High-strength corrosion-resistant plastic barrel and preparation method thereof
Through the synergistic effect of using modified resin and elastic materials in plastic buckets, the insufficient performance problem of existing plastic buckets under high strength and extreme chemical corrosion is solved, and the improvement of high strength, corrosion resistance and environmental protection performance is achieved.
Patent Information
- Application Number
- CN202411163457.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-23
AI Technical Summary
When existing plastic barrels face high-strength use environment and extreme chemical corrosion, they are difficult to meet the strength, corrosion resistance and toughness requirements, and have poor environmental protection performance.
The composite resin is prepared from phosphorus pentoxide, anhydrous ethanol and bisphenol A type epoxy resin, combined with polypropylene resin and natural rubber, and is made of polylactic acid, dicyclohexylmethane diisocyanate, dihydrazine isophthalate and polyhydrazine Carbonates are raw materials to prepare elastic materials and add them to plastic buckets to improve corrosion resistance and strength through the synergistic effect of modified resin and elastic materials.
The corrosion resistance, strength and toughness of plastic barrels are significantly improved. The grafting reaction of phosphate groups and epoxy resins enhances the chemical stability of the resin. The elastic material absorbs stress and stores energy, delays the generation of cracks, and improves the overall performance. And the use of bio-based materials reduces environmental pollution.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of plastic barrel preparation, and in particular relates to a high-strength corrosion-resistant plastic barrel and a preparation method thereof. Background Art
[0002] With the development of modern industry, especially the rapid rise of chemical, pharmaceutical, pesticide and food industries, the demand for storage and transportation of various corrosive liquids and solid chemicals is growing. These industries not only require containers to have excellent corrosion resistance to cope with the erosion of strong corrosive substances such as acids, alkalis and salts, but also put forward extremely high requirements on their strength and stability to ensure that the integrity and safety of the structure can be maintained under complex and changing environmental conditions.
[0003] Although traditional metal barrels have certain strength and corrosion resistance, their heavy weight, high cost, easy rust and difficult recycling limit their widespread application. In contrast, plastic barrels have gradually become the market's first choice due to their advantages such as lightness, corrosion resistance, easy processing and recycling. However, ordinary plastic barrels often fail to meet the requirements when facing high-intensity use environments and extreme chemical corrosion. Therefore, the development of high-strength and corrosion-resistant plastic barrels and their preparation methods has become an urgent need in the industry.
[0004] Patent CN 109705473 B discloses an anti-aging, highly transparent, high-strength polypropylene plastic barrel and its preparation method, comprising the following components: 100 parts of polypropylene resin, 2-8 parts of maleic anhydride grafted polypropylene, 1-3 parts of paraffin oil, 1-10 parts of modified nano powder, 0.1-0.5 parts of antioxidant, 0.1-0.5 parts of auxiliary antioxidant, 0.1-1.2 parts of free radical scavenger and 0.1-0.4 parts of nucleating agent; wherein the modified nano powder is obtained by modifying the nano powder with coupling agent, polyester polyol and surfactant. The polypropylene plastic barrel prepared by the invention has good comprehensive effects such as high heat resistance, leakage resistance and low temperature resistance, but the strength, corrosion resistance, toughness and environmental protection performance of the plastic barrel obtained by this method still have room for improvement. Summary of the invention
[0005] The purpose of the present invention is to provide a high-strength and corrosion-resistant plastic barrel and a preparation method thereof, so as to solve the technical problems of poor strength, corrosion resistance, toughness and environmental protection performance of plastic barrels in the prior art.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The invention provides a high-strength corrosion-resistant plastic barrel, which is composed of the following components in parts by weight: 70-80 parts of a composite resin, 10-20 parts of an elastic material, 2-4 parts of silicon dioxide powder, 1-3 parts of a compatibilizer, and 0.5-0.8 parts of an antioxidant, wherein the composite resin is prepared from a modified resin, a polypropylene resin, and a natural rubber, the modified resin is prepared from phosphorus pentoxide, anhydrous ethanol, and a bisphenol A epoxy resin, and the elastic material is prepared from polylactic acid, dicyclohexylmethane diisocyanate, isophthalic acid dihydrazine, and polycarbonate.
