A preparation method of emulsion polymerization terpolymer and its product and application

Through the two-stage initiation polymerization method, the problems of uneven catalyst distribution and emulsion polymerization in hydrogen fuel cells are solved, the reaction rate and performance of the catalyst are improved, and stable and efficient production is achieved.

CN118684806BActive Publication Date: 2024-11-08FUJIAN KERUN CENTURY HYDROGEN ENERGY MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411160723.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-08
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

In the existing hydrogen fuel cells, the distribution of the catalyst Pt is uneven, resulting in a low reaction rate of the positive electrode ORR, excessive catalyst usage, and difficult to achieve emulsion polymerization terpolymers or poor performance.

Method used

The second stage initiation polymerization method is adopted, firstly, the initial polymerization is performed in the oil-soluble first initiator to form particles with low polymerization degree, and then further polymerization is performed in the water-soluble second initiator to obtain a high molecular weight ionomer to improve the catalyst Proton conductivity and oxygen permeability.

Benefits of technology

The uniform distribution of catalysts is achieved, the reaction rate and catalytic effect of hydrogen fuel cells are improved, and the production process is stable, the temperature is easy to control, and it is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure 3DN9PVMEDC2T5SICNY6QAOI1LXN6WCOPPZESWJIV
    Figure 3DN9PVMEDC2T5SICNY6QAOI1LXN6WCOPPZESWJIV
Patent Text Reader

Abstract

The invention discloses a preparation method of an emulsion polymerization terpolymer, and its product and application. The preparation method comprises the following steps: (1) hydrolyzing an oxyperfluoroolefin having a sulfonyl fluoride group to obtain an oxyperfluoroolefin solution having a sulfonate group; (2) adding a perfluorodimethyldioxole monomer and an oxyperfluoroolefin solution having a sulfonate group to a reactor; (3) adding a first initiator solution to a reactor to obtain an initial reaction emulsion; (4) adding deionized water and an emulsifier to the initial reaction emulsion, and adjusting the pH to 8-9; (5) adding a second initiator, injecting tetrafluoroethylene monomer into the initial reaction emulsion through a pipeline, heating to 80-90°C, and maintaining the reaction for 12-24 hours; (6) cooling to room temperature, releasing pressure, precipitating, filtering and removing a solidified material in the reactor, washing, devolatilizing, and drying; (7) hydrolyzing and hydrogenating the dried product of step (6) to obtain a terpolymer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hydrogen fuel cells, and in particular to a preparation method of an emulsion polymerization terpolymer, a product thereof and an application thereof. Background Art

[0002] The most important part of a hydrogen fuel cell is the catalyst. The catalytic efficiency of the catalyst directly determines the power of the entire fuel cell; at the same time, the amount of platinum (Pt) in the catalyst also plays an important role in the cost of the entire fuel cell. In fact, the distribution of Pt in the fuel cell is uneven (8 / 9 of the Pt / C catalyst is distributed at the positive electrode of the fuel cell). This is because in a hydrogen fuel cell, the negative electrode undergoes the HOR reaction H2→2e-+2H (two electron transfer, fast kinetic process), and the positive electrode undergoes the ORR reaction O2+4e-+4H+→2H2O (four electron transfer, slow kinetic process). According to theoretical calculations comparing the two reaction kinetic processes, the positive electrode ORR reaction rate is 6 orders of magnitude lower than the negative electrode HOR reaction, so the reaction rate of the total reaction depends on the positive electrode. The chemical reaction rate is proportional to the amount of Pt catalyst used, so the amount of catalyst used at the positive electrode is about 8 times that of the negative electrode.

