A method for preparing a highly oxygen-permeable ionomer using diisopropyl peroxydicarbonate as an initiator, and the ionomer, film and application thereof
The low repetition and performance in the preparation of perfluoroinitiator were solved by using diisopropyl peroxide dicarbonate and trifluorotrichloroethane/2-chloro-1,1,2-trifluoroethylmethyl ether composite solvents. The problem of instability has achieved low cost and efficient preparation of highly oxygen-permeable ionomers, and improved the catalytic effect of hydrogen fuel cells.
Patent Information
- Application Number
- CN202411160803.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-22
AI Technical Summary
In the prior art, the preparation of highly oxygen permeable ionomers using perfluoroinitiators has problems such as low repeatability, unstable performance and high cost, and it has failed to effectively replace the high-cost perfluoroin structural initiator, affecting the hydrogen fuel cell. Catalytic effect.
Diisopropyl peroxide dicarbonate is used as the initiator, and poly(PDD-co- is enhanced by combining trifluorotrichloroethane and 2-chloro-1,1,2-trifluoroethylmethyl ether. PSVE) reaction yield and product quality improve its molecular weight, proton conductivity and oxygen permeability.
The low-cost and efficient preparation of high-oxygen permeability ionomers are achieved, with a yield of more than 95%, and the proton conductivity and oxygen permeability are significantly improved. The Pt/C catalyst layer suitable for hydrogen fuel cells is improved, which improves the catalytic effect.
Smart Images

Figure FDA0005068085930000011 
Figure VRWQBOBEYDSIUIDJGYSUZE0X2WDNYSRTO9J5OCFV
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hydrogen fuel cells, and in particular to a method for preparing a high oxygen permeability ionomer using diisopropyl peroxydicarbonate as an initiator, and the ionomer, film and application thereof. Background Art
[0002] The most important part of a hydrogen fuel cell is the catalyst. The catalytic efficiency of the catalyst directly determines the power of the entire fuel cell; at the same time, the amount of platinum (Pt) in the catalyst also plays an important role in the cost of the entire fuel cell. In fact, the distribution of Pt in the fuel cell is uneven (8 / 9 of the Pt / C catalyst is distributed in the positive electrode of the fuel cell). This is because in a hydrogen fuel cell, the HOR reaction occurs at the negative electrode. 2 →2e-+2H (two electron transfer, fast kinetics), ORR reaction occurs at the positive electrode O 2 +4e-+4H+→2H 2 O (four electron transfer, slow kinetics). According to theoretical calculations and comparison of the two reaction kinetics, the ORR reaction rate at the positive electrode is 6 orders of magnitude lower than the HOR reaction at the negative electrode, so the reaction rate of the overall reaction depends on the positive electrode. The chemical reaction rate is proportional to the amount of Pt catalyst used, so the amount of catalyst used at the positive electrode is about 8 times that of the negative electrode.
[0003] The catalyst Pt / C is adhered between the proton exchange membrane (PEM) and the gas diffusion layer (GDL) by a polymer binder. The polymer binder is called an ionomer. The surface of the catalyst Pt is wrapped by the ionomer, and oxygen must first permeate through the ionomer before it can contact the catalyst Pt, thereby initiating the ORR reaction. Therefore, the oxygen permeability of the ionomer has a significant effect on the catalytic effect of Pt. The higher the oxygen permeability of the ionomer, the better the catalytic effect of Pt. The currently commercially available ionomer is a Nafion-type perfluorosulfonic acid resin, and its oxygen permeability constant is 0.1-0.3cm 3 / m.24h.0.1MPa.
