auxiliary materials, solid waste aggregate, fiber, water reducing agent, water repellent and water and mix them evenly to obtain carbon mineralized inorganic artificial stone slurry, and keep its water content at 8-15wt%;
[0057] S2, breaking up the carbon mineralized inorganic artificial stone slurry, spreading it, transferring it to a press, and vibrating and pressing the mixed material under vacuum to obtain a carbon mineralized inorganic artificial stone blank fixed by a mold;
[0058] S3, transporting the carbon mineralized inorganic artificial stone body with the mold to a steam curing box for curing;
[0059] S4. After the curing is completed, the product is sent to a mineralization reactor for reaction, and the air is replaced by a gas containing carbon dioxide, and then a mineralization reaction is carried out;
[0060] S5. After the reaction is completed, demoulding, drying, thickness determination, grinding and polishing, and protective treatment are performed to obtain carbon mineralized inorganic artificial stone.
[0061] Preferably, in step S2, the vacuum degree of vibration pressing is -0.09 to -0.1 MPa, and the pressure of the pressing head is 0.1 to 5 MPa;
[0062] In step S3, the curing temperature is 40 to 100° C. and the curing time is 2 to 10 hours;
[0063] In step S4, the pressure of the mineralization reaction is 0.1-1 MPa, the temperature is 60-100° C., and the reaction time is 1-8 h.
[0064] Preferably, in step S1, the water content is maintained at 10-15wt%;
[0065] In step S2, the vacuum degree of vibration pressing is -0.09 to -0.1 MPa, and the pressure of the pressing head is 0.5 to 2 MPa;
[0066] In step S3, the curing temperature is 50-70°C and the curing time is 6-8h;
[0067] In step S4, the pressure of the mineralization reaction is 0.1-1 MPa, the temperature is 70-90° C., and the reaction time is 2-4 h.
[0068] The beneficial effects of the present invention are:
[0069] A carbon mineralized inorganic artificial stone with high mechanical strength, high carbon fixation rate, low water absorption rate and good gloss is prepared by using modified powder, auxiliary materials, inorganic fillers, solid waste aggregates, fibers, water repellents and water reducers as raw materials; by strictly controlling the mass ratio of solid waste powder to phenolic compounds and the mass ratio of phenolic compounds to reinforcing agents, the modification degree of solid waste powder is regulated, thereby optimizing the various properties of carbon mineralized inorganic artificial stone.
[0070] The phenolic compounds introduced into the modified solid waste powder have a benzene ring structure, which improves the dispersibility between the solid waste powders, reduces the agglomeration of the powders, and improves the force uniformity of the carbon mineralized inorganic artificial stone. Similarly, the early introduction of the reinforcing agent can not only cooperate with the phenolic compounds to modify the solid waste powder, but also improve the bonding strength between the components to increase the density and improve the product performance.
[0071] 3) The addition of inorganic fillers plays a role in material grading and improves the strength of carbon mineralized inorganic artificial stone; the addition of auxiliary materials not only further improves the strength of the product, but also gives it a certain glossiness and improves the aesthetics of the product.
[0072] 4) Add phenol compounds and enhancers as solid waste powder modifiers to the solid waste powder obtained by wet grinding, and introduce gas containing carbon dioxide to mineralize and modify the solid waste powder to obtain modified solid waste powder. Under the conditions of temperature and pressure, phenol compounds react with alkali metal salts to form phenol salts, and the ortho-carbon of the phenolic hydroxyl group is activated, and a nucleophilic addition reaction occurs with carbon dioxide. On the one hand, the product may cooperate with the carboxyl group in the enhancer structure to form a stable coordination relationship with the metal ions on the surface of the solid waste powder to form a complex, effectively filling and sealing the pores and cracks on the surface of the solid waste powder, forming a dense protective film, improving the density and impermeability of the system, thereby improving the mechanical strength of the product and reducing its water absorption. On the other hand, this process consumes more carbon dioxide, which is beneficial to the resource utilization of carbon dioxide.
[0073] 5) The modified powder that has been mineralized in advance can be used as a crystal nucleus, which is beneficial to the mineralization reaction in step S4 during the preparation process of carbon mineralized inorganic artificial stone. DETAILED DESCRIPTION
[0074] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0075] Except as shown in the operating examples or otherwise indicated, all numbers used in the specification and claims to indicate the amount of ingredients, physicochemical properties, etc. are understood to be adjusted by the term "about" in all cases. Therefore, unless otherwise indicated, the numerical parameters listed in the above specification and the attached claims are approximate values, and those skilled in the art can use the teachings disclosed herein to seek to obtain the desired properties and appropriately change these approximate values. The use of numerical ranges expressed as endpoints includes all numbers within the range and any range within the range, for example, 1 to 5 includes 1, 1.1, 1.3, 1.5, 2, 2.75, 3, 3.80, 4 and 5, etc.
[0076] In some embodiments, a carbon mineralized inorganic artificial stone is prepared from raw materials, by mass, comprising:
[0077] Raw material 1: auxiliary materials
[0078] The auxiliary material is 3-25 parts, preferably 6-16 parts, and the auxiliary material is used to improve the glossiness and strength of the carbon mineralized inorganic artificial stone.
[0079] The auxiliary material is selected from any one of quartz powder and granite, preferably selected from quartz powder.
