Rubber powder modified asphalt and preparation method thereof
By adding modified red mud, carbon nanotubes and specific stabilizers to the rubber powder modified asphalt, the problems of high viscosity and poor stability of existing rubber powder modified asphalt are solved, and low viscosity, high stability and wear resistance are achieved Improve the service life and service quality of the road surface.
Patent Information
- Application Number
- CN202411163473.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-23
AI Technical Summary
The existing rubber powder modified asphalt has poor rut resistance and poor wear resistance due to excessive viscosity and unstable system, which cannot effectively solve the problems of waste tire accumulation and improved asphalt performance.
Using a mixture of petroleum asphalt, rubber powder, modified red mud and carbon nanotubes, combined with dodecylbenzenesulfonic acid and bio-oil, oxidized polyethylene wax, and cycloalkane oil, through specific heating, stirring, and shearing Cutting and swelling process to prepare rubber powder modified asphalt with low viscosity and high stability.
It reduces the viscosity and temperature sensitivity of rubber powder modified asphalt, improves high and low temperature stability, fatigue resistance and wear resistance, enhances the road surface's resistance to permanent deformation and rut resistance, and is suitable for road surfaces.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of modified asphalt preparation, and specifically relates to rubber powder modified asphalt and a preparation method thereof. Background Art
[0002] Asphalt is a dark brown complex mixture of hydrocarbons of different molecular weights and their non-metallic derivatives. It is a high-viscosity organic liquid and an organic gelling material that is waterproof, moisture-proof and anti-corrosive. Asphalt is divided into three types: coal tar asphalt, petroleum asphalt and natural asphalt; among them, coal tar asphalt is a by-product of coking, petroleum asphalt is the residue after crude oil distillation, and natural asphalt is stored underground to form mineral layers or accumulate on the surface of the earth's crust. Asphalt is widely used in construction, road construction and other fields due to its excellent ductility.
[0003] The main components of waste tires are natural rubber powder, synthetic rubber powder, carbon black, antioxidants and metal oxides, which are basically beneficial to improving the performance of asphalt. Road researchers have already applied them to modified asphalt and asphalt mixtures to produce new high-performance rubber powder modified asphalt and its mixture. This not only solves the environmental and land occupation problems caused by the accumulation of waste tires, but also increases the viscosity of the base asphalt, improves the low-temperature performance of asphalt, increases the anti-aging and anti-fatigue properties of asphalt, and improves the service life and service quality of roads.
[0004] Rubber powder modified asphalt is made by adding a certain amount of rubber powder and admixtures to base asphalt at a certain temperature and time through stirring, shearing, swelling and development processes. However, due to surface energy, rubber powder and asphalt have poor mutual solubility, which easily leads to segregation and stratification. In addition, the viscosity of rubber powder modified asphalt is too high, which affects the quality of modified asphalt products. When it is applied to highway asphalt pavement, it has the defects of poor rutting resistance and poor wear resistance. Therefore, it is urgent to explore a rubber powder modified asphalt and its preparation method. Summary of the invention
[0005] The purpose of the present invention is to provide a rubber powder modified asphalt. The rubber powder modified asphalt has lower viscosity, higher system stability and plasticity. In addition, the present invention also provides a preparation method thereof.
[0006] The rubber powder modified asphalt of the present invention is composed of the following raw materials in parts by weight: 100 parts of petroleum asphalt, 23-25 parts of rubber powder, 6-8 parts of a mixture of modified red mud and carbon nanotubes, 3.3-4.7 parts of dodecylbenzene sulfonic acid and 5-7 parts of a stabilizer, wherein the stabilizer is a mixture of bio-oil, oxidized polyethylene wax and cycloalkane oil.
[0007] Preferably, the rubber powder modified asphalt described in the present invention is composed of the following raw materials, by weight: 100 parts of petroleum asphalt, 24 parts of rubber powder, 7 parts of a mixture of modified red mud and carbon nanotubes, 4 parts of dodecylbenzene sulfonic acid and 6 parts of a stabilizer, wherein the stabilizer is a mixture of bio-oil, oxidized polyethylene wax and cycloalkane oil.
[0008] in:
[0009] The mass ratio of the bio-oil, the oxidized polyethylene wax and the cycloalkane oil in the stabilizer is 1.2-1.4: 2.1-2.3: 0.8-1.0.
[0010] Rubber powder is prepared by crushing waste tires, and the particle size is 0.212-0.300mm.
[0011] The bio-oil is castor oil, and the manufacturer is Guyun Chemical (Changzhou) Co., Ltd.