[0003] The catalyst Pt / C is adhered between the proton exchange membrane (PEM) and the gas diffusion layer (GDL) by a polymer binder. The polymer binder is called an ionomer. The surface of the catalyst Pt is wrapped by the ionomer, and oxygen must first permeate through the ionomer before it can contact the catalyst Pt, thereby initiating the ORR reaction. Therefore, the oxygen permeability of the ionomer has a significant effect on the catalytic effect of Pt. The higher the oxygen permeability of the ionomer, the better the catalytic effect of Pt. Perfluorosulfonic acid resin poly (TFE-PDD-PSVE) is a new type of ionomer used in the positive electrode of hydrogen fuel cells in recent years. It is a terpolymer of tetrafluoroethylene monomer (TFE), perfluoro-2,2-dimethyl-1,3-dioxolane (PDD) and perfluorosulfonyl ethoxypropyl vinyl ether (PSVE).

[0004] At present, the synthesis process of poly(TFE-PDD-PSVE) publicly reported at home and abroad is basically bulk polymerization and solution polymerization, while emulsion polymerization is difficult to achieve or the performance of the obtained product is slightly inferior. Summary of the invention

[0005] In view of the problems existing in the background technology, the purpose of the present invention is to provide a method for preparing an emulsion polymerization terpolymer, which adopts a two-stage initiation polymerization, wherein oil-soluble diisopropyl peroxydicarbonate is dissolved in a first initiator solvent composed of trifluorotrichloroethane and 2-chloro-1,1,2-trifluoroethyl methyl ether to firstly polymerize the monomer droplets in the emulsion to obtain microparticles with a low degree of polymerization, and then a water-soluble second initiator is added to perform a second-stage polymerization reaction with the microparticles with a low degree of polymerization as the core, and finally obtain a high molecular weight ionomer, which has good comprehensive properties such as proton conductivity, oxygen permeability, and strength compared to traditional emulsion polymerization. The method is highly operable, easy to control temperature, and stable in production.

[0006] In order to achieve the above-mentioned object, the present invention provides a method for preparing an emulsion polymerization terpolymer, comprising the following steps: (1) hydrolyzing an oxyperfluoroolefin having a sulfonyl fluoride group with a 20wt% sodium hydroxide solution to obtain an oxyperfluoroolefin solution having a sulfonate group; (2) cleaning and drying a reaction kettle, passing ice water through the outer shell interlayer of the reaction kettle to control the temperature, and adding a perfluorodimethyldioxole monomer and an oxyperfluoroolefin solution having a sulfonate group into the reaction kettle; (3) adding a first initiator solution into the reaction kettle, stirring evenly and sealing the reaction kettle, and repeatedly performing vacuuming and nitrogen passing operations 2-3 times, controlling the temperature of the reaction kettle to 40-50°C, and cooling the reaction kettle to 0-5°C after a reaction time of 0.5-1h to obtain an initial reaction emulsion; the first initiator solution is a diisopropyl peroxydicarbonate solution. The method comprises the following steps: (1) adding deionized water and an emulsifier to the initial reaction emulsion in the reactor, and adding 20 wt % sodium hydroxide solution to adjust the pH value to 8-9; (2) adding a second initiator, purging the reactor with nitrogen and sealing it, injecting tetrafluoroethylene monomer into the initial reaction emulsion through a pipeline, closing the pipeline and maintaining the pressure at 1.5-1.8 MPa, heating to 80-90° C., and maintaining the reaction for 12-24 hours; continuing to fill with nitrogen and maintaining the pressure at 2-2.5 MPa, heating to 100-110° C. and maintaining the reaction for 1-3 hours; (3) cooling to room temperature, releasing the pressure, precipitating, filtering out the solidified product in the reactor, washing, devolatilizing, and drying; and (4) hydrolyzing and hydrogenating the dried product in step (6) to obtain a terpolymer.

[0007] Optionally, the structural formula of the perfluorodimethyldioxole monomer is:

[0008] or .

[0009] Optionally, the oxyperfluoroolefin having a sulfonyl fluoride group is perfluorosulfonyl ethoxypropyl vinyl ether, and the structural formula is CF2═CFOCF2CF(CF3)OCF2CF2SO2F; the structural formula of the oxyperfluoroolefin having a sulfonate group is CF2═CFOCF2CF(CF3)OCF2CF2SO2Na.