[0008] Preferably, the method for preparing the composite resin comprises the following steps:
[0009] Q1: Add phosphorus pentoxide to a container containing anhydrous ethanol, place the container in an ice-water bath, heat and stir after adding, continue to heat and add deionized water for hydrolysis reaction, cool after the reaction is over to obtain an intermediate product;
[0010] Q2: Add the intermediate product to bisphenol A epoxy resin, heat and stir to react, then continue to keep the temperature to react, cool down, and obtain modified resin;
[0011] Q3: The modified resin, polypropylene resin and natural rubber are mixed, melt-extruded and granulated to obtain a composite resin.
[0012] In the above process, the synthetic reaction formula of the modified resin is as follows:
[0013]
[0014] Preferably, in Q1, the molar ratio of phosphorus pentoxide to anhydrous ethanol is (1-2): (4-8), and the phosphorus pentoxide is slowly added in three portions during the addition process, and stirred during the addition process. After the phosphorus pentoxide is completely dissolved, it is added again until the addition is completed. The heating and stirring temperature is 70-80°C, the stirring time is 3-4h, the heating temperature is continued to be 90-95°C, and the hydrolysis reaction time is 2-4h.
[0015] Preferably, in Q2, the molar ratio of the intermediate product to the bisphenol A epoxy resin is (2-4): (1-2), the average molecular weight of the bisphenol A epoxy resin is 1000, the heating and stirring reaction temperature is 80-90°C, the reaction time is 2-3h, the insulation reaction temperature is 70-80°C, and the insulation time is 0.5-1h; in Q3, the mass ratio of the modified resin, the polypropylene resin and the natural rubber is (20-30): (40-50): (10-20).
[0016] Preferably, the method for preparing the elastic material comprises the following steps:
[0017] S1: adding polylactic acid into a container, heating and melting it, extracting the water in the polylactic acid and the air in the container with a vacuum pump, then adding dicyclohexylmethane diisocyanate and dibutyltin dilaurate under nitrogen protection, heating and stirring, and obtaining a prepolymer;
[0018] S2: Add N,N-dimethylacetamide to the prepolymer, then add isophthalic acid dihydrazide, stir to react, add polycarbonate, continue to react, and after the reaction is completed, heat to obtain an elastic material.
[0019] In the above process, the synthetic reaction formula of the elastic material is as follows:
[0020]
[0021] Preferably, in S1, the molar ratio of polylactic acid to dicyclohexylmethane diisocyanate is (1-2):(2-4), the average molecular weight of polylactic acid is 2000, the heating melting temperature is 78-82°C, the heating stirring temperature is 60-65°C, and the stirring time is 3-4h.
[0022] Preferably, in S2, the molar ratio of prepolymer, isophthalic acid dihydrazide and polycarbonate is (1.1-2.2):(0.5-1):(1-2.2), the stirring reaction temperature is 28-32°C, the time is 2-3h, the average molecular weight of polycarbonate is 3000, the continued reaction time is 48-50h, and the heating temperature is 45-50°C.
[0023] Preferably, the method for preparing the high-strength and corrosion-resistant plastic barrel comprises the following steps:
[0024] Step (1): adding the composite resin and the elastic material into a heating stirrer for heating and stirring, and adding a compatibilizer, silica powder and an antioxidant during the heating and stirring process to obtain a mixed raw material;
[0025] Step (2): adding the mixed raw material to a dehydration kettle for heating and dehydration treatment to obtain a dehydrated raw material, adding the dehydrated raw material to a twin-screw extruder to extrude plastic particles, and placing the extruded plastic particles in a blow molding machine, blowing and shaping them according to a plastic barrel mold to obtain a plastic barrel blank;
[0026] Step (3): After fine processing and trimming of the plastic barrel blank, a high-strength and corrosion-resistant plastic barrel is obtained.
[0027] Preferably, in step (1), the heating and stirring temperature is 130-160° C., and the heating and stirring time is 2-4 h.
[0028] Preferably, in step (2), the temperature in the twin-screw extruder is 150-180°C, and the blowing and shaping pressure is 0.8-1.2 MPa.
[0029] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0030] 1. The present invention first uses phosphorus pentoxide, anhydrous ethanol and bisphenol A epoxy resin as raw materials to prepare a modified resin, and then mixes the modified resin with polypropylene resin and natural rubber to obtain a composite resin. The composite resin is used as the main raw material of a plastic barrel to effectively improve its corrosion resistance, strength and toughness. Then, polylactic acid, dicyclohexylmethane diisocyanate, isophthalic acid dihydrazine and polycarbonate are used as raw materials to prepare an elastic material, which is added as an additive in the preparation process of the plastic barrel to effectively improve its toughness and strength.
