A wind turbine blade recycled composite material and its preparation method and application

The preparation of wind power blade recycled composite materials through the radiation method has solved the problems of environmental pollution and resource waste in the treatment of wind power blade waste, achieved efficient recycling and improved mechanical performance, and has the advantages of green environmental protection and economic benefits.

CN118684836BActive Publication Date: 2024-11-15ORANGE (SHANGHAI) ENVIRONMENTAL TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411194482.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-15
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

The waste of wind power blades is difficult to degrade naturally, and conventional treatment methods lead to environmental pollution and resource waste. The existing recycling technology has problems such as reduced mechanical properties, large environmental impact and high resource consumption.

Method used

The regeneration composite material of wind power blades is prepared by irradiation method. The first irradiation of the wind power blade pellets is used to generate active fillers, mix unsaturated polyester resin and crosslinking enhancer, and perform the second irradiation and pressure crosslinking. Curing, forming a three-dimensional network structure, retaining glass fiber components, and improving mechanical properties.

Benefits of technology

It has achieved efficient recycling of wind power blade materials, achieved excellent mechanical properties, was green and environmentally friendly, resource conservation, and had economic benefits and application value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention belongs to the technical field of wind turbine blade materials, and specifically relates to a wind turbine blade recycled composite material and a preparation method and application thereof. The present invention subjects wind turbine blade granules to a first irradiation to obtain an active filler; the active filler, an unsaturated polyester resin and a cross-linking enhancer are mixed to obtain a mixture; the mixture is pressed in a mold to obtain a preformed body; under the conditions of a second irradiation and pressure, the preformed body is cross-linked and cured to obtain the wind turbine blade recycled composite material. The present invention realizes the recycling of wind turbine blade materials and the preparation of recycled composite materials. The obtained wind turbine blade recycled composite material has excellent mechanical properties. At the same time, the recycling and reuse of wind turbine blade waste has the advantages of being green, efficient, environmentally friendly and resource-saving, and has certain economic benefits and application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of wind turbine blade materials, and in particular relates to a wind turbine blade recycled composite material and a preparation method and application thereof. Background Art

[0002] Although wind power generation is a clean and renewable energy source, the entire unit equipment will generate a large amount of wind turbine blade waste that needs to be processed during the production process and after retirement. Among them, the combination of reinforcing fiber (currently mainly glass fiber) and polymer matrix (currently mainly epoxy resin, etc.) occupies the vast majority of the mass of wind turbine blade material components. The content of reinforcing fiber in wind turbine blade materials is about 60~70wt%, and the content of polymer matrix is ​​about 30~40wt%. This makes wind turbine blade waste difficult to degrade naturally and is extremely polluting. Conventional methods such as random stacking, direct landfill, and simple incineration are not effective solutions. They will occupy a large amount of land resources, cause secondary pollution, and cause serious harm to the environment. Therefore, from the perspective of environmental protection and resource utilization, the best way to deal with wind turbine blade materials is recycling.

[0003] At present, the relevant processing technologies for wind turbine blade recycling include thermal recovery, chemical recovery, and physical recovery. These three methods have their own advantages and disadvantages. Among them, the thermal recovery method involves high-temperature treatment, which can be mainly divided into combustion or incineration (only for energy recovery) and fluidized bed combustion (mainly for recycling reinforcing fibers) and anaerobic combustion (i.e. pyrolysis). The thermal recovery method can recover energy, oil and filler without using solvents and catalysts, but the size and performance of the recycled materials will be reduced accordingly. The fiber products may contain oxidized residues or carbon, which cannot be completely harmless, and there are emissions and carbon dioxide, which have a negative impact on the environment. The most studied chemical recovery method is the solvent recovery method. This method uses solvents to destroy the resin macromolecular bonds at a certain temperature and pressure, so as to achieve the purpose of separating and recovering resin and glass fiber. Thus, the recovery of single oligomers and fillers is achieved, and the shape, size, composition and mechanical properties of the recovered fillers remain unchanged. However, a large amount of organic solvents and catalysts are used in the recycling process. The large amount of volatilization of organic solvents will directly have an adverse impact on the environment, and the residual organic solvents will form new hazardous wastes. Therefore, the chemical recycling method is difficult to recycle on a large scale, and the treatment of hazardous wastes will consume a lot of resources and manpower, material and financial resources. Therefore, the chemical method often does not make up for the loss. The physical recycling method mainly includes disassembly and reuse, mechanical crushing and comprehensive utilization. The recycled wind turbine blade materials can be used as fillers or matrices for the production of secondary materials. The recycling process of this method is simple and reliable, and the adverse effects on energy consumption and the environment are relatively small. Therefore, it is a relatively economical and reasonable recycling method with certain development prospects. However, the current physical recycling method usually only crushes the wind turbine blades and directly adds them to other substrates as inert fillers for molding. There is no force between the inert filler and the substrate, so the mechanical strength of the substrate is not significantly improved, and even the mechanical properties of the substrate are greatly reduced, which greatly limits the application of wind turbine blade recycling materials. Summary of the invention