[0010] Optionally, the mass ratio of the tetrafluoroethylene monomer, the perfluorodimethyldioxole monomer, the oxoperfluoroolefin having a sulfonyl fluoride group, the first initiator and the second initiator is 5-10:10-20:30-50:0.5-1:1.5-2.

[0011] Optionally, the volume ratio of trifluorotrichloroethane to 2-chloro-1,1,2-trifluoroethyl methyl ether is 5:2-3; the ratio of the first initiator to the composite solvent is 0.5-1 g:0.1 mL.

[0012] Optionally, the second initiator is one or a combination of ammonium persulfate, sodium persulfate and potassium persulfate.

[0013] Optionally, the emulsifier is one or a combination of sodium dodecyl sulfate, sodium dodecyl sulfonate, ammonium perfluorooctanoate and sodium perfluorooctanoate.

[0014] The present invention also provides a terpolymer obtained by the preparation method as described above.

[0015] The present invention also provides an application of the terpolymer as described above, which is applied to a Pt / C catalyst layer of a hydrogen fuel cell.

[0016] The beneficial effects of the present invention are as follows:

[0017] 1. The present invention is the first to alkaline hydrolyze the oxygen-perfluoroolefin with sulfonyl fluoride group to obtain hydrophilic sulfonate group, which has hydrophobic and hydrophilic properties, and can make the perfluorodimethyldioxole monomer and the oxygen-perfluoroolefin with sulfonate group form tiny agglomerated microdroplets; the first initiator diisopropyl peroxydicarbonate easily enters the microdroplets in a specific composite solvent of trifluorotrichloroethane and 2-chloro-1,1,2-trifluoroethyl methyl ether to initiate the first stage polymerization reaction, and the reaction temperature is controlled to form microparticles with low polymerization degree. The second initiator soluble in water is added to the second stage, and deionized water and emulsifier are added, and the emulsion polymerization is continued by heating. The tetrafluoroethylene monomer in the solution enters the micelle with the microparticle as the core, and undergoes polymerization reaction with the remaining perfluorodimethyldioxole monomer and the oxygen-perfluoroolefin with sulfonate group to obtain a high molecular weight ionomer. The ionomer has good comprehensive properties such as proton conductivity, oxygen permeability, and strength. This indicates that the polymer framework of the microparticles composed of the perfluorodimethyldioxole monomer and the oxyperfluoroolefin with a sulfonate group in the first stage polymerization reaction is beneficial to the subsequent polymerization reaction and it is easy to obtain a high molecular weight ionomer. Moreover, the oxygen permeability of the ionomer is not reduced by the addition of tetrafluoroethylene, and better strength is obtained.

[0018] 2. The synthesis method of the present invention is controllable, the production process is stable, and it is easy to obtain oxygen-permeable ionomers with a desired molecular weight distribution. The product performance qualification rate is high and it is suitable for large-scale production. DETAILED DESCRIPTION

[0019] In order to make the above-mentioned objects, features and advantages of the invention more obvious and easy to understand, the specific embodiments of the invention are described in detail below.