[0031] 2. The present invention uses phosphorus pentoxide, anhydrous ethanol, bisphenol A epoxy resin, polypropylene resin and natural rubber as raw materials to prepare a composite resin. Using it as the main raw material of a plastic barrel can effectively improve its corrosion resistance, strength and toughness. The phosphoric acid group is grafted into the bisphenol A epoxy resin, which can effectively increase the cross-linking density of the epoxy resin and arrange its molecular chains more closely, thereby reducing the penetration and diffusion of the corrosive medium inside the resin and delaying the occurrence of the corrosion process. The phosphoric acid group can resist the erosion of chemical substances and has stable chemical stability. After being grafted with the bisphenol A epoxy resin, the chemical stability can be transferred to the entire resin system, so that the composite resin shows higher stability when facing corrosive media, thereby improving the corrosion resistance of the plastic barrel, and further improving its strength and toughness.
[0032] 3. The present invention uses polylactic acid, dicyclohexylmethane diisocyanate, isophthalic acid dihydrazine and polycarbonate as raw materials to prepare an elastic elastic material, which is added to the composite resin as an additive to effectively improve the strength and toughness of the plastic barrel. The elastic material exists as a dispersed phase in the composite resin. When impacted by external force, the elastic material can absorb and disperse part of the stress, reduce the stress concentration phenomenon of the composite resin, and delay the generation and expansion of cracks; when the elastic material is deformed during the force-bearing process, part of the mechanical energy will be converted into elastic potential energy for storage. When the external force is removed, the elastic material gradually returns to its original state and releases the stored energy, thereby consuming part of the impact energy and improving the toughness of the material; the synergistic effect formed between the elastic material and the resin matrix makes the overall performance of the plastic barrel better than that of a single component. The two cooperate with each other and jointly bear the load to achieve strength improvement. At the same time, the polylactic acid used in the elastic material is a bio-based and renewable biodegradable material, which can be decomposed into carbon dioxide and water by microorganisms in the environment and will not cause long-term pollution to the environment. DETAILED DESCRIPTION
[0033] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Example 1
[0035] This embodiment discloses a method for preparing a composite resin, comprising the following steps:
[0036] Q1: Add 1.5g of phosphorus pentoxide to a container containing 2.46mL of anhydrous ethanol. The container is placed in an ice-water bath. During the addition process, the phosphorus pentoxide is slowly added in three portions with stirring. After the phosphorus pentoxide is completely dissolved, add again until the addition is complete. After the addition is complete, heat to 75°C and stir for 4h. After the stirring is complete, continue to heat to 90°C, add 0.05mL of deionized water, and hydrolyze for 4h. After the reaction is complete, cool to obtain an intermediate product.
[0037] Q2: 1.17 mL of the intermediate product was added to 4.87 g of bisphenol A epoxy resin with an average molecular weight of 1000, heated and stirred at 90°C for 3 h, then kept at 80°C for 0.5 h, and cooled to obtain a modified resin;
[0038] Q3: 25 g of modified resin, 45 g of polypropylene resin and 15 g of natural rubber were mixed, melt-extruded and granulated to obtain a composite resin.
[0039] This embodiment discloses a method for preparing an elastic material, comprising the following steps:
[0040] S1: 11.46 g of polylactic acid with an average molecular weight of 2000 was added to a container, heated to 80°C to melt, and the water in the polylactic acid and the air in the container were extracted with a vacuum pump. Subsequently, 3 g of dicyclohexylmethane diisocyanate and 0.22 mL of dibutyltin dilaurate were added under nitrogen protection, and heated at 65°C with stirring for 4 h to obtain a prepolymer;
[0041] S2: 40 mL of N,N-dimethylacetamide was added to 8.86 g of prepolymer, followed by 0.15 g of isophthalic acid dihydrazine, and the mixture was stirred at 32° C. for 3 h. 10.21 g of polycarbonate with an average molecular weight of 3000 was added, and the reaction was continued for 48 h. After the reaction was completed, the mixture was heated at 50° C. to obtain an elastic material.