[0004] The purpose of the present invention is to provide a wind turbine blade recycled composite material and its preparation method and application. The wind turbine blade recycled composite material provided by the present invention has excellent mechanical properties and can realize green, efficient, value-added recovery and regeneration of wind turbine blade waste, which is environmentally friendly, saves resources, and has certain economic benefits and application value.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing a wind turbine blade regeneration composite material, comprising the following steps:

[0007] The wind turbine blade granules are subjected to a first irradiation to obtain an active filler;

[0008] The active filler, unsaturated polyester resin and cross-linking enhancer are mixed to obtain a mixture; the unsaturated polyester resin includes one or more of a para-terephthalate unsaturated polyester resin, a bisphenol A unsaturated polyester resin and an isophthalate unsaturated polyester resin; the mass ratio of the wind turbine blade granules to the polyester resin is (1:1) to (7:3); the mass of the cross-linking enhancer accounts for 2 to 3% of the total mass of the wind turbine blade granules and the polyester resin;

[0009] Pressing the mixture in a mold to obtain a preformed body;

[0010] Under the conditions of second irradiation and pressure application, the preformed body is cross-linked and cured to obtain the wind turbine blade recycled composite material.

[0011] Preferably, the wind turbine blade granules are obtained by crushing wind turbine blade materials, and the particle size of the wind turbine blade granules is 0.2-2 mm.

[0012] Preferably, the first irradiation is performed using Co-60 gamma rays, the dose of the first irradiation is 10-300 kGray, and the irradiation time is 3-10 min.

[0013] Preferably, the crosslinking enhancer includes one or more of methyl methacrylate, diallyl phthalate and propane trimethanol triacrylate.

[0014] Preferably, the mixing is carried out in a mixer at a temperature of 60-100° C. and a time of 5-10 min.

[0015] Preferably, the mixing is carried out under stirring, and the stirring speed is 20-30 rad / min.

[0016] Preferably, the pressing temperature is 60-100° C., the pressure is 5-10 MPa, and the heat and pressure holding time is 3-8 min.

[0017] Preferably, the second irradiation is performed using Co-60 gamma rays, the dose of the second irradiation is 10-300 kGy, and the irradiation time is 10-25 min; the pressure during the cross-linking and curing is 8-10 MPa.

[0018] The present invention provides a wind turbine blade recycled composite material prepared by the preparation method described in the above technical solution.

[0019] The present invention provides the use of the wind turbine blade recycled composite material described in the above technical solution as an artificial board.