[0080] The average particle size of the auxiliary material is 150-400 mesh, preferably 200-300 mesh.
[0081] Auxiliary materials not only enhance the mechanical strength of carbon mineralized inorganic artificial stone, but also optimize its glossiness and improve the aesthetics of the product.
[0082] Raw material 2: Inorganic filler
[0083] 5-28 parts of inorganic filler, preferably 7-20 parts,
[0084] The inorganic filler is selected from any one or more of slag, fly ash, and fine tailings, preferably selected from any one or more of slag and fly ash;
[0085] The average particle size of the inorganic filler is 50-300 mesh, preferably 60-240 mesh.
[0086] Raw material three: solid waste aggregate
[0087] 20-120 parts of solid waste aggregate, preferably 35-90 parts;
[0088] The solid waste aggregate is selected from any one or more of steel slag particles, magnesium slag particles, sawdust, coarse tailings, and waste concrete particles, preferably selected from any one or more of steel slag particles and magnesium slag particles;
[0089] The average particle size of the solid waste aggregate is 0.01-8 mm, preferably 0.01-5 mm.
[0090] Inorganic fillers and solid waste aggregates are used for grading between raw materials. Large-sized solid waste aggregates are used for strength support, and small-sized inorganic fillers are used for filling holes. Through the grading between coarse and fine aggregates, the packing density is increased, the structural density inside the product is improved, and thus the mechanical properties are improved.
[0091] Raw material 4: fiber
[0092] 1-7 parts of fiber, preferably 2-5 parts;
[0093] The fiber is selected from any one or more of basalt fiber, polypropylene fiber, and glass fiber, preferably selected from any one or more of basalt fiber and polypropylene fiber;
[0094] The average diameter of the fibers is 10-20 μm and the length is 8-19 mm.
[0095] Raw material 5: water repellent
[0096] 0.2-2.0 parts of water repellent, preferably 0.3-0.8 parts;
[0097] The water repellent is selected from any one or more of octyltriethoxysilane, calcium stearate, and methyl calcium silicate, and is preferably selected from any one or more of octyltriethoxysilane and calcium stearate.
[0098] Raw material six: water reducing agent
[0099] Water reducing agent 0.2-1.5 parts, preferably 0.3-0.8 parts;
[0100] The water reducer is selected from any one or more of polycarboxylate water reducers and naphthalene water reducers, preferably polycarboxylate water reducers.
[0101] Raw material seven: modified powder
[0102] The modified powder is 15-70 parts, preferably 20-51 parts;
[0103] The modified powder is the solid waste powder obtained by modifying the solid waste powder after wet grinding. That is, phenol compounds and enhancers are added to the solid waste powder after wet grinding as solid waste powder modifiers, and carbon dioxide-containing gas is introduced to mineralize and modify the solid waste powder to obtain the modified powder.
[0104] Under the conditions of elevated temperature and pressure, phenol compounds react with alkali metal salts to form phenol salts, the ortho-carbon of the phenolic hydroxyl group is activated, and an addition reaction occurs with the carbonyl carbon of carbon dioxide. The resulting synergistic enhancer forms a stable coordination relationship with the metal ions on the surface of the solid waste powder to form a complex, which effectively fills and seals the pores and cracks on the surface of the solid waste powder, forming a dense protective film, thereby improving the density and impermeability of the system, thereby improving the mechanical strength of the product and reducing its water absorption.
[0105] In some embodiments, the raw materials for preparing the modified powder include, by mass, 30-70 parts of solid waste powder, 3-20 parts of phenolic compounds, and 1-18 parts of enhancer.
[0106] In some embodiments, the solid waste raw material used to prepare solid waste powder is at least one of steel slag, magnesium slag, calcium silicate slag, blast furnace slag, coal gangue, carbide slag, alkali slag, zero slag, and thiourea slag.
[0107] In some embodiments, the solid waste raw material used to prepare solid waste powder is at least one of steel slag, magnesium slag, calcium-silicon slag, and blast furnace slag.
[0108] Among them, the calcium-silicon slag is the calcium-silicon slag after aluminum extraction treatment.
[0109] In some embodiments, the solid waste powder is obtained by wet grinding of solid waste raw materials, that is, at room temperature, the water content of the solid waste raw materials is maintained at 30-70%, wet grinding is performed for 0.5-2 hours, and then dried at 40-60° C. to a water content of 5-10%, to obtain solid waste powder. Alkali metal salts are distributed on the surface of the wet-ground solid waste powder.
[0110] In some embodiments, the average particle size of the solid waste powder is 100-300 mesh.
[0111] In some embodiments, the phenol compound is at least one of resorcinol, m-aminophenol, 4-methylcatechol, 4-isopropylphenol, and 2-sec-butylphenol;
[0112] The benzene ring structure in phenol compounds improves the dispersibility between solid waste powders, reduces the agglomeration of powders, and improves the force uniformity of carbon mineralized inorganic artificial stone. In addition, the products of the nucleophilic addition reaction of phenol compounds and carbon dioxide, synergistic enhancers, form complexes on the surface of solid waste powders to fill pores and form a dense protective film on the surface of solid waste, which not only improves the density of the product and improves the performance of the product, but also consumes more carbon dioxide.