[0020] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0021] The preparation method of the emulsion polymerization terpolymer according to the present invention comprises the following steps: (1) hydrolyzing an oxyperfluoroolefin having a sulfonyl fluoride group with a 20wt% sodium hydroxide solution to obtain an oxyperfluoroolefin solution having a sulfonate group; (2) cleaning and drying a reaction kettle, passing ice water through the outer shell interlayer of the reaction kettle to control the temperature, and adding a perfluorodimethyldioxole monomer and an oxyperfluoroolefin solution having a sulfonate group into the reaction kettle; (3) adding a first initiator solution into the reaction kettle, stirring evenly and sealing the reaction kettle, and repeating the vacuum and nitrogen gas flow operation for 2-3 times, controlling the temperature of the reaction kettle to 40-50°C, and cooling the reaction kettle to 0-5°C after a reaction time of 0.5-1h to obtain an initial reaction emulsion; the first initiator solution is prepared by dissolving diisopropyl peroxydicarbonate in trichlorotrifluoroethane (F 113) and 2-chloro-1,1,2-trifluoroethyl methyl ether; (4) adding deionized water and an emulsifier to the initial reaction emulsion in the reactor, and adding 20wt% sodium hydroxide solution to adjust the pH to 8-9; (5) adding a second initiator, purging the reactor with nitrogen and sealing it, injecting tetrafluoroethylene monomer into the initial reaction emulsion through a pipeline, closing the pipeline and maintaining the pressure at 1.5-1.8Mpa, raising the temperature to 80-90°C, and maintaining the reaction for 12-24h; continuing to fill with nitrogen and maintaining the pressure at 2-2.5Mpa, heating to 100-110°C and maintaining for 1-3h; (6) cooling to room temperature, releasing the pressure, precipitating, filtering out the solidified material in the reactor, washing, devolatilizing, and drying; (7) hydrolyzing and hydrogenating the dried product in step (6) to obtain a terpolymer.

[0022] In the preparation method of the emulsion polymerization terpolymer according to the present invention, the structural formula of the perfluorodimethyldioxole monomer is:

[0023] or .

[0024] In the preparation method of the emulsion polymerization terpolymer according to the present invention, the oxyperfluoroolefin having a sulfonyl fluoride group is perfluorosulfonylethoxypropyl vinyl ether (PSVE), and the structural formula is CF2═CFOCF2CF(CF3)OCF2CF2SO2F; the structural formula of the oxyperfluoroolefin having a sulfonate group is CF2═CFOCF2CF(CF3)OCF2CF2SO2Na.

[0025] In the preparation method of the emulsion polymerization terpolymer according to the present invention, the mass ratio of the tetrafluoroethylene monomer, the perfluorodimethyldioxole monomer, the oxoperfluoroolefin having a sulfonyl fluoride group, the first initiator and the second initiator may be 5-10:10-20:30-50:0.5-1:1.5-2.

[0026] In the preparation method of the emulsion polymerization terpolymer according to the present invention, the volume ratio of trifluorotrichloroethane (F113) and 2-chloro-1,1,2-trifluoroethyl methyl ether can be 5:2-3; the ratio of the first initiator and the composite solvent can be 0.5-1g:0.1mL.

[0027] In the method for preparing the emulsion polymerized terpolymer according to the present invention, the second initiator may be one or a combination of ammonium persulfate, sodium persulfate and potassium persulfate.

[0028] In the method for preparing the emulsion polymerization terpolymer according to the present invention, the emulsifier may be one or a combination of sodium dodecyl sulfate, sodium dodecyl sulfonate, ammonium perfluorooctanoate and sodium perfluorooctanoate.

[0029] The terpolymer according to the present invention can be applied to a Pt / C catalyst layer of a hydrogen fuel cell.

[0030] The preparation method of the emulsion polymerization terpolymer of the present invention, its product and application are specifically described below by way of examples. Main raw materials and equipment used: Unless otherwise specified, the raw materials and equipment of each embodiment and comparative example are the same; materials without specifying specific models or types are from the same common models purchased from the market, and are not specifically limited.