[0020] The invention provides a preparation method of a wind turbine blade recycled composite material, comprising the following steps: subjecting wind turbine blade granules to a first irradiation to obtain an active filler; mixing the active filler, an unsaturated polyester resin and a cross-linking enhancer to obtain a mixture; the unsaturated polyester resin comprises one or more of a terephthalate unsaturated polyester resin, a bisphenol A unsaturated polyester resin and an isophthalate unsaturated polyester resin; the mass ratio of the wind turbine blade granules to the polyester resin is (1:1) to (7:3); the mass of the cross-linking enhancer accounts for 2 to 3% of the total mass of the wind turbine blade granules and the polyester resin; pressing the mixture in a mold to obtain a preformed body; and cross-linking and curing the preformed body under the conditions of a second irradiation and pressure to obtain the wind turbine blade recycled composite material. The present invention adopts an irradiation method to prepare a high-performance wind turbine blade regeneration composite material. First, the wind turbine blade granules are irradiated for the first time, and active free radicals can be generated on the molecular chains of the polymer matrix (epoxy resin) in the wind turbine blade granules, thereby converting them into active fillers that can undergo chemical crosslinking reactions. Then, the present invention mixes the obtained active fillers, unsaturated polyester resins and crosslinking enhancers to obtain a preformed body, and then crosslinks and cures the preformed body under the conditions of a second irradiation and pressure. Under the conditions of the second irradiation, the present invention optimizes the dosage ratio of the active fillers, the unsaturated polyester resins and the crosslinking enhancers. The crosslinking enhancers absorb high-energy radiation and decompose to generate free radicals. At this time, the active free radicals carried on the epoxy resin molecular chains in the active fillers can work together with the crosslinking enhancers to initiate free radical polymerization of the unsaturated polyester resin. Therefore, in the crosslinking system of the unsaturated polyester of the present invention, the epoxy molecular chains with active free radicals will also participate in the crosslinking reaction. Both the active fillers and the crosslinking enhancers participate in the crosslinking system. The present invention finally forms a wind turbine blade regeneration composite material with a three-dimensional network structure, which can significantly enhance the mechanical properties of the composite material. On the other hand, the method provided by the present invention avoids the process of separating the epoxy resin and the reinforcing fiber (glass fiber) in the wind turbine blade granules, retains the glass fiber component in the composite material, and further improves the mechanical strength of the composite material. In summary, the present invention realizes the recycling of wind turbine blade materials and the preparation of recycled composite materials. The obtained wind turbine blade recycled composite material has excellent mechanical properties. At the same time, the recycling and reuse of wind turbine blade waste has the advantages of being green, efficient, environmentally friendly and resource-saving, and has certain economic benefits and application value. DETAILED DESCRIPTION

[0021] The present invention provides a method for preparing a wind turbine blade regeneration composite material, comprising the following steps:

[0022] The wind turbine blade granules are subjected to a first irradiation to obtain an active filler;

[0023] The active filler, unsaturated polyester resin and cross-linking enhancer are mixed to obtain a mixture; the unsaturated polyester resin includes one or more of a para-terephthalate unsaturated polyester resin, a bisphenol A unsaturated polyester resin and an isophthalate unsaturated polyester resin; the mass ratio of the wind turbine blade granules to the polyester resin is (1:1) to (7:3); the mass of the cross-linking enhancer accounts for 2 to 3% of the total mass of the wind turbine blade granules and the polyester resin;

[0024] Pressing the mixture in a mold to obtain a preformed body;

[0025] Under the conditions of second irradiation and pressure application, the preformed body is cross-linked and cured to obtain the wind turbine blade recycled composite material.

[0026] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.

[0027] The present invention subjects the wind turbine blade granules to a first irradiation to obtain an active filler. In the present invention, the wind turbine blade granules are obtained by crushing the wind turbine blade material. In a specific embodiment of the present invention, the wind turbine blade material is the wind turbine blade waste that needs to be processed during the production process and after retirement of the wind turbine generator set equipment. In the present invention, the crushing is preferably carried out in a crusher, and the operating conditions of the crushing preferably include: a spindle speed of 4500r / min, a feed particle size of 6mm, a crushing fineness of 60~150 mesh, and a motor power of 4kW. In a specific embodiment of the present invention, the crusher used for the crushing is a universal crusher provided by Jiangsu Chitong Machinery Manufacturing Co., Ltd., model 20B.

[0028] In the present invention, the pulverization obtains a pulverized product. In the present invention, the pulverized product obtained after the pulverization is screened to obtain the wind turbine blade granules. In the present invention, the screening is preferably performed using an SDB-200 top-impact vibrating screen. The operating conditions of the screening preferably include: the maximum diameter of the screen is 200 mm, the screen layer stacking height is 400 mm, the turning radius is 12.5 mm, the screen shaking times is 221 r / min, the shock times is 147 r / min, the upper and lower amplitudes are formed to be 5 mm, the timing range is 0~60 min, the motor power is 0.37 kW, the voltage is 380 V, the speed is 2800 kg, and the weight is 130 kg.

[0029] In the present invention, the particle size of the wind turbine blade granules is preferably 0.2-2 mm.