[0113] In some embodiments, the reinforcing agent is at least one of polyacrylic acid and chloroacetic acid resin;
[0114] In some embodiments, the reinforcing agent is polyacrylic acid.
[0115] With the introduction of the enhancer, the carboxylic acid in its structure can cooperate with the product of the nucleophilic addition of phenolic compounds and carbon dioxide to form a complex on the surface of solid waste powder, fill the tiny pores of the solid waste powder, and form a dense protective film to improve the density and impermeability of the system. It can also increase the bonding strength between the components, improve the density of the product, and thus improve the product performance.
[0116] In some embodiments, the mass ratio of solid waste powder to phenolic compound is 1:(0.05-0.5);
[0117] In some embodiments, the mass ratio of solid waste powder to phenolic compound is 1:(0.1-0.3).
[0118] In some embodiments, the mass ratio of the phenolic compound to the enhancer is 1:(0.1-1.2);
[0119] In some embodiments, the mass ratio of the phenolic compound to the enhancer is 1:(0.3-0.9).
[0120] A method for preparing carbon mineralized inorganic artificial stone:
[0121] S1. Take the modified powder, auxiliary materials, solid waste aggregate, fiber, water reducer, water repellent and water and mix them evenly to obtain carbon mineralized inorganic artificial stone slurry, and keep its water content at 8-15%wt, preferably 10-15wt%.
[0122] S2. Break up the carbon mineralized inorganic artificial stone slurry, distribute it, and transfer it to a press. Vibrate and press the mixed material under vacuum to obtain a carbon mineralized inorganic artificial stone body fixed by a mold; the vacuum degree is -0.09 to -0.1 MPa, and the pressure of the pressing head is 0.1-5 MPa, preferably 0.5-2 MPa.
[0123] S3, transporting the carbon mineralized inorganic artificial stone body with the mold to a steam curing box for curing, the curing temperature is 40-100° C., preferably 50-70° C., and the curing time is 2-10 hours, preferably 6-8 hours.
[0124] S4. After the curing is completed, the mixture is sent to a mineralization reactor for reaction. After the air is replaced by a gas containing carbon dioxide, the mixture is pressurized to 0.1-1 MPa, heated to 60-100° C., preferably 70-90° C., and kept warm for reaction for 1-8 hours, preferably 2-4 hours;
[0125] S5. After the reaction is completed, demoulding, drying, thickness determination, grinding and polishing, and protective treatment are performed to obtain carbon mineralized inorganic artificial stone.
[0126] The modified powder preparation steps include:
[0127] (1) Take solid waste powder, add phenol compound and enhancer in sequence, stir evenly, and obtain a mixed material;
[0128] (2) The mixed material is placed in a mineralization reactor, and after the air is replaced by a gas containing carbon dioxide, the pressure is increased to 0.1-1 MPa, the temperature is raised to 60-100°C, and the reaction is kept at this temperature for 1-8 hours. After the reaction is completed, the product is ground to obtain a modified powder.
[0129] In some embodiments, the modified powder preparation step includes:
[0130] (1) Take 30-70 parts of wet-grinded solid waste powder (100-300 mesh), add 3-20 parts of phenolic compounds and 1-18 parts of enhancer in sequence, mix well, and stir for 5-10 minutes to obtain a mixed material;
[0131] (2) The mixed material is placed in a mineralization reactor, and after the air is replaced by a gas containing carbon dioxide, the mixture is pressurized to 0.1-0.5 MPa, and the temperature is raised to 80-100°C. The mixture is kept warm for 2-6 hours. After the reaction is completed, the product is ground into 200-500 mesh to obtain a modified powder.
[0132] In some embodiments, the carbon dioxide concentration in the carbon dioxide-containing gas is 8-100%;
[0133] In some embodiments, the concentration of carbon dioxide in the carbon dioxide-containing gas is 50-100%;
[0134] In some embodiments, the gas containing carbon dioxide also includes nitrogen, oxygen, water vapor and other gases.
[0135] Example
[0136] The following examples describe the disclosure of the present invention in more detail, and these examples are intended for illustrative purposes only, as various modifications and variations within the scope of the disclosure of the present invention are apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by mass, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.
[0137] Example 1
[0138] The raw materials for preparing a carbon mineralized inorganic artificial stone include: 36 parts of modified powder (300 mesh), 10.8 parts of auxiliary quartz powder (250 mesh), 13.6 parts of inorganic filler slag (160 mesh), 63 parts of solid waste aggregate steel slag particles (2 mm), 1.8 parts of fiber basalt fiber (diameter of 15 μm, length of 15 mm), 0.5 parts of water reducing agent polycarboxylic acid water reducing agent, and 0.5 parts of water repellent octyltriethoxysilane.
[0139] A method for preparing carbon mineralized inorganic artificial stone comprises the following steps:
[0140] S1. Preparation of carbon mineralized inorganic artificial stone slurry
[0141] S11, take 50 parts of 200-mesh solid waste powder (steel slag) treated by wet grinding, add 10 parts of phenol compound (resorcinol) and 6.5 parts of reinforcing agent (polyacrylic acid) in sequence, mix well, and stir for 8 minutes to obtain a mixed material;
[0142] The wet grinding treatment of solid waste powder (steel slag) is as follows: at room temperature, the moisture content of the solid waste raw material steel slag is maintained at 50%, wet grinding is performed for 1.3 hours, and then drying is performed at 50°C to a moisture content of 8% to obtain solid waste powder.