[0004] At present, perfluorosulfonic acid resin poly(PDD-co-PSVE) is a new type of ionomer used for the positive electrode of hydrogen fuel cells in recent years. It is a copolymer of perfluoro-2,2-dimethyl-1,3-dioxolane (PDD) and perfluorosulfonylethoxypropyl vinyl ether (PSVE). The synthesis process of poly(PDD-co-PSVE) reported publicly at home and abroad is a free radical polymerization reaction system. The initiator is a perfluoro organic peroxide, and the monomers PDD and PSVE are both perfluoro structures (also containing more F atoms). The initiator and the monomer have good compatibility, which is conducive to the polymerization reaction and the formation of poly(PDD-co-PSVE). However, there are no mature products of perfluoro initiators on the market. The perfluoro initiators prepared by the preparation methods disclosed by various companies have low repeatability and unstable performance. The yield of perfluoro initiators obtained in the product is low, and separation is difficult, which greatly affects the initiation effect. How to use existing non-fluorinated initiators to achieve low-cost, efficient and stable preparation of poly(PDD-co-PSVE) is an urgent problem to be solved. In addition, the preparation method of perfluorosulfonic acid resin disclosed in Patent 1 (CN116284538A) uses perfluoro-2,2-dimethyl-1,3-dioxolane and sulfonyl fluoride vinyl ether as monomers, fluorocarbon solvents such as perfluorocyclohexane and 1,2-trifluoro-1,2,2-trichloroethane and chlorofluoroalkanes as solvents, and peroxydicarbonates as initiators. However, Patent 1, which is the representative of the prior art, does not consider the influence of solvent characteristics on the ionomer polymerization system of a certain initiator, and how to achieve low-cost initiators to replace high-cost perfluoro structure initiators and obtain stable high oxygen permeability ionomers is the focus of research and development in this industry. Summary of the invention
[0005] In view of the problems existing in the background technology, the purpose of the present invention is to provide a method for preparing an ionomer using diisopropyl peroxydicarbonate as an initiator. The present invention adopts diisopropyl peroxydicarbonate, a common free radical initiator on the market, and unexpectedly finds that the combination of trifluorotrichloroethane and 2-chloro-1,1,2-trifluoroethyl methyl ether can improve the reaction yield and product quality of poly(PDD-co-PSVE); compared with other solvents, the comprehensive properties of poly(PDD-co-PSVE) such as molecular weight, proton conductivity and oxygen permeability are improved, and the intensity of use is also significantly improved.
[0006] In order to achieve the above object, the present invention provides a method for preparing an ionomer using diisopropyl peroxydicarbonate as an initiator, wherein the polymerization monomers of the ionomer include perfluorodimethyl dioxole monomer and perfluorosulfonyl ethoxypropyl vinyl ether; the perfluorodimethyl dioxole monomer and the perfluorosulfonyl ethoxypropyl vinyl ether are respectively dissolved in trifluorotrichloroethane; the initiator is diisopropyl peroxydicarbonate, and the diisopropyl peroxydicarbonate is dissolved in a composite solvent, and the composite solvent is composed of trifluorotrichloroethane and 2-chloro-1,1,2-trifluoroethyl methyl ether in a volume ratio of 10:1-2; wherein the perfluorodimethyl dioxole monomer has a structural formula of:
[0007] ;
[0008] The perfluorosulfonyl ethoxypropyl vinyl ether has the structural formula: CF 2 ═CFOCF 2 CF(CF 3 )OCF 2 CF 2 SO 2 F.
[0009] Optionally, the mass ratio of the perfluorodimethyldioxole monomer (PDD), perfluorosulfonylethoxypropyl vinyl ether (PSVE) and diisopropyl peroxydicarbonate (IPP) is 8-15:40-60:1.6-2.
[0010] Optionally, the ratio of perfluorodimethyldioxole monomer (PDD) to trifluorotrichloroethane (F113) is 100 g:1 mL; the ratio of perfluorosulfonylethoxypropyl vinyl ether (PSVE) to trifluorotrichloroethane (F113) is 100 g:1 mL; and the ratio of diisopropyl peroxydicarbonate (IPP) to the composite solvent is 60-80 g:1 mL.