[0030] In the present invention, the first irradiation is preferably carried out using Co-60 gamma rays, and the dose of the first irradiation is preferably 10-300 kGray, more preferably 10-200 kGray, further preferably 10-100 kGray, most preferably 10-20 kGray, specifically preferably 10 kGray, 12 kGray, 14 kGray or 16 kGray; the irradiation time is preferably 3-10 min, more preferably 5-8 min, specifically preferably 5 min, 6 min, 7 min, 8 min. In the present invention, during the first irradiation process: active free radicals are generated on the molecular chains of the epoxy resin in the wind turbine blade granules, and the obtained active filler can participate in the cross-linking reaction of the unsaturated matrix material, thereby forming a three-dimensional network cross-linked structure composed of three systems (unsaturated polyester resin, epoxy resin molecular chains with active free radicals, and cross-linking enhancers) in the subsequent cross-linking curing reaction.

[0031] After obtaining the active filler, the present invention mixes the active filler, unsaturated polyester resin and crosslinking enhancer to obtain a mixture. In the present invention, the unsaturated polyester resin preferably includes one or more of terephthalic unsaturated polyester resin, bisphenol A unsaturated polyester resin and isophthalic unsaturated polyester resin. The crosslinking enhancer preferably includes one or more of methyl methacrylate, diallyl phthalate and propane trimethylol triacrylate, and more preferably propane trimethylol triacrylate. The mass ratio of the wind turbine blade granules and the polyester resin is preferably (1:1) to (7:3), and more preferably 1:1, 1.5:1 or 7:3. The mass of the crosslinking enhancer accounts for 1.5 to 3% of the total mass of the wind turbine blade granules and the polyester resin, and is preferably 3%, 2.5% or 2%. The mixing is preferably carried out in a mixer, the mixing temperature is preferably 60 to 100°C, more preferably 60 to 85°C, and the time is preferably 5 to 10 min. The mixing is carried out under stirring conditions, and the stirring speed is preferably 20 to 30 rad / min.

[0032] After obtaining the mixture, the present invention presses the mixture in a mold to obtain a preformed body. In the present invention, the mold is preferably an aluminum mold. In the subsequent second irradiation process, the irradiated rays can penetrate the aluminum mold and then irradiate the preformed body in the mold. In the present invention, the pressing temperature is preferably 60~100℃, and the pressing temperature is preferably consistent with the temperature of the mixing process; the pressure is preferably 5~10MPa, and specifically preferably 8MPa; the heat preservation and pressure holding time is preferably 3~8min, and specifically preferably 5min.

[0033] The present invention can make the mixed material fully flow and fill the entire mold through pressing.

[0034] After obtaining the preformed body, the present invention cross-links and cures the preformed body under the conditions of second irradiation and pressure to obtain the wind turbine blade regeneration composite material. In the present invention, the cross-linking and curing process is preferably carried out under room temperature. In the present invention, the second irradiation is preferably carried out using Co-60γ rays, and the dose of the second irradiation is preferably 10~300kGy, more preferably 10~150kGy, further preferably 10~100kGy, most preferably 10~50kGy, specifically preferably 25kGy, 20kGy, 15kGy or 10kGy; the irradiation time is preferably 10~25min, more preferably 10~20min, specifically preferably 16min, 14min, 12min or 10min. The pressure of the cross-linking and curing is preferably 8~10MPa, specifically preferably 8MPa.

[0035] In the present invention, during the second irradiation process, the monomer in the cross-linking enhancer absorbs radiation energy and decomposes to generate free radicals, thereby initiating a curing cross-linking reaction of the unsaturated polyester resin. During the cross-linking reaction, the epoxy resin molecular chain (active filler) carrying active free radicals will also join the cross-linking reaction of the unsaturated polyester resin, and finally form a three-dimensional network cross-linking structure composed of three systems (unsaturated polyester resin, epoxy resin molecular chain with active free radicals and cross-linking enhancer).

[0036] In the present invention, after the cross-linking and curing reaction is completed, the mold is opened to take out the target wind turbine blade recycled composite material product.

[0037] The present invention provides a wind turbine blade recycled composite material prepared by the preparation method described in the above technical solution.

[0038] The wind turbine blade regeneration composite material provided by the present invention has a three-dimensional network cross-linked structure, contains reinforcing fibers, and has excellent mechanical properties.