[0143] S12, putting the mixed material into a mineralization reactor, replacing the air with a carbon dioxide-containing gas with a carbon dioxide concentration of 90%, pressurizing it to 0.1MPa, heating it to 90°C, and keeping it warm for 4h. After the reaction is completed, grinding the product into 300 mesh to obtain a modified powder;
[0144] S13, take 36 parts of modified powder, 10.8 parts of auxiliary material (quartz powder), 13.6 parts of inorganic filler (slag), 63 parts of solid waste aggregate (steel slag particles), 1.8 parts of fiber (basalt fiber), 0.5 parts of water reducer (polycarboxylate water reducer), 0.5 parts of water repellent (octyl triethoxy silane) and water and mix them evenly to obtain carbon mineralized inorganic artificial stone slurry, and keep its water content at 12%wt;
[0145] S2. Break up the carbon mineralized inorganic artificial stone slurry, spread it, and transfer it to a press. Vibrate and press the mixed material under vacuum to obtain a carbon mineralized inorganic artificial stone body fixed by a mold; the vacuum degree is -0.09MPa, and the pressure of the pressing head is 1.5MPa.
[0146] S3. The carbon mineralized inorganic artificial stone body with the mold is transported to a steam curing box for curing at a temperature of 60° C. for 7 hours.
[0147] S4. After the curing is completed, it is sent to the mineralization reactor for reaction. After the air is replaced by the gas containing carbon dioxide, the pressure is increased to 0.5MPa, the temperature is raised to 80°C, and the reaction is kept at this temperature for 3h;
[0148] S5. After the reaction is completed, demoulding, drying, thickness determination, grinding and polishing, and protective treatment are performed to obtain carbon mineralized inorganic artificial stone.
[0149] In this embodiment, the mass ratio of the solid waste powder (steel slag) to the phenol compound (resorcinol) is 50:10=1:0.2, and the mass ratio of the phenol compound (resorcinol) to the enhancer (polyacrylic acid) is 10:6.5=1:0.65.
[0150] Example 2
[0151] The raw materials for preparing a carbon mineralized inorganic artificial stone include: 20 parts of modified powder (250 mesh), 6 parts of auxiliary quartz powder (200 mesh), 7.5 parts of inorganic filler slag (60 mesh), 35 parts of solid waste aggregate steel slag particles (4 mm), 1 part of fiber basalt fiber (diameter 13 μm, length 16 mm), 0.3 parts of water reducing agent polycarboxylic acid water reducing agent, and 0.3 parts of water repellent octyltriethoxysilane.
[0152] A method for preparing carbon mineralized inorganic artificial stone comprises the following steps:
[0153] S1. Preparation of carbon mineralized inorganic artificial stone slurry
[0154] S11, taking 30 parts of 130-mesh solid waste powder (steel slag) treated by wet grinding, adding 3 parts of phenolic compounds (resorcinol) and 1 part of reinforcing agent (polyacrylic acid) in sequence, mixing evenly, and stirring for 6 minutes to obtain a mixed material;
[0155] Among them, the wet grinding treatment of solid waste powder (steel slag) is as follows: at room temperature, the moisture content of the solid waste raw material steel slag is maintained at 35%, wet grinding is performed for 2 hours, and then drying is performed at 40°C to a moisture content of 5% to obtain solid waste powder.
[0156] S12, putting the mixed material into a mineralization reactor, replacing the air with a carbon dioxide-containing gas with a carbon dioxide concentration of 70%, pressurizing it to 0.5MPa, heating it to 80°C, and keeping it warm for 6 hours. After the reaction is completed, grinding the product into 230 mesh to obtain a modified powder;
[0157] S13, take 20 parts of modified powder, 6 parts of auxiliary materials (quartz powder), 7.5 parts of inorganic filler (slag), 35 parts of solid waste aggregate (steel slag particles), 1 part of fiber (basalt fiber), 0.3 parts of water reducer (polycarboxylate water reducer), 0.3 parts of water repellent (octyl triethoxy silane) and water and mix them evenly to obtain carbon mineralized inorganic artificial stone slurry, and keep its water content at 10%wt;
[0158] S2. Break up the carbon mineralized inorganic artificial stone slurry, spread it, and transfer it to a press. Vibrate and press the mixed material under vacuum to obtain a carbon mineralized inorganic artificial stone blank fixed by a mold; the vacuum degree is -0.1MPa, and the pressure of the pressing head is 1MPa.
[0159] S3. The carbon mineralized inorganic artificial stone body with the mold is transported to a steam curing box for curing at a temperature of 50° C. for 8 hours.
[0160] S4. After the curing is completed, it is sent to the mineralization reactor for reaction. After the air is replaced by the gas containing carbon dioxide, the pressure is increased to 0.2MPa, the temperature is raised to 90°C, and the reaction is kept warm for 4 hours.
[0161] S5. After the reaction is completed, demoulding, drying, thickness determination, grinding and polishing, and protective treatment are performed to obtain carbon mineralized inorganic artificial stone.
[0162] In this embodiment, the mass ratio of the solid waste powder (steel slag) to the phenol compound (resorcinol) is 30:3=1:0.1, and the mass ratio of the phenol compound (resorcinol) to the enhancer (polyacrylic acid) is 3:1=1:0.33.