[0042] This embodiment discloses a high-strength and corrosion-resistant plastic barrel, which is composed of the following components in parts by weight: 75 parts of composite resin, 15 parts of elastic material, 3 parts of silicon dioxide powder, 2 parts of a compatibilizer, and 0.7 parts of an antioxidant.
[0043] This embodiment discloses a method for preparing a high-strength, corrosion-resistant plastic barrel, comprising the following steps:
[0044] Step (1): adding the composite resin and the elastic material into a heating stirrer for heating and stirring at 160° C. for 4 hours, and adding a compatibilizer, silica powder and an antioxidant during the heating and stirring process to obtain a mixed raw material;
[0045] Step (2): adding the mixed raw material to a dehydration kettle for heating and dehydration treatment to obtain a dehydrated raw material, adding the dehydrated raw material to a twin-screw extruder at 180° C. to extrude plastic particles, and placing the extruded plastic particles in a blow molding machine, blowing and shaping them according to a plastic barrel mold, the blowing and shaping pressure is 0.9 MPa, to obtain a plastic barrel blank;
[0046] Step (3): After fine processing and trimming of the plastic barrel blank, a high-strength and corrosion-resistant plastic barrel is obtained.
[0047] Example 2
[0048] This embodiment discloses a method for preparing a composite resin, comprising the following steps:
[0049] Q1: 1.02 g of phosphorus pentoxide was added to a container containing 1.64 mL of anhydrous ethanol. The container was placed in an ice-water bath. During the addition process, phosphorus pentoxide was slowly added in three portions with stirring. After phosphorus pentoxide was completely dissolved, it was added again until the addition was complete. After the addition was complete, the temperature was raised to 75°C and stirred for 4 hours. After the stirring was completed, the temperature was continued to be raised to 90°C, 0.03 mL of deionized water was added, and the hydrolysis reaction was carried out for 4 hours. After the reaction was completed, the temperature was lowered to obtain an intermediate product.
[0050] Q2: 0.78 mL of the intermediate product was added to 3.25 g of bisphenol A epoxy resin with an average molecular weight of 1000, heated and stirred at 90°C for 3 h, then kept at 80°C for 0.5 h, and cooled to obtain a modified resin;
[0051] Q3: 20 g of modified resin, 40 g of polypropylene resin and 10 g of natural rubber were mixed, melt-extruded and granulated to obtain a composite resin.
[0052] This embodiment discloses a method for preparing an elastic material, comprising the following steps:
[0053] S1: 7.64 g of polylactic acid with an average molecular weight of 2000 was added to a container, heated to 80°C to melt, and the water in the polylactic acid and the air in the container were extracted with a vacuum pump. Subsequently, 2 g of dicyclohexylmethane diisocyanate and 0.22 mL of dibutyltin dilaurate were added under nitrogen protection, and heated at 65°C with stirring for 4 h to obtain a prepolymer;
[0054] S2: 40 mL of N,N-dimethylacetamide was added to 5.91 g of prepolymer, followed by 0.1 g of isophthalic acid dihydrazine, and the mixture was stirred at 32° C. for 3 h. 6.38 g of polycarbonate with an average molecular weight of 3000 was added, and the reaction was continued for 48 h. After the reaction was completed, the mixture was heated at 50° C. to obtain an elastic material.
[0055] The present embodiment discloses a high-strength and corrosion-resistant plastic barrel, which is composed of the following components in parts by weight: 70 parts of composite resin, 10 parts of elastic material, 2 parts of silicon dioxide powder, 1 part of a compatibilizer, and 0.5 parts of an antioxidant.
[0056] This embodiment discloses a method for preparing a high-strength, corrosion-resistant plastic barrel, comprising the following steps:
[0057] Step (1): adding the composite resin and the elastic material into a heating stirrer for heating and stirring at 160° C. for 4 hours, and adding a compatibilizer, silica powder and an antioxidant during the heating and stirring process to obtain a mixed raw material;
[0058] Step (2): adding the mixed raw material to a dehydration kettle for heating and dehydration treatment to obtain a dehydrated raw material, adding the dehydrated raw material to a twin-screw extruder at 180° C. to extrude plastic particles, and placing the extruded plastic particles in a blow molding machine, blowing and shaping them according to a plastic barrel mold, the blowing and shaping pressure is 0.9 MPa, to obtain a plastic barrel blank;
[0059] Step (3): After fine processing and trimming of the plastic barrel blank, a high-strength and corrosion-resistant plastic barrel is obtained.