[0039] The present invention provides the application of the wind turbine blade recycled composite material as a man-made board. The present invention has no special requirements on the specific application method of the wind turbine blade recycled composite material.

[0040] Compared with the prior art, the present invention has the following significant beneficial effects:

[0041] The present invention adopts the method of preparing high-performance wind turbine blade recycled composite material by irradiation, avoids the process and operation of separating glass fiber from resin, realizes 100% recycling, reduces resource waste and environmental pollution, and greatly saves production costs.

[0042] The preparation of the regenerated composite material in the present invention is to form a new three-dimensional network cross-linked structure by cross-linking reaction between active fillers and unsaturated polyester resin matrix, and epoxy resin and unsaturated polyester resin are used for cross-linking reaction under Co-60 gamma ray irradiation, while glass fiber will not be damaged and the mechanical properties of glass fiber are retained. The cross-linking reaction between the two resins greatly improves the compatibility of the system, and its mechanical properties, thermal stability, wear resistance, solvent resistance and creep resistance are all improved to varying degrees. In addition, all materials of the present invention are easy to obtain, the cost is relatively low, and the preparation method is simple and clear.

[0043] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0044] In the following embodiments and comparative examples: the recycled wind turbine blades are sourced from Jerry Environmental Technology Co., Ltd., the mass percentage of glass fiber in the recycled wind turbine blades is 60-70%, the mass percentage of epoxy resin is 30-40%, and the performance parameters of the recycled wind turbine blades include: tensile strength of 70-75 MPa, bending strength of 115-120 MPa, and impact strength of 35-40 J / cm 2 The test method of the mechanical properties of the recovered wind turbine blades is the same as the test method of the data in Table 1. The unsaturated polyester resin is a terephthalate unsaturated polyester resin, and the manufacturer is Tianhe Resin Co., Ltd. The cross-linking enhancer is propane trimethylol triacrylate, and the manufacturer of propane trimethylol triacrylate is Nantong Runfeng Petrochemical Co., Ltd., with a CAS number of 15625-89-5, and the appearance is a yellow transparent liquid.

[0045] In the following examples and comparative examples: the pulverization of the recycled wind turbine blades was carried out using a universal pulverizer provided by Jiangsu Chitong Machinery Manufacturing Co., Ltd., model 20B; the pulverization operating conditions included: a spindle speed of 4500r / min, a feed particle size of 6mm, a pulverization fineness of 60-150 meshes, and a motor power of 4kW. The particle size of the pulverized wind turbine blade particles was ≤5mm.

[0046] The SDB-200 top-impact vibrating screen is used for screening the recycled wind turbine blades after crushing. The operating conditions of the screening include: the maximum diameter of the screen is 200mm, the screen layer stacking height is 400mm, the turning radius is 12.5mm, the screen shaking frequency is 221r / min, the shock frequency is 147r / min, the upper and lower amplitude is 5mm, the timing range is 0~60min, the motor power is 0.37kW, the voltage is 380V, the speed is 2800kg, and the weight is 130kg. The particle size of the wind turbine blade pellets obtained after screening is 1~2mm.

[0047] Example 1

[0048] In this embodiment, after the recycled wind turbine blade material is crushed and sieved, 500g of pellets are weighed and first irradiated for 5min by releasing Co-60γ rays through an irradiation device, with an irradiation dose of 10KGray, and the pellets are converted into active fillers. Then, 500g of unsaturated polyester resin and 30g of cross-linking enhancer are placed in a mixer to mix them evenly (mixing temperature is 60°C, time is 10min, and speed is 30rad / min). After sufficient mixing, the mixture is injected into the target mold, heated and pressurized to 60°C, 8MPa, and kept warm and pressurized for 5min to fill the mold with the mixture. After the irradiation device releases Co-60γ rays with an irradiation dose of 25kGy, the cross-linking enhancer absorbs radiation energy and decomposes to produce free radicals, which triggers the cross-linking reaction between the epoxy resin molecular chain with active free radicals and the unsaturated polyester resin. During the curing cross-linking reaction, the pressure is increased to 8MPa to make the product dense and reduce product defects. After the reaction is completed, the mold is opened to take out the recycled composite material sheet.