[0163] Example 3
[0164] The raw materials for preparing a carbon mineralized inorganic artificial stone include: 51 parts of modified powder (450 mesh), 15.5 parts of auxiliary quartz powder (280 mesh), 19.5 parts of inorganic filler slag (200 mesh), 90 parts of solid waste aggregate steel slag particles (1 mm), 2.6 parts of fiber basalt fiber (diameter 20 μm, length 10 mm), 0.8 parts of water reducing agent polycarboxylic acid water reducing agent, and 0.8 parts of water repellent octyltriethoxysilane.
[0165] A method for preparing carbon mineralized inorganic artificial stone comprises the following steps:
[0166] S1. Preparation of carbon mineralized inorganic artificial stone slurry
[0167] S11, taking 70 parts of 270-mesh solid waste powder (steel slag) that has been wet-milled, adding 20 parts of phenolic compound (resorcinol) and 18 parts of reinforcing agent (polyacrylic acid) in sequence, mixing evenly, and stirring for 10 minutes to obtain a mixed material;
[0168] Among them, the wet grinding treatment of solid waste powder (steel slag) is as follows: at room temperature, the moisture content of the solid waste raw material steel slag is maintained at 65%, wet grinding is performed for 0.5 h, and then drying is performed at 60°C to a moisture content of 10% to obtain solid waste powder.
[0169] S12, putting the mixed material into a mineralization reactor, replacing the air with a carbon dioxide-containing gas with a carbon dioxide concentration of 80%, pressurizing it to 0.3MPa, heating it to 100°C, and keeping it warm for 2h. After the reaction is completed, grinding the product to 450 mesh to obtain a modified powder;
[0170] S13, take 51 parts of modified powder, 15.5 parts of auxiliary material (quartz powder), 19.5 parts of inorganic filler (slag), 90 parts of solid waste aggregate (steel slag particles), 2.6 parts of fiber (basalt fiber), 0.8 parts of water reducer (polycarboxylate water reducer), 0.8 parts of water repellent (octyl triethoxy silane) and water and mix them evenly to obtain carbon mineralized inorganic artificial stone slurry, and keep its water content at 15%wt;
[0171] S2. Break up the carbon mineralized inorganic artificial stone slurry, spread it, and transfer it to a press. Vibrate and press the mixed material under vacuum to obtain a carbon mineralized inorganic artificial stone body fixed by a mold; the vacuum degree is -0.09MPa, and the pressure of the pressing head is 2MPa.
[0172] S3. The carbon mineralized inorganic artificial stone body with the mold is transported to a steam curing box for curing at a temperature of 70° C. for 6 hours.
[0173] S4. After the curing is completed, it is sent to the mineralization reactor for reaction. After the air is replaced by the gas containing carbon dioxide, the pressure is increased to 1MPa, the temperature is raised to 70°C, and the reaction is kept at this temperature for 2h;
[0174] S5. After the reaction is completed, demoulding, drying, thickness determination, grinding and polishing, and protective treatment are performed to obtain carbon mineralized inorganic artificial stone.
[0175] In this embodiment, the mass ratio of solid waste powder (steel slag) to phenol compound (resorcinol) is 70:20=1:0.29, and the mass ratio of resorcinol to enhancer (polyacrylic acid) is 20:18=1:0.9.
[0176] Example 4
[0177] Example 4 is basically the same as Example 1, the main difference being that in the process of preparing the modified powder in step S1, the masses of the added solid waste powder and the phenolic compound are different, specifically, 57 parts of the added solid waste powder (steel slag), 3 parts of the phenolic compound (resorcinol), and 6.5 parts of the enhancer (polyacrylic acid).
[0178] In this embodiment, the mass ratio of solid waste powder (steel slag) to phenol compound (resorcinol) is 57:3=1:0.05.
[0179] Example 5
[0180] Example 5 is basically the same as Example 1, the main difference being that in the process of preparing the modified powder in step S1, the masses of the added solid waste powder and the phenolic compound are different, specifically, 43 parts of the added solid waste powder (steel slag), 17 parts of the phenolic compound (resorcinol), and 6.5 parts of the enhancer (polyacrylic acid).
[0181] In this embodiment, the mass ratio of steel slag to resorcinol is 43:17=1:0.4.
[0182] Example 6
[0183] Example 6 is basically the same as Example 1, the main difference being that in the process of preparing the modified powder in step S1, the masses of the added phenolic compound and the enhancer are different, specifically, 14 parts of the added phenolic compound (resorcinol), 2.5 parts of the enhancer (polyacrylic acid), and 50 parts of the solid waste powder (steel slag).
[0184] In this embodiment, the mass ratio of the phenol compound (resorcinol) to the enhancer (polyacrylic acid) is 14:2.5=1:0.18.
[0185] Example 7
[0186] Example 7 is basically the same as Example 1, the main difference being that in the process of preparing the modified powder in step S1, the masses of the added phenolic compound and the enhancer are different, specifically, 8 parts of the added phenolic compound (resorcinol), 8.5 parts of the enhancer (polyacrylic acid), and 50 parts of the solid waste powder (steel slag).