[0031] Example 1

[0032] (1) 30 kg of perfluorosulfonylethoxypropyl vinyl ether (PSVE) was hydrolyzed with 50 kg of 20 wt% sodium hydroxide solution to obtain a sodium perfluoroethoxypropyl vinyl ether sulfonate (PSVE-Na) solution;

[0033] (2) Clean and dry the reactor, pass ice water through the outer shell of the reactor to control the temperature, and add 10 kg of perfluorodimethyldioxole monomer (PDD) and sodium perfluoroethoxypropyl vinyl ether sulfonate (PSVE-Na) solution into the reactor;

[0034] (3) 0.5 kg of diisopropyl peroxydicarbonate was dissolved in 100 mL of a composite solvent (the volume ratio of F113 and 2-chloro-1,1,2-trifluoroethyl methyl ether was 2:1) to obtain a first initiator solution; the first initiator solution was added to a reactor, stirred evenly and the reactor was sealed, and the vacuum and nitrogen were repeatedly operated twice, the reactor temperature was controlled at 40°C, and the reaction time was 0.5 h, and then the temperature was lowered to 0°C to obtain an initial reaction emulsion;

[0035] (4) Add 500 kg of deionized water and 2.5 kg of sodium dodecyl sulfate to the initial reaction emulsion in the reactor, and add 20 wt % sodium hydroxide solution to adjust the pH to 8-9;

[0036] (5) Add 1.5 kg of ammonium persulfate, purge the reactor with nitrogen and seal it, inject 5 kg of tetrafluoroethylene monomer into the initial reaction emulsion through the pipeline, close the pipeline and maintain the pressure at 1.5 MPa, raise the temperature to 80 °C, and keep the reaction for 12 h; continue to fill with nitrogen to maintain the pressure at 2 MPa, heat to 100 °C and keep it for 1 h;

[0037] (6) Cooling to room temperature, releasing pressure, precipitating, filtering out the solidified material in the reaction kettle, washing, devolatilizing, and drying;

[0038] (7) The dried product of step (6) is hydrolyzed and hydrogenated to obtain a terpolymer.

[0039] Example 2

[0040] (1) 50 kg of perfluorosulfonylethoxypropyl vinyl ether (PSVE) was hydrolyzed with 50 kg of 20 wt% sodium hydroxide solution to obtain a sodium perfluoroethoxypropyl vinyl ether sulfonate (PSVE-Na) solution;

[0041] (2) Clean and dry the reactor, pass ice water through the outer shell of the reactor to control the temperature, and add 20 kg of perfluorodimethyldioxole monomer (PDD) and sodium perfluoroethoxypropyl vinyl ether sulfonate (PSVE-Na) solution into the reactor;

[0042] (3) 1 kg of diisopropyl peroxydicarbonate was dissolved in 100 mL of a composite solvent (the volume ratio of F113 and 2-chloro-1,1,2-trifluoroethyl methyl ether was 2:1) to obtain a first initiator solution; the first initiator solution was added to a reactor, stirred evenly and the reactor was sealed, and the vacuum and nitrogen were repeatedly operated for 3 times. The reactor temperature was controlled at 50°C, and the reaction time was 1 hour, and then the temperature was lowered to 5°C to obtain an initial reaction emulsion;

[0043] (4) Add 500 kg of deionized water and 3 kg of sodium dodecyl sulfate to the initial reaction emulsion in the reactor, and add 20 wt % sodium hydroxide solution to adjust the pH to 8-9;

[0044] (5) Add 2 kg of ammonium persulfate, purge the reactor with nitrogen and seal it, inject 10 kg of tetrafluoroethylene monomer into the initial reaction emulsion through the pipeline, close the pipeline and maintain the pressure at 1.8 MPa, raise the temperature to 90 °C, and keep the reaction for 24 hours; continue to fill with nitrogen and maintain the pressure at 2.5 MPa, heat to 110 °C and keep it for 3 hours;

[0045] (6) Cooling to room temperature, releasing pressure, precipitating, filtering out the solidified material in the reaction kettle, washing, devolatilizing, and drying;

[0046] (7) The dried product of step (6) is hydrolyzed and hydrogenated to obtain a terpolymer.