[0011] Optionally, the method for preparing an ionomer using diisopropyl peroxydicarbonate as an initiator as described above comprises the following steps: (1) purging a reactor with nitrogen for 3-5 times, introducing liquid nitrogen into the shell interlayer of the reactor to cool the reactor, and maintaining the temperature of the reactor below -20°C; (2) dissolving PDD and PSVE in F113 respectively to obtain a PDD solution and a PSVE solution; dissolving IPP in a composite solvent to obtain an IPP solution; (3) sequentially adding the PDD solution and PSVE in the reactor; SVE solution, add IPP solution while the stirring paddle is stirring, stop stirring, evacuate and pass nitrogen, repeat the operation 2-3 times; (4) start stirring, seal the reactor, maintain pressure and gradually increase the temperature to 45-60°C, and maintain the reaction for 2-6 hours; continue to maintain pressure and heat to 90-100°C and maintain for 5-8 hours; (5) cool to room temperature, release pressure, filter out the solidified material in the reactor, devolatilize, wash and dry; (6) hydrolyze and hydrogenate to obtain a hydrogen-type high oxygen permeability ionomer.
[0012] The present invention also provides a high oxygen permeability ionomer prepared by the preparation method as described above, wherein the number average molecular weight Mn of the ionomer is greater than 190,000; and wherein the ionomer has a proton conductivity greater than 106 mS / cm at 80°C and 95% relative humidity, and has a proton conductivity greater than 51×10 -9 SCCcm / cm 2 Oxygen permeability in scmHg.
[0013] The present invention also provides a film made from the above-mentioned high oxygen permeability ionomer, wherein the tensile strength of the film is greater than 50 MPa.
[0014] The present invention also provides an application of the high oxygen permeability ionomer as described above, wherein the high oxygen permeability ionomer is applied to a Pt / C catalyst layer of a hydrogen fuel cell.
[0015] The beneficial effects of the present invention are as follows:
[0016] 1. The solvent or composite solvent selected in the present invention can significantly improve the initiation efficiency of diisopropyl peroxydicarbonate in the polymerization process of poly(PDD-co-PSVE), and the yield of poly(PDD-co-PSVE) reaches more than 95%, with stable productivity.
[0017] 2. The composite solvent obtained by using trichlorotrifluoroethane and 2-chloro-1,1,2-trifluoroethyl methyl ether in combination can significantly improve the initiation efficiency of diisopropyl peroxydicarbonate in the synthesis process, indicating that trichlorotrifluoroethane and 2-chloro-1,1,2-trifluoroethyl methyl ether are a more suitable composite solvent, which has a significant promoting effect on improving the initiation efficiency of diisopropyl peroxydicarbonate in the poly(PDD-co-PSVE) polymerization system; in the experiment, the use of other similar solvents could not achieve the expected reaction yield and product quality. DETAILED DESCRIPTION
[0018] In order to make the above-mentioned objects, features and advantages of the invention more obvious and easy to understand, the specific embodiments of the invention are described in detail below.
[0019] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0020] In the ionomer preparation method using diisopropyl peroxydicarbonate as an initiator according to the present invention, the polymerization monomers of the ionomer include perfluorodimethyl dioxole monomer and perfluorosulfonyl ethoxypropyl vinyl ether; the perfluorodimethyl dioxole monomer and the perfluorosulfonyl ethoxypropyl vinyl ether are dissolved in trifluorotrichloroethane respectively; the initiator is diisopropyl peroxydicarbonate, and the diisopropyl peroxydicarbonate is dissolved in a composite solvent, and the composite solvent is composed of trifluorotrichloroethane and 2-chloro-1,1,2-trifluoroethyl methyl ether in a volume ratio of 10:1-2; wherein the perfluorodimethyl dioxole monomer has a structural formula of:
[0021] ;
[0022] The perfluorosulfonyl ethoxypropyl vinyl ether has the structural formula: CF 2 ═CFOCF 2 CF(CF 3 )OCF 2 CF 2 SO 2 F.
[0023] In the method for preparing an ionomer using diisopropyl peroxydicarbonate as an initiator according to the present invention, the mass ratio of the perfluorodimethyldioxole monomer (PDD), perfluorosulfonylethoxypropyl vinyl ether (PSVE) and diisopropyl peroxydicarbonate (IPP) may be 8-15:40-60:1.6-2.