[0187] In this embodiment, the mass ratio of the phenol compound (resorcinol) to the enhancer (polyacrylic acid) is 8:8.5=1:1.06.
[0188] Comparative Example 1
[0189] Comparative Example 1 is basically the same as Example 1, with the main difference being that in step S1, step S11 is not performed, and in step S12, the wet-grinded solid waste powder (steel slag) is directly placed in the mineralization reactor. That is, the solid waste powder is only mineralized, and no phenolic compound and enhancer are added to modify the solid waste powder.
[0190] Comparative Example 2
[0191] Comparative Example 2 is substantially the same as Example 1, except that in step S11, 50 parts of 200-mesh solid waste powder (steel slag) treated with wet grinding are taken, 16.5 parts of reinforcing agent (polyacrylic acid) are added, mixed evenly, and stirred for 8 minutes to obtain a mixed material. That is, in the process of preparing the modified powder, only 16.5 parts of reinforcing agent (polyacrylic acid) are added, and no phenolic compound (resorcinol) is added.
[0192] Comparative Example 3
[0193] Comparative Example 3 is basically the same as Example 1, except that in step S11, 50 parts of 200-mesh solid waste powder (steel slag) treated with wet grinding are taken, 16.5 parts of phenolic compound (resorcinol) are added, mixed evenly, and stirred for 8 minutes to obtain a mixed material. That is, in the process of preparing the modified powder, only 16.5 parts of phenolic compound (resorcinol) are added, and no reinforcing agent (polyacrylic acid) is added.
[0194] Comparative Example 4
[0195] Comparative Example 4 is basically the same as Example 1, except that in step S1, resorcinol and polyacrylic acid are directly added to the carbon mineralized inorganic artificial stone slurry. The specific steps are:
[0196] S1. Preparation of carbon mineralized inorganic artificial stone slurry
[0197] S11, weigh 50 parts of 200-mesh solid waste powder (steel slag) treated with wet grinding, put it into a mineralization reactor, replace the air with a carbon dioxide-containing gas with a carbon dioxide concentration of 90%, pressurize it to 0.1MPa, heat it to 90°C, keep it warm for 4 hours, grind it to 300 mesh, and obtain mineralized solid waste powder (steel slag);
[0198] S12, take 27.1 parts of mineralized solid waste powder (steel slag), 5.4 parts of phenolic compounds (resorcinol), 3.5 parts of reinforcing agent (polyacrylic acid), 10.8 parts of auxiliary materials (quartz powder), 13.6 parts of inorganic filler (slag), 63 parts of solid waste aggregate (steel slag particles), 1.8 parts of fiber (basalt fiber), 0.5 parts of water reducer (polycarboxylic acid water reducer), 0.5 parts of water repellent (octyl triethoxy silane) and water and mix them evenly to obtain carbon mineralized inorganic artificial stone slurry, keeping its water content at 12%wt.
[0199] Comparative Example 5
[0200] Comparative Example 5 is substantially the same as Example 1, the main difference being that in step S1, no auxiliary material (quartz powder) is added, and the amount of inorganic filler (slag) added is 24.4 parts.
[0201] Experimental Examples
[0202] The flexural strength, compressive strength, water absorption and glossiness of the inorganic artificial large panels prepared in Examples 1-7 and Comparative Examples 1-5 were tested, and the test results are shown in Table 1. Among them:
[0203] With reference to JC / T2604-2021 "Stone-like concrete panels and tiles", the flexural strength and compressive strength tests were performed on the carbon mineralized inorganic artificial stones obtained in Examples 1-7 and Comparative Examples 1-5.
[0204] With reference to GB / T4111-2013 “Test methods for concrete blocks and bricks”, the water absorption rate of the carbon mineralized inorganic artificial stones obtained in Examples 1-7 and Comparative Examples 1-5 was tested.
[0205] With reference to GB / T13891-2008 “Method for Determining Specular Gloss of Building Finishing Materials”, the glossiness of the carbon mineralized inorganic artificial stones obtained in Examples 1-7 and Comparative Examples 1-5 was tested.
[0206] The carbon fixation rate is the difference in carbon dioxide concentration in the mineralization reactor before and after the mineralization reaction.
[0207] Table 1:
[0208]
[0209] In Examples 1 to 3, by limiting the type and amount of raw materials and adjusting the preparation process, the prepared carbon mineralized inorganic artificial stone has high mechanical strength, good impermeability, and gloss. The flexural strength reaches more than 25.7 MPa, the compressive strength reaches more than 157.9 MPa, the carbon fixation rate reaches more than 26.0%, the water absorption rate reaches less than 2.4%, and the glossiness reaches more than 58°.
[0210] Compared with Example 1, Example 4 uses less resorcinol, which may lead to a decrease in the benzene ring content on the surface of the solid waste powder steel slag, which not only makes the solid waste powder steel slag itself prone to agglomeration, but also causes it to be unevenly dispersed in the carbon mineralized inorganic artificial stone, affecting the internal structure of the product, and causing the mechanical properties and gloss to decline; and the reduction in the amount of resorcinol reduces the absorption of carbon dioxide, but due to the increase in the steel slag content, the overall carbon fixation rate does not decrease significantly; in addition, the generated substances that can form a complex with polyacrylic acid are reduced, and the holes and gaps in the steel slag cannot be effectively filled, so that the strength and hydrophobicity of the carbon mineralized inorganic artificial stone slurry are also reduced, so the strength of the product deteriorates and the water absorption rate increases.