[0060] Example 3
[0061] This embodiment discloses a method for preparing a composite resin, comprising the following steps:
[0062] Q1: Add 1.98g of phosphorus pentoxide to a container containing 3.28mL of anhydrous ethanol. The container is placed in an ice-water bath. During the addition process, the phosphorus pentoxide is slowly added in three times. Stirring is performed during the addition process. After the phosphorus pentoxide is completely dissolved, add again until the addition is completed. After the addition is completed, heat to 75°C and stir for 4h. After the stirring is completed, continue to heat to 90°C, add 0.05mL of deionized water, and hydrolyze for 4h. After the reaction is completed, cool to obtain an intermediate product.
[0063] Q2: 1.56 mL of the intermediate product was added to 6.49 g of bisphenol A epoxy resin with an average molecular weight of 1000, heated and stirred at 90°C for 3 h, then kept at 80°C for 0.5 h, and cooled to obtain a modified resin;
[0064] Q3: 30 g of modified resin, 50 g of polypropylene resin and 20 g of natural rubber were mixed, melt-extruded and granulated to obtain a composite resin.
[0065] This embodiment discloses a method for preparing an elastic material, comprising the following steps:
[0066] S1: 15.28 g of polylactic acid with an average molecular weight of 2000 was added to a container, heated to 80°C to melt, and the water in the polylactic acid and the air in the container were extracted with a vacuum pump. Then, 4 g of dicyclohexylmethane diisocyanate and 0.22 mL of dibutyltin dilaurate were added under nitrogen protection, and heated at 65°C with stirring for 4 h to obtain a prepolymer;
[0067] S2: 40 mL of N,N-dimethylacetamide was added to 11.81 g of prepolymer, followed by 0.2 g of isophthalic acid dihydrazine, and the mixture was stirred at 32° C. for 3 h. 14.04 g of polycarbonate with an average molecular weight of 3000 was added, and the reaction was continued for 48 h. After the reaction was completed, the mixture was heated at 50° C. to obtain an elastic material.
[0068] This embodiment discloses a high-strength and corrosion-resistant plastic barrel, which is composed of the following components in parts by weight: 80 parts of composite resin, 20 parts of elastic material, 4 parts of silicon dioxide powder, 3 parts of a compatibilizer, and 0.8 parts of an antioxidant.
[0069] This embodiment discloses a method for preparing a high-strength, corrosion-resistant plastic barrel, comprising the following steps:
[0070] Step (1): adding the composite resin and the elastic material into a heating stirrer for heating and stirring at 160° C. for 4 hours, and adding a compatibilizer, silica powder and an antioxidant during the heating and stirring process to obtain a mixed raw material;
[0071] Step (2): adding the mixed raw material to a dehydration kettle for heating and dehydration treatment to obtain a dehydrated raw material, adding the dehydrated raw material to a twin-screw extruder at 180° C. to extrude plastic particles, and placing the extruded plastic particles in a blow molding machine, blowing and shaping them according to a plastic barrel mold, the blowing and shaping pressure is 0.9 MPa, to obtain a plastic barrel blank;
[0072] Step (3): After fine processing and trimming of the plastic barrel blank, a high-strength and corrosion-resistant plastic barrel is obtained.
[0073] Example 4
[0074] This embodiment discloses a method for preparing a composite resin, comprising the following steps:
[0075] Q1: Add 1.2g of phosphorus pentoxide to a container containing 2.07mL of anhydrous ethanol. The container is placed in an ice-water bath. During the addition process, the phosphorus pentoxide is slowly added in three portions with stirring. After the phosphorus pentoxide is completely dissolved, add again until the addition is complete. After the addition is complete, heat to 75°C and stir for 4h. After the stirring is complete, continue to heat to 90°C, add 0.05mL of deionized water, and hydrolyze for 4h. After the reaction is complete, cool to obtain an intermediate product.
[0076] Q2: 0.93 mL of the intermediate product was added to 4.05 g of bisphenol A epoxy resin with an average molecular weight of 1000, heated and stirred at 90°C for 3 h, then kept at 80°C for 0.5 h, and cooled to obtain a modified resin;
[0077] Q3: 22 g of modified resin, 42 g of polypropylene resin and 12 g of natural rubber were mixed, melt-extruded and granulated to obtain a composite resin.