[0047] Example 3

[0048] (1) 40 kg of perfluorosulfonylethoxypropyl vinyl ether (PSVE) was hydrolyzed with 50 kg of 20 wt% sodium hydroxide solution to obtain a sodium perfluoroethoxypropyl vinyl ether sulfonate (PSVE-Na) solution;

[0049] (2) Clean and dry the reactor, pass ice water through the outer shell of the reactor to control the temperature, and add 15 kg of perfluorodimethyldioxole monomer (PDD) and sodium perfluoroethoxypropyl vinyl ether sulfonate (PSVE-Na) solution into the reactor;

[0050] (3) 0.8 kg of diisopropyl peroxydicarbonate was dissolved in 100 mL of a composite solvent (the volume ratio of F113 and 2-chloro-1,1,2-trifluoroethyl methyl ether was 2:1) to obtain a first initiator solution; the first initiator solution was added to a reactor, stirred evenly and the reactor was sealed, and the vacuum and nitrogen were repeatedly operated for 3 times. The reactor temperature was controlled at 45°C, and the reaction time was 1 hour and then the temperature was lowered to 2°C to obtain an initial reaction emulsion;

[0051] (4) Add 500 kg of deionized water and 3 kg of sodium perfluorooctanoate to the initial reaction emulsion in the reactor, and add 20 wt % sodium hydroxide solution to adjust the pH to 8-9;

[0052] (5) Add 1.8 kg of sodium persulfate, purge the reactor with nitrogen and seal it, inject 8 kg of tetrafluoroethylene monomer into the initial reaction emulsion through the pipeline, close the pipeline and maintain the pressure at 1.7 MPa, raise the temperature to 85 °C, and keep the reaction for 18 hours; continue to fill with nitrogen to maintain the pressure at 2.35 MPa, heat to 105 °C and keep it for 2 hours;

[0053] (6) Cooling to room temperature, releasing pressure, precipitating, filtering out the solidified material in the reaction kettle, washing, devolatilizing, and drying;

[0054] (7) The dried product of step (6) is hydrolyzed and hydrogenated to obtain a terpolymer.

[0055] Comparative Example 1

[0056] (1) Clean and dry the reactor, pass ice water through the outer shell of the reactor to control the temperature, and add a solution consisting of 15 kg PDD, 40 kg PSVE and 50 kg deionized water into the reactor;

[0057] (2) Add 500 kg of deionized water and 3 kg of sodium perfluorooctanoate into the reactor, and add 20 wt% sodium hydroxide solution to adjust the pH to 8-9;

[0058] (3) Add 1.8 kg of sodium persulfate, purge the reactor with nitrogen and seal it, inject 8 kg of tetrafluoroethylene monomer into the initial reaction emulsion through the pipeline, close the pipeline and maintain the pressure at 1.7 MPa, raise the temperature to 85 °C, and keep the reaction for 18 hours; continue to fill with nitrogen to maintain the pressure at 2.35 MPa, heat to 105 °C and keep it for 2 hours;

[0059] (4) Cooling to room temperature, releasing pressure, precipitating, filtering out the solidified material in the reaction kettle, washing, devolatilizing, and drying;

[0060] (5) The dried product of step (4) is hydrolyzed and hydrogenated to obtain a terpolymer.

[0061] Comparative Example 2

[0062] Except for omitting step (3), the rest is the same as Example 3.

[0063] Performance Testing

[0064] 1. The yield (ratio of product to raw material), exchange equivalent EW value (GB / T20042.3-2022) and number average molecular weight of the hydrogen-type ionomers of the examples and comparative examples were tested respectively.

[0065] 2. At 23°C and 0% relative humidity, the oxygen permeability of the catalyst layer after peeling off from the surface of the base membrane PET was tested using an instrument (MoconOX-Tran®, Minneapolis, MN, USA); at 80°C and 95% relative humidity, the catalyst layer was loaded into the electrolyte membrane of the electrochemical cell, the test electrodes were connected to both sides of the electrolyte membrane, an external voltage was applied, and the proton conductivity was calculated.