[0211] Compared with Example 1, there is more resorcinol in Example 5, and the uniform dispersibility of solid waste powder steel slag and the impermeability of carbon mineralized inorganic artificial stone are improved. However, from the data, the participation of too much resorcinol does not contribute to the improvement of the performance of carbon mineralized inorganic artificial stone. On the contrary, the strength data decreases slightly. This may be due to the fact that too much resorcinol cannot further play the role of filling holes and gaps, but leads to a decrease in the content of steel slag in the modified powder. Although the increase of resorcinol can absorb more carbon dioxide, due to the reduction of steel slag content and the complex coated on the outer layer of steel slag, the contact between carbon dioxide and steel slag is affected, so the overall carbon fixation rate is reduced. It can be seen that, combined with the test data of Examples 1-5, the mass ratio of steel slag and resorcinol is preferably 1: (0.1-0.3).
[0212] Compared with Example 1, the reason why the performance of the other products in Example 6, except for the carbon fixation rate, is reduced may be that: although resorcinol helps to absorb more carbon dioxide to generate products, further improving the carbon fixation rate, the limited polyacrylic acid reduces the amount of the overall complex formed between it and the product, and the filling rate of the pores and cracks on the surface of the solid waste powder steel slag is reduced, affecting the density and impermeability of the product; at the same time, too little polyacrylic acid cannot provide good bonding strength to the system, which also leads to a decrease in the density of the carbon mineralized inorganic artificial stone system, so its various performances are reduced.
[0213] Compared with Example 1, the performance of the product in Example 7 is reduced. The reason may be that the amount of substances generated by resorcinol in cooperation with alkali metal salts and carbon dioxide on the surface of solid waste powder is reduced. Although there is enough polyacrylic acid to form a complex with the substances generated by resorcinol to fill the pores and cracks of the solid waste powder steel slag, the amount of the complex is reduced due to the reduction in the amount of substances generated by resorcinol, thereby deteriorating the density of the product. Therefore, combined with the test data of Examples 1-3, 6, and 7, the mass ratio of resorcinol to polyacrylic acid is preferably 1: (0.3-0.9).
[0214] Compared with Example 1, the reasons for the decline in various properties of the product in Comparative Example 1 may be: in Comparative Example 1, on the one hand, the lack of resorcinol and polyacrylic acid cannot absorb carbon dioxide and generate complexes, and there are still a large number of pores and cracks on the solid waste powder steel slag, and the internal structure of the product cannot be effectively optimized, resulting in poor density; on the other hand, the lack of polyacrylic acid cannot provide bonding strength for the components of the system, which also leads to the deterioration of the internal structure of the carbon mineralized inorganic artificial stone and the reduction of density, so its various properties are reduced. In addition, compared with Example 1, its absorption of carbon dioxide is also relatively reduced.
[0215] Compared with Example 1, in Comparative Example 2, the solid waste powder steel slag is not modified by using resorcinol, which may result in the introduction of benzene rings on the surface of the modified steel slag, a higher degree of powder agglomeration, and poorer mechanical strength and impermeability, affecting the mechanical properties and water absorption rate of the carbon mineralized inorganic artificial stone, and being unable to absorb carbon dioxide and unable to form a complex with polyacrylic acid to fill the internal holes and gaps of the steel slag. The density of the solid waste powder steel slag is reduced, so the various performances of the carbon mineralized inorganic artificial stone are significantly reduced.
[0216] Compared with Example 1, in Comparative Example 3, polyacrylic acid is not used to modify the steel slag, which may result in: on the one hand, it is unable to further form a complex with the substance generated by resorcinol to effectively fill the pores and cracks on the surface of the solid waste powder steel slag, resulting in a significant decrease in the density of the product; on the other hand, it leads to a decrease in the bonding strength between the components of the system, the internal structure of the carbon mineralized inorganic artificial stone deteriorates, and the density is further reduced, so the mechanical strength, impermeability and gloss of the product are all reduced.
[0217] Compared with Example 1, the various properties of the product in Comparative Example 4 are significantly reduced. The reason may be that in Comparative Example 4, resorcinol and polyacrylic acid are directly added to the carbon mineralized inorganic artificial stone slurry. This process cannot activate the ortho-carbon of the phenolic hydroxyl group in the phenol compound, and there is no carbon dioxide. It is even more impossible for the activated product to further undergo a nucleophilic addition reaction with carbon dioxide, and ultimately it is impossible to form a complex with polyacrylic acid, and it is impossible to optimize the pore structure of the solid waste powder steel slag, and the internal structure of the carbon mineralized inorganic artificial stone blank is not significantly adjusted, and the mechanical properties of the carbon mineralized inorganic artificial stone are not significantly improved.
[0218] Comparative Example 5 is compared with Example 1. In Comparative Example 5, the amount of auxiliary material added is changed to inorganic filler. Without the addition of auxiliary material, the glossiness of the carbon mineralized inorganic artificial stone is significantly deteriorated, and the compressive strength and flexural strength are slightly decreased.