[0024] The method for preparing an ionomer using diisopropyl peroxydicarbonate as an initiator according to the present invention may include the following steps: (1) purging a reactor with nitrogen for 3-5 times, introducing liquid nitrogen into the shell interlayer of the reactor to cool the reactor, and maintaining the temperature of the reactor below -20°C; (2) dissolving PDD and PSVE in F113 to obtain a PDD solution and a PSVE solution; dissolving IPP in a composite solvent to obtain an IPP solution; (3) sequentially adding the PDD solution and PSVE solution into the reactor. SVE solution, add IPP solution while the stirring paddle is stirring, stop stirring, evacuate and pass nitrogen, repeat the operation 2-3 times; (4) start stirring, seal the reactor, maintain pressure and gradually increase the temperature to 45-60°C, and maintain the reaction for 2-6 hours; continue to maintain pressure and heat to 90-100°C and maintain for 5-8 hours; (5) cool to room temperature, release pressure, filter out the solidified material in the reactor, devolatilize, wash and dry; (6) hydrolyze and hydrogenate to obtain a hydrogen-type high oxygen permeability ionomer.
[0025] In the method for preparing an ionomer using diisopropyl peroxydicarbonate as an initiator according to the present invention, the ratio of perfluorodimethyldioxole monomer (PDD) to trifluorotrichloroethane (F113) can be 100 g:1 mL; the ratio of perfluorosulfonylethoxypropyl vinyl ether (PSVE) to trifluorotrichloroethane (F113) can be 100 g:1 mL; and the ratio of diisopropyl peroxydicarbonate (IPP) to the composite solvent can be 60-80 g:1 mL.
[0026] In the high oxygen permeability ionomer prepared according to the preparation method of the present invention, the number average molecular weight Mn of the ionomer is greater than 190,000; and wherein the ionomer has a proton conductivity greater than 106 mS / cm at 80°C and 95% relative humidity, and has a proton conductivity greater than 51×10 -9 SCCcm / cm 2 Oxygen permeability in scmHg.
[0027] The tensile strength of the film prepared from the high oxygen permeability ionomer according to the present invention is greater than 50 MPa.
[0028] The high oxygen permeability ionomer according to the present invention can be applied to the Pt / C catalyst layer of a hydrogen fuel cell.
[0029] The following examples specifically illustrate the method for preparing a highly oxygen permeable ionomer using diisopropyl peroxydicarbonate as an initiator, the ionomer, the film and the application of the present invention. Main raw materials and equipment used: Unless otherwise specified, the raw materials and equipment of each embodiment and comparative example are the same; materials without specifying specific models or types are from the same common models purchased on the market, and no specific restrictions are made.
[0030] Example 1
[0031] (1) The reactor was purged with nitrogen for 5 times, and liquid nitrogen was introduced into the outer shell interlayer of the reactor to cool down and keep the temperature of the reactor below -20°C; (2) PDD and PSVE were dissolved in F113 respectively to obtain PDD solution and PSVE solution; the ratio of PDD to F113 in the PDD solution was 100 g:1 mL, and the ratio of PSVE to F113 in the PSVE solution was 100 g:1 mL; IPP was dissolved in a composite solvent of F113 and 2-chloro-1,1,2-trifluoroethyl methyl ether with a volume ratio of 5:1 to obtain an IPP solution, and the ratio of diisopropyl peroxydicarbonate (IPP) to the composite solvent in the IPP solution was 80 g:1 mL. 1mL; (3) Add PDD solution and PSVE solution to the reactor in sequence, add IPP solution while the stirring paddle is kept stirring, stop stirring, evacuate and pass nitrogen, and repeat the operation for 3 times; the mass ratio of PDD, PSVE and IPP is 8:40:1.6; (4) Start stirring, close the reactor, maintain pressure and gradually increase the temperature to 60°C, and maintain the reaction for 6h; continue to maintain pressure and heat to 100°C for 8h; (5) Cool to room temperature, release pressure, filter out the solidified material in the reactor, devolatilize, wash and dry; (6) Hydrolyze with 20wt% KOH aqueous solution and hydrogenate with 20wt% hydrochloric acid solution to obtain a hydrogen-type high oxygen permeability ionomer.