[0049] Example 2

[0050] In this embodiment, after the recycled wind turbine blade material is crushed and sieved, 600g of pellets are weighed and first released by the irradiation device Co-60γ rays for 6min irradiation, the irradiation dose is 12KGray, and the pellets are converted into active fillers. Then, 400g of unsaturated polyester resin and 25g of cross-linking enhancer are placed in a mixer to mix them evenly (mixing temperature is 60℃, time is 10min, speed is 30rad / min), and after sufficient mixing, the mixture is injected into the target mold, heated and pressurized to 60℃, 8MPa, and kept warm and pressurized for 5min to fill the mold with the mixture. After the irradiation device releases Co-60γ rays, the irradiation dose is 20kGy, and the pellets are irradiated through the mold for 14min, the cross-linking enhancer absorbs radiation energy and decomposes to produce free radicals, which triggers the cross-linking reaction between the epoxy resin molecular chain with active free radicals and the unsaturated polyester resin. During the curing cross-linking reaction, the pressure is increased to 8MPa to make the product dense and reduce product defects. After the reaction is completed, the mold is opened to take out the recycled composite material sheet.

[0051] Example 3

[0052] In this embodiment, after the recycled wind turbine blade material is crushed and sieved, 700g of pellets are weighed and first irradiated by the irradiation device to release Co-60γ rays for 7min, with an irradiation dose of 14KGray, and converted into active fillers. The pellets are then placed in a mixer with 300g of unsaturated polyester resin and 20g of cross-linking enhancer to mix them evenly (mixing temperature is 60℃, time is 10min, speed is 30rad / min), and after sufficient mixing, the mixture is injected into the target mold, heated and pressurized to 60℃, 8MPa, and kept warm and pressurized for 5min to fill the mold with the mixture. After the irradiation device releases Co-60γ rays with an irradiation dose of 15kGy, the pellets are irradiated through the mold for 12min, and the cross-linking enhancer absorbs radiation energy to decompose and generate free radicals, which triggers the cross-linking reaction between the epoxy resin molecular chain with active free radicals and the unsaturated polyester resin. During the curing cross-linking reaction, the pressure is increased to 8MPa to make the product dense and reduce product defects. After the reaction is completed, the mold is opened to take out the recycled composite material sheet.

[0053] Example 4

[0054] In this embodiment, after the recycled wind turbine blade material is crushed and sieved, 600g of pellets are weighed and first irradiated for 5min by releasing Co-60γ rays through an irradiation device, with an irradiation dose of 10KGray, and the pellets are converted into active fillers. Then, 400g of unsaturated polyester resin and 25g of cross-linking enhancer are placed in a mixer to mix them evenly (mixing temperature is 60℃, time is 10min, and speed is 30rad / min). After sufficient mixing, the mixture is injected into the target mold, heated and pressurized to 60℃, 8MPa, and kept warm and pressurized for 5min to fill the mold with the mixture. After the irradiation device releases Co-60γ rays with an irradiation dose of 25kGy, the cross-linking enhancer absorbs radiation energy and decomposes to produce free radicals, which triggers the cross-linking reaction between the epoxy resin molecular chain with active free radicals and the unsaturated polyester resin. During the curing cross-linking reaction, the pressure is increased to 8MPa to make the product dense and reduce product defects. After the reaction is completed, the mold is opened to take out the recycled composite material sheet.

[0055] Example 5

[0056] In this embodiment, after the recycled wind turbine blade material is crushed and sieved, 700g of pellets are weighed and first released by the irradiation device Co-60γ rays for 5min irradiation, the irradiation dose is 10KGray, and the pellets are converted into active fillers. Then, 300g of unsaturated polyester resin and 20g of cross-linking enhancer are placed in a mixer to mix them evenly (mixing temperature is 60℃, time is 10min, speed is 30rad / min), and after sufficient mixing, the mixture is injected into the target mold, heated and pressurized to 60℃, 8MPa, and kept warm and pressurized for 5min to fill the mold with the mixture. After the irradiation device releases Co-60γ rays, the irradiation dose is 25kGy, and the pellets are irradiated through the mold for 16min, the cross-linking enhancer absorbs radiation energy and decomposes to produce free radicals, which triggers the cross-linking reaction between the epoxy resin molecular chain with active free radicals and the unsaturated polyester resin. During the curing cross-linking reaction, the pressure is increased to 8MPa to make the product dense and reduce product defects. After the reaction is completed, the mold is opened to take out the recycled composite material sheet.