[0219] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A carbon mineralized inorganic artificial stone, characterized in that: By mass, the raw materials include: 15-70 parts of modified powder, 3-25 parts of auxiliary materials, 5-28 parts of inorganic fillers, 20-120 parts of solid waste aggregates, 1-7 parts of fibers, 0.2-2.0 parts of water repellent, and 0.2-1.5 parts of water reducing agent; The raw materials for preparing the modified powder include solid waste powder, phenolic compounds and a reinforcing agent; The mass ratio of the solid waste powder to the phenol compound is 1:(0.05-0.5); The mass ratio of the phenol compound to the enhancer is 1:(0.1-1.2); The solid waste powder includes alkali metal salts; the solid waste raw material used to prepare the solid waste powder is steel slag; The reinforcing agent is at least one of polyacrylic acid and chloroacetic acid resin; The auxiliary material is selected from any one or two of quartz powder and granite; The solid waste aggregate is selected from steel slag particles; The preparation method of the modified powder is as follows: phenol compounds and enhancers are added to solid waste powder, and a gas containing carbon dioxide is introduced to mineralize and modify the solid waste powder to obtain the modified powder.
2. The carbon mineralized inorganic artificial stone according to claim 1, characterized in that: The mass ratio of the solid waste powder to the phenol compound is 1:(0.1-0.3); the mass ratio of the phenol compound to the enhancer is 1:(0.3-0.9).
3. The carbon mineralized inorganic artificial stone according to claim 1, characterized in that: The phenol compound is at least one of resorcinol, m-aminophenol, 4-methylcatechol, 4-isopropylphenol and 2-sec-butylphenol.
4. The carbon mineralized inorganic artificial stone according to claim 1, characterized in that: The raw materials for preparation include, by mass: 20-51 parts of modified powder, 6-16 parts of auxiliary materials, 7-20 parts of inorganic fillers, 35-90 parts of solid waste aggregates, 2-5 parts of fibers, 0.3-0.8 parts of water repellent, and 0.3-0.8 parts of water reducing agent; The average particle size of the auxiliary material is 150-400 mesh; The average particle size of the inorganic filler is 50-300 mesh; The average particle size of the solid waste aggregate is 0.01-8 mm; The average diameter of the fibers is 10-20 μm and the length is 8-19 mm.
5. The carbon mineralized inorganic artificial stone according to claim 1, characterized in that: The inorganic filler is selected from any one or more of slag, fly ash, and fine tailings; The fiber is selected from any one or more of basalt fiber, polypropylene fiber, and glass fiber; The hydrophobic agent is selected from any one or more of octyltriethoxysilane, calcium stearate, and methyl calcium silicate; The water reducer is selected from any one or more of polycarboxylate water reducer and naphthalene water reducer; The average particle size of the auxiliary material is 200-300 mesh; The average particle size of the inorganic filler is 60-240 mesh; The average particle size of the solid waste aggregate is 0.01-5 mm.
6. The carbon mineralized inorganic artificial stone according to claim 1, characterized in that: The modified powder preparation step comprises: (1) Take solid waste powder, add phenol compound and enhancer in sequence, stir evenly, and obtain a mixed material; (2) Put the mixed material into a mineralization reactor, replace the air with a gas containing carbon dioxide, pressurize it to 0.1-1MPa, raise the temperature to 60-100°C, and keep the temperature for 1-8h. After the reaction is completed, grind the product to obtain a modified powder; The mass concentration of carbon dioxide in the carbon dioxide-containing gas is 8-100%; The fiber is selected from any one or more of basalt fiber and polypropylene fiber; The water repellent is selected from any one or more of octyltriethoxysilane and calcium stearate.
7. The carbon mineralized inorganic artificial stone according to claim 6, characterized in that: The solid waste powder is obtained by wet grinding of solid waste raw materials; The average particle size of the solid waste powder is 100-300 mesh; The mass concentration of carbon dioxide in the carbon dioxide-containing gas is 50-100%.
8. A method for preparing the carbon mineralized inorganic artificial stone according to any one of claims 1 to 7, characterized in that: The steps include: S1. Take the modified powder, auxiliary materials, solid waste aggregate, fiber, water reducing agent, water repellent and water and mix them evenly to obtain carbon mineralized inorganic artificial stone slurry, and keep its water content at 8-15wt%; S2, breaking up the carbon mineralized inorganic artificial stone slurry, spreading it, transferring it to a press, and vibrating and pressing the mixed material under vacuum to obtain a carbon mineralized inorganic artificial stone blank fixed by a mold; S3, transporting the carbon mineralized inorganic artificial stone body with the mold to a steam curing box for curing; S4. After the curing is completed, the product is sent to a mineralization reactor for reaction, and the air is replaced by a gas containing carbon dioxide, and then a mineralization reaction is carried out; S5. After the reaction is completed, demoulding, drying, thickness determination, grinding and polishing, and protective treatment are performed to obtain carbon mineralized inorganic artificial stone.
9. The method for preparing the carbon mineralized inorganic artificial stone according to claim 8, characterized in that: In step S2, the vacuum degree of vibration pressing is -0.09 to -0.1 MPa, and the pressure of the pressure head is 0.1 to 5 MPa; In step S3, the curing temperature is 40-100° C. and the curing time is 2-10 hours; In step S4, the pressure of the mineralization reaction is 0.1-1 MPa, the temperature is 60-100° C., and the reaction time is 1-8 h.