[0032] Example 2
[0033] (1) nitrogen was purged into the reactor for 3 times, and liquid nitrogen was introduced into the outer shell interlayer of the reactor to cool down and keep the temperature of the reactor below -20°C; (2) PDD and PSVE were dissolved in F113 respectively to obtain PDD solution and PSVE solution; the ratio of PDD to F113 in the PDD solution was 100 g:1 mL, and the ratio of PSVE to F113 in the PSVE solution was 100 g:1 mL; IPP was dissolved in a composite solvent of F113 and 2-chloro-1,1,2-trifluoroethyl methyl ether with a volume ratio of 10:1 to obtain an IPP solution, and the ratio of IPP to the composite solvent in the IPP solution was 60 g:1 mL; (3) Add PDD solution and PSVE solution to the reactor in sequence, add IPP solution while the stirring paddle is stirring, stop stirring, evacuate and pass nitrogen, and repeat the operation twice; the mass ratio of PDD, PSVE and IPP is 15:60:2; (4) Start stirring, close the reactor, maintain pressure and gradually increase the temperature to 45°C, and maintain the reaction for 2h; continue to maintain pressure and heat to 90°C for 5h; (5) Cool to room temperature, release pressure, filter out the solidified material in the reactor, devolatilize, wash and dry; (6) Hydrolyze with 20wt% KOH aqueous solution and hydrogenate with 20wt% hydrochloric acid solution to obtain a hydrogen-type high oxygen permeability ionomer.
[0034] Example 3
[0035] (1) nitrogen purged the reactor 4 times, and liquid nitrogen was introduced into the outer shell interlayer of the reactor to cool down, and the temperature of the reactor was maintained below -20°C; (2) PDD and PSVE were dissolved in F113 respectively to obtain PDD solution and PSVE solution; the ratio of PDD to F113 in the PDD solution was 100 g:1 mL, and the ratio of PSVE to F113 in the PSVE solution was 100 g:1 mL; IPP was dissolved in a composite solvent of F113 and 2-chloro-1,1,2-trifluoroethyl methyl ether with a volume ratio of 10:1.5 to obtain an IPP solution, and the ratio of diisopropyl peroxydicarbonate (IPP) to the composite solvent in the IPP solution was 70 g :1mL; (3) Add PDD solution and PSVE solution to the reactor in sequence, add IPP solution while the stirring paddle is stirring, stop stirring, evacuate and pass nitrogen, and repeat the operation for 3 times; the mass ratio of PDD, PSVE and IPP is 12:50:1.8; (4) Start stirring, close the reactor, maintain pressure and gradually increase the temperature to 52°C, and maintain the reaction for 4h; continue to maintain pressure and heat to 95°C for 6.5h; (5) Cool to room temperature, release pressure, filter out the solidified material in the reactor, devolatilize, wash and dry; (6) Hydrolyze with 20wt% KOH aqueous solution and hydrogenate with 20wt% hydrochloric acid solution to obtain a hydrogen-type high oxygen permeability ionomer.
[0036] Comparative Example 1
[0037] Except that F113 replaced the composite solvent, the other steps were the same as those in Example 3.
[0038] Comparative Example 2
[0039] Except that the solvent FC-72 (perfluorohexane) was used instead of the composite solvent, the other steps were the same as those in Example 3.
[0040] Comparative Example 3
[0041] Vertrel TM XF(CF 3 CFHCFHCF 2 CF 3 ) instead of the composite solvent, the rest is the same as in Example 3.
[0042] Performance Testing
[0043] 1. The yield (ratio of product to raw material), exchange equivalent EW value (GB / T20042.3-2022) and number average molecular weight of the hydrogen-type ionomers of the examples and comparative examples were tested respectively.
[0044] 2. At 23°C and 0% relative humidity, the oxygen permeability of the catalyst layer after peeling off from the surface of the base membrane PET was tested using an instrument (MoconOX-Tran®, Minneapolis, MN, USA); at 80°C and 95% relative humidity, the catalyst layer was loaded into the electrolyte membrane of the electrochemical cell, the test electrodes were connected to both sides of the electrolyte membrane, an external voltage was applied, and the proton conductivity was calculated.