[0078] This embodiment discloses a method for preparing an elastic material, comprising the following steps:
[0079] S1: 9.06 g of polylactic acid with an average molecular weight of 2000 was added to a container, heated to 80°C to melt, and the water in the polylactic acid and the air in the container were extracted with a vacuum pump. Subsequently, 1.1 g of dicyclohexylmethane diisocyanate and 0.22 mL of dibutyltin dilaurate were added under nitrogen protection, and heated at 65°C with stirring for 4 h to obtain a prepolymer;
[0080] S2: 40 mL of N,N-dimethylacetamide was added to 7.39 g of prepolymer, followed by 0.12 g of isophthalic acid dihydrazine, and the mixture was stirred at 32° C. for 3 h. 8.17 g of polycarbonate with an average molecular weight of 3000 was added, and the reaction was continued for 48 h. After the reaction was completed, the mixture was heated at 50° C. to obtain an elastic material.
[0081] The present embodiment discloses a high-strength and corrosion-resistant plastic barrel, which is composed of the following components in parts by weight: 72 parts of composite resin, 12 parts of elastic material, 2.5 parts of silicon dioxide powder, 1.5 parts of a compatibilizer, and 0.6 parts of an antioxidant.
[0082] This embodiment discloses a method for preparing a high-strength, corrosion-resistant plastic barrel, comprising the following steps:
[0083] Step (1): adding the composite resin and the elastic material into a heating stirrer for heating and stirring at 160° C. for 4 hours, and adding a compatibilizer, silica powder and an antioxidant during the heating and stirring process to obtain a mixed raw material;
[0084] Step (2): adding the mixed raw material to a dehydration kettle for heating and dehydration treatment to obtain a dehydrated raw material, adding the dehydrated raw material to a twin-screw extruder at 180° C. to extrude plastic particles, and placing the extruded plastic particles in a blow molding machine, blowing and shaping them according to a plastic barrel mold, the blowing and shaping pressure is 0.9 MPa, to obtain a plastic barrel blank;
[0085] Step (3): After fine processing and trimming of the plastic barrel blank, a high-strength and corrosion-resistant plastic barrel is obtained.
[0086] Example 5
[0087] This embodiment discloses a method for preparing a composite resin, comprising the following steps:
[0088] Q1: 1.8 g of phosphorus pentoxide was added to a container containing 1.85 mL of anhydrous ethanol. The container was placed in an ice-water bath. During the addition process, the phosphorus pentoxide was slowly added in three portions with stirring. After the phosphorus pentoxide was completely dissolved, it was added again until the addition was completed. After the addition was completed, the temperature was raised to 75°C and stirred for 4 hours. After the stirring was completed, the temperature was continued to be raised to 90°C, 0.05 mL of deionized water was added, and the hydrolysis reaction was carried out for 4 hours. After the reaction was completed, the temperature was lowered to obtain an intermediate product.
[0089] Q2: 1.27 mL of the intermediate product was added to 5.12 g of bisphenol A epoxy resin with an average molecular weight of 1000, heated and stirred at 90°C for 3 h, then kept at 80°C for 0.5 h, and cooled to obtain a modified resin;
[0090] Q3: 28 g of modified resin, 47 g of polypropylene resin and 18 g of natural rubber were mixed, melt-extruded and granulated to obtain a composite resin.
[0091] This embodiment discloses a method for preparing an elastic material, comprising the following steps:
[0092] S1: 12.42 g of polylactic acid with an average molecular weight of 2000 was added to a container, heated to 80°C to melt, and the water in the polylactic acid and the air in the container were extracted with a vacuum pump. Subsequently, 3.4 g of dicyclohexylmethane diisocyanate and 0.22 mL of dibutyltin dilaurate were added under nitrogen protection, and heated at 65°C with stirring for 4 h to obtain a prepolymer;
[0093] S2: 40 mL of N,N-dimethylacetamide was added to 9.73 g of prepolymer, followed by 0.17 g of isophthalic acid dihydrazine, and the mixture was stirred at 32° C. for 3 h. 12.53 g of polycarbonate with an average molecular weight of 3000 was added, and the reaction was continued for 48 h. After the reaction was completed, the mixture was heated at 50° C. to obtain an elastic material.