[0066] 3. After the hydrogen-type ionomer is dissolved in the solvent, it is cast into a film with a thickness of 0.5 mm; the mechanical strength of the hydrogen-type ionomer film is tested using a universal material testing machine (GB / T20042.3-2022).

[0067] See Table 1 for specific data.

[0068] Table 1

[0069]

[0070] It can be seen from the data of the examples and comparative examples that the present invention performs hydrolysis and alkalization and two-stage polymerization on perfluorosulfonylethoxypropyl vinyl ether in advance, with high yield, and can obtain a hydrogen-type ionomer film with excellent performance.

[0071] The above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the present invention.

Claims

1. A method for preparing an emulsion polymerization terpolymer, characterized in that: The steps include: (1) hydrolyzing an oxyperfluoroolefin having a sulfonyl fluoride group with a 20 wt % sodium hydroxide solution to obtain an oxyperfluoroolefin solution having a sulfonate group; (2) cleaning and drying the reaction kettle, passing ice water through the outer shell interlayer of the reaction kettle to control the temperature, and adding the perfluorodimethyldioxole monomer and the sulfonate-containing oxyperfluoroolefin solution into the reaction kettle; (3) adding the first initiator solution to the reaction kettle, stirring evenly and sealing the reaction kettle, evacuating and passing nitrogen gas 2-3 times, controlling the temperature of the reaction kettle to 40-50° C., reacting for 0.5-1 h, and then cooling to 0-5° C. to obtain an initial reaction emulsion; the first initiator solution is obtained by dissolving diisopropyl peroxydicarbonate in a composite solvent consisting of trifluorotrichloroethane and 2-chloro-1,1,2-trifluoroethyl methyl ether; (4) adding deionized water and an emulsifier to the initial reaction emulsion in the reactor, and adding 20 wt % sodium hydroxide solution to adjust the pH to 8-9; (5) Add the second initiator, purge the reactor with nitrogen and seal it, inject tetrafluoroethylene monomer into the initial reaction emulsion through the pipeline, close the pipeline and maintain the pressure at 1.5-1.8 MPa, raise the temperature to 80-90° C., and keep the reaction for 12-24 hours; continue to fill with nitrogen and maintain the pressure at 2-2.5 MPa, heat to 100-110° C. and keep it for 1-3 hours; (6) cooling to room temperature, releasing the pressure, precipitating, filtering out the solidified material in the reaction kettle, washing, devolatilizing, and drying; (7) hydrolyzing and hydrogenating the dried product of step (6) to obtain a terpolymer; The mass ratio of the tetrafluoroethylene monomer, the perfluorodimethyldioxole monomer, the oxoperfluoroolefin having a sulfonyl fluoride group, the first initiator and the second initiator is 5-10:10-20:30-50:0.5-1:1.5-2; The volume ratio of trifluorotrichloroethane and 2-chloro-1,1,2-trifluoroethyl methyl ether is 5:2-3; the ratio of the first initiator and the composite solvent is 0.5-1g:0.1mL; The second initiator is one or a combination of ammonium persulfate, sodium persulfate and potassium persulfate.

2. The method for preparing the emulsion polymerization terpolymer according to claim 1, characterized in that: The structural formula of the perfluorodimethyldioxole monomer is:

3. The method for preparing the emulsion polymerization terpolymer according to claim 1, characterized in that: The oxygen-perfluoroolefin having a sulfonyl fluoride group is perfluorosulfonyl ethoxypropyl vinyl ether, and its structural formula is CF2═CFOCF2CF(CF3)OCF2CF2SO2F; the structural formula of the oxygen-perfluoroolefin having a sulfonate group is CF2═CFOCF2CF(CF3)OCF2CF2SO2Na.

4. The method for preparing the emulsion polymerization terpolymer according to claim 1, characterized in that: The emulsifier is one or a combination of sodium dodecyl sulfate, sodium dodecyl sulfonate, ammonium perfluorooctanoate and sodium perfluorooctanoate.