[0012] The cycloparaffin oil is NAP1004, and the manufacturer is Karamay Petrochemical Company.
[0013] The preparation method of the mixture of modified red mud and carbon nanotubes consists of the following steps:
[0014] ① Add sintered red mud into water, then add dilute sulfuric acid to adjust the pH value of the system to 10.5, sieve with a 60-mesh sieve, take the sieve and dry it to prepare the red mud raw material;
[0015] ② The red mud raw material and carbon nanotubes prepared in step ① are placed in a ball mill, and distilled water and KH550 silane coupling agent are added for ball milling modification to prepare a mixture of modified red mud and carbon nanotubes.
[0016] in:
[0017] The chemical composition of the sintered red mud in step ① is as follows in terms of mass percentage: Fe 2 O 3 11.05%, Al 2 O 3 7.59%, SiO 2 21.78%, CaO 41.59%, Na 2 O 3.01%, TiO 2 3.24%, K 2 O 0.35%, MgO 1.65%, loss on ignition 9.74%.
[0018] In step ①, the drying is performed at 105-110° C. for 5-5.5 hours.
[0019] In step ②, the mass ratio of the mixture of red mud raw material and carbon nanotubes to distilled water is 1:3-3.5.
[0020] In step ②, the mass of KH550 silane coupling agent accounts for 5.5-6.0% of the mass of the mixture of red mud raw material and carbon nanotubes.
[0021] During the ball milling modification in step ②, the rotation speed of the ball mill is 500-600 r / min, and the ball milling time is 3-3.2 h.
[0022] The method for preparing the rubber powder modified asphalt of the present invention comprises the following steps:
[0023] (1) Melting petroleum asphalt at 163-165°C, adding rubber powder to the petroleum asphalt and stirring evenly, then adding a mixture of modified red mud and carbon nanotubes, dodecylbenzene sulfonic acid and a stabilizer, keeping the mixture at 180-185°C for 30-35 minutes, and then shearing;
[0024] (2) After the shearing is completed, swelling is carried out to prepare rubber powder modified asphalt.
[0025] in:
[0026] In step (1), the shearing speed is 5000-7000 r / min, and the shearing time is 40-50 min.
[0027] In step (2), the swelling temperature is 180-185° C. and the swelling time is 70-75 min.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] (1) The rubber powder modified asphalt described in the present invention is compounded with a stabilizer, dodecylbenzene sulfonic acid, and a mixture of modified red mud and carbon nanotubes. The three act synergistically to reduce the viscosity and temperature sensitivity of the prepared rubber powder modified asphalt, and improve the high and low temperature stability, plasticity and wear resistance of the system. Among them, the stabilizer can reduce the processing temperature and viscosity of the rubber powder modified asphalt, and improve the high and low temperature stability and fatigue resistance of the rubber powder modified asphalt. The addition of dodecylbenzene sulfonic acid can degrade the rubber powder, increase the hardness of the prepared rubber powder modified asphalt, and enhance the deformation recovery ability. When it is applied to highway pavement, it can improve the road surface's resistance to permanent deformation and rutting. The addition of a mixture of modified red mud and carbon nanotubes can improve the wear resistance, heat aging resistance and temperature sensitivity of the rubber modified asphalt system.
[0030] (2) The rubber powder modified asphalt described in the present invention has a synergistic effect among the bio-oil, oxidized polyethylene wax and cycloalkane oil in the stabilizer. Among them, the bio-oil is castor oil. The addition of castor oil can reduce the processing temperature of rubber asphalt, accelerate the swelling rate of rubber, and improve the anti-fatigue properties and high and low temperature stability of the modified asphalt, improve the overall rheological properties of asphalt, and at the same time increase the amount of rubber incorporated. The addition of oxidized polyethylene wax can reduce the viscosity of rubber powder modified asphalt and improve the stability of the system. The addition of cycloalkane oil can further reduce the viscosity of the modified asphalt and improve the compatibility between rubber powder and asphalt.
[0031] (3) The reason why the mixture of modified red mud and carbon nanotubes is added to the rubber powder modified asphalt of the present invention is that carbon nanotubes have the properties of light weight, high thermal conductivity and high modulus. The addition of carbon nanotubes can improve the wear resistance and elastic recovery of the rubber modified asphalt system. When compounded with red mud, the addition of red mud can reduce the temperature sensitivity of the rubber modified asphalt system and improve the stability of the system. The modification treatment of silane coupling agent can improve the dispersibility in the system, improve the interfacial force and prevent the occurrence of agglomeration.