[0094] The present embodiment discloses a high-strength and corrosion-resistant plastic barrel, which is composed of the following components in parts by weight: 76 parts of composite resin, 18 parts of elastic material, 3.5 parts of silicon dioxide powder, 1.8 parts of a compatibilizer, and 0.57 parts of an antioxidant.
[0095] This embodiment discloses a method for preparing a high-strength, corrosion-resistant plastic barrel, comprising the following steps:
[0096] Step (1): adding the composite resin and the elastic material into a heating stirrer for heating and stirring at 160° C. for 4 hours, and adding a compatibilizer, silica powder and an antioxidant during the heating and stirring process to obtain a mixed raw material;
[0097] Step (2): adding the mixed raw material to a dehydration kettle for heating and dehydration treatment to obtain a dehydrated raw material, adding the dehydrated raw material to a twin-screw extruder at 180° C. to extrude plastic particles, and placing the extruded plastic particles in a blow molding machine, blowing and shaping them according to a plastic barrel mold, the blowing and shaping pressure is 0.9 MPa, to obtain a plastic barrel blank;
[0098] Step (3): After fine processing and trimming of the plastic barrel blank, a high-strength and corrosion-resistant plastic barrel is obtained.
[0099] Comparative Example 1
[0100] Comparative Example 1 Compared with Example 1, in the preparation process of the composite resin in Comparative Example 1, phosphorus pentoxide was not added, and other conditions remained unchanged.
[0101] Comparative Example 2
[0102] Comparative Example 2 Compared with Example 1, in the preparation process of the composite resin in Comparative Example 2, no bisphenol A epoxy resin was added, and other conditions remained unchanged.
[0103] Comparative Example 3
[0104] Comparative Example 3 Compared with Example 1, in the preparation process of the elastic material in Comparative Example 3, no polylactic acid is added, and other conditions remain unchanged.
[0105] Comparative Example 4
[0106] Comparative Example 4 Compared with Example 1, in the preparation process of the elastic material in Comparative Example 4, no polycarbonate is added, and other conditions remain unchanged.
[0107] Comparative Example 5
[0108] Comparative Example 5 Compared with Example 1, in the preparation process of the plastic barrel in Comparative Example 5, no modified resin is added, and other conditions remain unchanged.
[0109] Comparative Example 6
[0110] Comparative Example 6 Compared with Example 1, in the preparation process of the plastic barrel in Comparative Example 6, no elastic material is added, and other conditions remain unchanged.
[0111] The samples prepared according to Examples 1-5 and Comparative Examples 1-6 were subjected to performance tests, the shear strength of the samples was tested according to HG / T 3839-2006, the corrosion resistance of the samples was tested according to GB / T 10125-2021, and the mass reduction rate = [(m 前 -m 后 ) / m 前 ]×100%, the elongation at break of the sample was tested according to GB / T 13022-91, and the test results are shown in Table 1:
[0112] Table 1
[0113]
[0114] It can be seen from the test results in Table 1 that the plastic barrels prepared in Examples 1-5 of the present invention have excellent corrosion resistance, strength and toughness. Comparison between Comparative Example 1 and Examples 1-5 shows that adding phosphorus pentoxide can effectively improve the corrosion resistance, strength and toughness of the plastic barrel; comparison between Comparative Example 2 and Examples 1-5 shows that adding bisphenol A epoxy resin can effectively improve the corrosion resistance, strength and toughness of the plastic barrel; comparison between Comparative Example 3 and Examples 1-5 shows that adding polylactic acid can effectively improve the strength and toughness of the plastic barrel; comparison between Comparative Example 4 and Examples 1-5 shows that adding polycarbonate can effectively improve the strength and toughness of the plastic barrel; comparison between Comparative Example 5 and Examples 1-5 shows that adding modified resin can effectively improve the corrosion resistance, strength and toughness of the plastic barrel; comparison between Comparative Example 6 and Examples 1-5 shows that adding elastic material can effectively improve the strength and toughness of the plastic barrel.