[0057] Comparative Example 1

[0058] In this embodiment, after the recycled wind turbine blade material is crushed and sieved, 800g of pellets are weighed and first released by the irradiation device Co-60γ rays for 5min irradiation, the irradiation dose is 10KGray, and the pellets are converted into active fillers. Then, 200g of unsaturated polyester resin and 15g of cross-linking enhancer are placed in a mixer to mix them evenly (mixing temperature is 60℃, time is 10min, speed is 30rad / min), and after sufficient mixing, the mixture is injected into the target mold, heated and pressurized to 60℃, 8MPa, and kept warm and pressurized for 5min to fill the mold with the mixture. After the irradiation device releases Co-60γ rays, the irradiation dose is 25kGy, and the pellets are irradiated through the mold for 16min, the cross-linking enhancer absorbs radiation energy and decomposes to produce free radicals, which triggers the cross-linking reaction between the epoxy resin molecular chain with active free radicals and the unsaturated polyester resin. During the curing cross-linking reaction, the pressure is increased to 8MPa to make the product dense and reduce product defects. After the reaction is completed, the mold is opened to take out the recycled composite material sheet.

[0059] Comparative Example 2

[0060] In this embodiment, after the recycled wind turbine blade material is crushed and sieved, 800g of pellets are weighed and first released by the irradiation device Co-60γ rays for 8min irradiation, the irradiation dose is 16KGray, and the pellets are converted into active fillers. Then, 200g of unsaturated polyester resin and 15g of cross-linking enhancer are placed in a mixer to mix them evenly (mixing temperature is 60℃, time is 10min, speed is 30rad / min), and after sufficient mixing, the mixture is injected into the target mold, heated and pressurized to 60℃, 8MPa, and kept warm and pressurized for 5min to fill the mold with the mixture. After the irradiation device releases Co-60γ rays, the irradiation dose is 10kGy, and after penetrating the mold to irradiate the pellets for 10min, the cross-linking enhancer absorbs radiation energy and decomposes to produce free radicals, which triggers the cross-linking reaction between the epoxy resin molecular chain with active free radicals and the unsaturated polyester resin. During the curing cross-linking reaction, the pressure is increased to 8MPa to make the product dense and reduce product defects. After the reaction is completed, the mold is opened to take out the recycled composite material sheet.

[0061] Comparative Example 3

[0062] In this comparative example, 1000g of unsaturated polyester resin and 30g of cross-linking enhancer are placed in a mixer to mix them evenly (mixing temperature is 60°C, time is 10min, speed is 30rad / min), and after sufficient mixing, the mixture is injected into the target mold, heated and pressurized to 60°C, 8MPa, and kept warm and pressurized for 5min to fill the mold with the mixture. The Co-60γ ray is released by the irradiation device, and the irradiation dose is 25kGy. After penetrating the mold to irradiate the mixture for 16min, the cross-linking enhancer absorbs the radiation energy and turns into an active monomer, which triggers the cross-linking reaction between the epoxy resin molecular chain with active free radicals and the unsaturated polyester resin. During the curing cross-linking reaction, the pressure is increased to 8MPa to make the product dense and reduce product defects. After the reaction is completed, the mold is opened to take out the recycled composite material board.

[0063] Comparative Example 4

[0064] In this comparative example, 600g of unirradiated wind turbine blade granules, 400g of unsaturated polyester resin and 25g of cross-linking enhancer are placed in a mixer to mix them evenly (mixing temperature is 60°C, time is 10min, speed is 30rad / min), and after sufficient mixing, the mixture is injected into the target mold, heated and pressurized to 60°C, 8MPa, and kept warm and pressurized for 5min to fill the mold with the mixture. The Co-60γ ray is released by the irradiation device, and the irradiation dose is 20kGy. After penetrating the mold to irradiate the mixture for 14min, the cross-linking enhancer absorbs the radiation energy and turns into an active monomer, which triggers the cross-linking reaction between the epoxy resin molecular chain with active free radicals and the unsaturated polyester resin. During the curing cross-linking reaction, the pressure is increased to 8MPa to make the product dense and reduce product defects. After the reaction is completed, the mold is opened to take out the recycled composite material sheet.