[0045] 3. After the hydrogen-type ionomer is dissolved in a solvent, it is cast into a film with a thickness of 0.5 mm; the mechanical strength of the hydrogen-type ionomer film is tested using a universal material testing machine (GB / T20042.3-2022). Specific data are shown in Table 1.
[0046] Table 1
[0047]
[0048] It can be seen from the data of the embodiments and comparative examples that the composite solvent composed of 2-chloro-1,1,2-trifluoroethyl methyl ether and F113 of the present invention can promote the polymerization of poly(PDD-co-PSVE) with IPP as the initiator, with high yield, and the obtained hydrogen-type ionomer film has good performance.
[0049] The above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the present invention.
Claims
1. A method for preparing a high oxygen permeability ionomer using diisopropyl peroxydicarbonate as an initiator, characterized in that: The polymerization monomers of the ionomer include perfluorodimethyl dioxole monomer and perfluorosulfonyl ethoxypropyl vinyl ether; the perfluorodimethyl dioxole monomer and perfluorosulfonyl ethoxypropyl vinyl ether are dissolved in trifluorotrichloroethane respectively; the initiator is diisopropyl peroxydicarbonate, and diisopropyl peroxydicarbonate is dissolved in a composite solvent, and the composite solvent is composed of trifluorotrichloroethane and 2-chloro-1,1,2-trifluoroethyl methyl ether in a volume ratio of 10:1-2; wherein the perfluorodimethyl dioxole monomer has a structural formula of: The perfluorosulfonyl ethoxypropyl vinyl ether has the structural formula: CF2═CFOCF2CF(CF3)OCF2CF2SO2F.
2. The method for preparing a high oxygen permeability ionomer using diisopropyl peroxydicarbonate as an initiator according to claim 1, characterized in that: The mass ratio of the perfluorodimethyldioxole monomer, perfluorosulfonylethoxypropyl vinyl ether and diisopropyl peroxydicarbonate is 8-15:40-60:1.6-2.
3. The method for preparing a high oxygen permeability ionomer using diisopropyl peroxydicarbonate as an initiator according to claim 1 or 2, characterized in that: The method comprises the following steps: (1) purging a reactor with nitrogen for 3-5 times, introducing liquid nitrogen into the outer shell interlayer of the reactor to cool down, and maintaining the temperature of the reactor below -20°C; (2) dissolving perfluorodimethyl dioxole monomer and perfluorosulfonyl ethoxypropyl vinyl ether in trifluorotrichloroethane respectively to obtain a perfluorodimethyl dioxole monomer solution and a perfluorosulfonyl ethoxypropyl vinyl ether solution; dissolving diisopropyl peroxydicarbonate in a composite solvent to obtain a diisopropyl peroxydicarbonate solution; (3) sequentially adding perfluorodimethyl dioxole, diisopropyl peroxydicarbonate and diisopropyl peroxydicarbonate into the reactor; and (4) adding diisopropyl peroxydicarbonate and diisopropyl peroxydicarbonate into the reactor. Add diisopropyl peroxydicarbonate solution to heterocyclopentene monomer solution and perfluorosulfonyl ethoxypropyl vinyl ether solution while stirring with a stirring paddle, stop stirring, evacuate and pass nitrogen, and repeat the operation 2-3 times; (4) start stirring, seal the reaction kettle, maintain pressure and gradually increase the temperature to 45-60°C, and maintain the reaction for 2-6 hours; continue to maintain pressure and heat to 90-100°C and maintain for 5-8 hours; (5) cool to room temperature, release pressure, filter out the solidified material in the reaction kettle, devolatilize, wash and dry; (6) hydrolyze and hydrogenate to obtain a hydrogen-type high oxygen permeability ionomer.
4. The method for preparing a high oxygen permeability ionomer using diisopropyl peroxydicarbonate as an initiator as claimed in claim 3, characterized in that: The ratio of perfluorodimethyldioxole monomer to trifluorotrichloroethane is 100 g:1 mL; the ratio of perfluorosulfonylethoxypropyl vinyl ether to trifluorotrichloroethane is 100 g:1 mL; and the ratio of diisopropyl peroxydicarbonate to the composite solvent is 60-80 g:1 mL.