[0115] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
[0116] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. High-strength and corrosion-resistant plastic barrels, It is characterized in that The invention is composed of the following components in parts by weight: 70-80 parts of a composite resin, 10-20 parts of an elastic material, 2-4 parts of silicon dioxide powder, 1-3 parts of a compatibilizer, and 0.5-0.8 parts of an antioxidant, wherein the composite resin is prepared from a modified resin, a polypropylene resin, and a natural rubber, the modified resin is prepared from phosphorus pentoxide, anhydrous ethanol, and a bisphenol A epoxy resin, and the elastic material is prepared from polylactic acid, dicyclohexylmethane diisocyanate, isophthalic acid dihydrazine, and polycarbonate; The preparation method of the composite resin comprises the following steps: Q1: Add phosphorus pentoxide to a container containing anhydrous ethanol, place the container in an ice-water bath, heat and stir after adding, continue to heat and add deionized water for hydrolysis reaction, cool after the reaction is over to obtain an intermediate product; Q2: Add the intermediate product to bisphenol A epoxy resin, heat and stir to react, then continue to keep the temperature to react, cool down, and obtain modified resin; Q3: The modified resin, polypropylene resin and natural rubber are mixed, melt-extruded and granulated to obtain a composite resin; The method for preparing the elastic material comprises the following steps: S1: adding polylactic acid into a container, heating and melting it, extracting the water in the polylactic acid and the air in the container with a vacuum pump, then adding dicyclohexylmethane diisocyanate and dibutyltin dilaurate under nitrogen protection, heating and stirring, and obtaining a prepolymer; S2: adding N,N-dimethylacetamide to the prepolymer, then adding isophthalic acid dihydrazine, stirring to react, adding polycarbonate, continuing the reaction, and heating after the reaction is completed to obtain an elastic material; In S1, the molar ratio of polylactic acid to dicyclohexylmethane diisocyanate is (1-2): (2-4), the average molecular weight of polylactic acid is 2000, the heating melting temperature is 78-82° C., the heating stirring temperature is 60-65° C., and the stirring time is 3-4 h; In S2, the molar ratio of prepolymer, isophthalic acid dihydrazide and polycarbonate is (1.1-2.2): (0.5-1): (1-2.2), the stirring reaction temperature is 28-32°C, the time is 2-3h, the average molecular weight of polycarbonate is 3000, the continued reaction time is 48-50h, and the heating temperature is 45-50°C.
2. The high-strength, corrosion-resistant plastic barrel according to claim 1, It is characterized in that In the Q1, the molar ratio of phosphorus pentoxide to anhydrous ethanol is (1-2): (4-8). During the addition process, phosphorus pentoxide is slowly added in three portions with stirring. After the phosphorus pentoxide is completely dissolved, it is added again until the addition is complete. The heating and stirring temperature is 70-80°C, the stirring time is 3-4h, the heating temperature is continued to be 90-95°C, and the hydrolysis reaction time is 2-4h.
3. The high-strength, corrosion-resistant plastic barrel according to claim 1, It is characterized in that In Q2, the molar ratio of the intermediate product to the bisphenol A epoxy resin is (2-4): (1-2), the average molecular weight of the bisphenol A epoxy resin is 1000, the heating and stirring reaction temperature is 80-90°C, the reaction time is 2-3h, the insulation reaction temperature is 70-80°C, and the insulation time is 0.5-1h; in Q3, the mass ratio of the modified resin, the polypropylene resin and the natural rubber is (20-30): (40-50): (10-20).
4. A method for preparing a high-strength, corrosion-resistant plastic barrel according to any one of claims 1 to 3, It is characterized in that The following steps are involved: Step (1): adding the composite resin and the elastic material into a heating type stirrer for heating and stirring, and adding a compatibilizer, silica powder and an antioxidant during the heating and stirring process to obtain a mixed raw material; Step (2): adding the mixed raw material to a dehydration kettle for heating and dehydration treatment to obtain a dehydrated raw material, adding the dehydrated raw material to a twin-screw extruder to extrude plastic particles, and placing the extruded plastic particles in a blow molding machine, blowing and shaping them according to a plastic barrel mold to obtain a plastic barrel blank; Step (3): After fine processing and trimming of the plastic barrel blank, a high-strength and corrosion-resistant plastic barrel is obtained.
5. The method for preparing the high-strength, corrosion-resistant plastic barrel according to claim 4, It is characterized in that In the step (1), the heating and stirring temperature is 130-160° C., and the heating and stirring time is 2-4 hours.
6. The method for preparing the high-strength, corrosion-resistant plastic barrel according to claim 4, It is characterized in that In the step (2), the temperature in the twin-screw extruder is 150-180° C., and the blowing and shaping pressure is 0.8-1.2 MPa.