[0065] The mechanical properties test results of the composite materials prepared in Examples 1 to 5 and Comparative Examples 1 to 4 are shown in Table 1, wherein: the test method for tensile strength: GB / T 1040.1-2006, the test method for flexural strength: GB / T 1449-2005, the test method for impact strength: GB / T 1043.2-2018, the test method for Tg (glass transition temperature): GB / T33061.11-2022, the test method for thermal decomposition temperature: GB / T 37631-2019.

[0066] Table 1 Mechanical properties of recycled composite materials made from recycled wind turbine blade materials

[0067]

[0068] As can be seen from Table 1, compared with Example 1, Example 4, Example 5 and Comparative Example 1, the products prepared by the present invention by reasonably controlling the mass ratio of the active filler, the unsaturated polyester resin and the cross-linking enhancer have significantly improved tensile strength, flexural strength and impact strength compared with the product prepared in Comparative Example 1.

[0069] The mechanical properties and thermal stability of the recycled composite material prepared by the present invention are better improved compared with the pure unsaturated polyester resin (Comparative Example 3), and the recycled wind turbine blade material is not only 100% utilized, but also the glass fiber fabric is reused. The recycled composite material prepared from the unirradiated granules (Comparative Example 4) is improved by about 10-20% in terms of thermodynamic properties compared with the pure unsaturated polyester resin (Comparative Example 3), but because the wind turbine blade granules are not irradiated and are inert fillers, a certain mechanical property of the wind turbine blade recycled composite material is slightly reduced. On the other hand, if the mass proportion of the wind turbine blade granules is too high, the improvement in performance is reduced (Comparative Example 1 result). The present invention obtains a recycled composite material with excellent mechanical properties and thermal stability by reasonably adjusting the mass ratio of granules and unsaturated polyester resin.

[0070] The present invention provides a method for preparing a high-performance wind turbine blade regeneration composite material by irradiation, which realizes the green, efficient and value-added recycling of wind turbine blades, avoids the separation process of glass fiber and resin and retains the mechanical strength of glass fiber, saves resources, and has important economic significance and application value.

[0071] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for preparing a wind turbine blade recycled composite material, characterized in that: The following steps are involved: The wind turbine blade granules are subjected to a first irradiation to obtain an active filler; The active filler, unsaturated polyester resin and cross-linking enhancer are mixed to obtain a mixture; the unsaturated polyester resin includes one or more of terephthalic unsaturated polyester resin, bisphenol A unsaturated polyester resin and isophthalic unsaturated polyester resin; the mass ratio of the wind turbine blade granules to the polyester resin is (1:1) to (7:3); the cross-linking enhancer is one or more of methyl methacrylate, diallyl phthalate and propane trimethylol triacrylate; the mass of the cross-linking enhancer accounts for 2 to 3% of the total mass of the wind turbine blade granules and the polyester resin; Pressing the mixture in a mold to obtain a preformed body; Under the conditions of second irradiation and pressure application, the preformed body is cross-linked and cured to obtain the wind turbine blade recycled composite material.

2. The preparation method according to claim 1, characterized in that: The wind turbine blade granules are obtained by crushing wind turbine blade materials, and the particle size of the wind turbine blade granules is 0.2-2 mm.

3. The preparation method according to claim 1 or 2, characterized in that: The first irradiation is performed using Co-60 gamma rays, the dose of the first irradiation is 10-300 kGray, and the irradiation time is 3-10 min.

4. The preparation method according to claim 1, characterized in that: The mixing is carried out in a mixer at a temperature of 60-100° C. and a time of 5-10 minutes.

5. The preparation method according to claim 1, characterized in that: The mixing is carried out under stirring conditions, and the stirring speed is 20-30 rad / min.

6. The preparation method according to claim 1, characterized in that: The pressing temperature is 60-100° C., the pressure is 5-10 MPa, and the heat preservation and pressure holding time is 3-8 minutes.

7. The preparation method according to claim 1, characterized in that: The second irradiation is performed using Co-60γ rays, the dose of the second irradiation is 10-300 kGy, and the irradiation time is 10-25 min; the pressure condition during the cross-linking and curing is 8-10 MPa.

8. The wind turbine blade recycled composite material prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the wind turbine blade recycled composite material as claimed in claim 8 as an artificial board.