[0032] (4) The method for preparing the rubber powder modified asphalt of the present invention has a simple process, easy to control parameters, and easy to realize industrial production. DETAILED DESCRIPTION
[0033] The present invention is further described below with reference to the embodiments.
[0034] Example 1
[0035] The rubber powder modified asphalt described in this Example 1 is composed of the following raw materials, in parts by weight: 100 parts of petroleum asphalt, 24 parts of rubber powder, 7 parts of a mixture of modified red mud and carbon nanotubes, 4 parts of dodecylbenzene sulfonic acid and 6 parts of a stabilizer, wherein the stabilizer is a mixture of bio-oil, oxidized polyethylene wax and cycloalkane oil.
[0036] in:
[0037] The mass ratio of bio-oil, oxidized polyethylene wax and cycloalkane oil in the stabilizer is 1.3:2.2:0.9.
[0038] Rubber powder is prepared by crushing waste tires, and the particle size is 0.250mm.
[0039] The bio-oil is castor oil, and the manufacturer is Guyun Chemical (Changzhou) Co., Ltd.
[0040] The cycloparaffin oil is NAP1004, and the manufacturer is Karamay Petrochemical Company.
[0041] The preparation method of the mixture of modified red mud and carbon nanotubes consists of the following steps:
[0042] ① Add sintered red mud into water, then add dilute sulfuric acid to adjust the pH value of the system to 10.5, sieve with a 60-mesh sieve, take the sieve and dry it to prepare the red mud raw material;
[0043] ② The red mud raw material and carbon nanotubes prepared in step ① are placed in a ball mill, and distilled water and KH550 silane coupling agent are added for ball milling modification to prepare a mixture of modified red mud and carbon nanotubes.
[0044] in:
[0045] The chemical composition of the sintered red mud in step ① is as follows in terms of mass percentage: Fe 2 O 3 11.05%, Al 2 O 3 7.59%, SiO 2 21.78%, CaO 41.59%, Na 2 O 3.01%, TiO 2 3.24%, K 2 O 0.35%, MgO 1.65%, loss on ignition 9.74%.
[0046] In step ①, the drying is performed at 107° C. for 5.3 h.
[0047] In step ②, the mass ratio of the mixture of red mud raw material and carbon nanotubes to distilled water is 1:3.3.
[0048] In step ②, the mass of KH550 silane coupling agent accounts for 5.8% of the mass of the mixture of red mud raw material and carbon nanotubes.
[0049] During the ball milling modification in step ②, the rotation speed of the ball mill is 550 r / min, and the ball milling time is 3.1 h.
[0050] The method for preparing the rubber powder modified asphalt described in this embodiment 1 comprises the following steps:
[0051] (1) Melting petroleum asphalt at 164°C, adding rubber powder to the petroleum asphalt and stirring evenly, then adding a mixture of modified red mud and carbon nanotubes, dodecylbenzene sulfonic acid and stabilizer, keeping the mixture at 183°C for 33 minutes, and then shearing;
[0052] (2) After the shearing is completed, swelling is carried out to prepare rubber powder modified asphalt.
[0053] in:
[0054] In step (1), the shearing speed is 6000 r / min and the shearing time is 45 min.
[0055] In step (2), the swelling temperature is 183° C. and the swelling time is 73 min.
[0056] Example 2
[0057] The rubber powder modified asphalt described in this Example 2 is composed of the following raw materials, in parts by weight: 100 parts of petroleum asphalt, 23 parts of rubber powder, 8 parts of a mixture of modified red mud and carbon nanotubes, 3.3 parts of dodecylbenzene sulfonic acid and 5 parts of a stabilizer, wherein the stabilizer is a mixture of bio-oil, oxidized polyethylene wax and cycloalkane oil.
[0058] in:
[0059] The mass ratio of bio-oil, oxidized polyethylene wax and cycloalkane oil in the stabilizer is 1.4:2.1:0.8.
[0060] Rubber powder is prepared by crushing waste tires, and the particle size is 0.212mm.
[0061] The bio-oil is castor oil, and the manufacturer is Guyun Chemical (Changzhou) Co., Ltd.
[0062] The cycloparaffin oil is NAP1004, and the manufacturer is Karamay Petrochemical Company.
[0063] The preparation method of the mixture of modified red mud and carbon nanotubes consists of the following steps:
[0064] ① Add sintered red mud into water, then add dilute sulfuric acid to adjust the pH value of the system to 10.5, sieve with a 60-mesh sieve, take the sieve and dry it to prepare the red mud raw material;
[0065] ② The red mud raw material and carbon nanotubes prepared in step ① are placed in a ball mill, and distilled water and KH550 silane coupling agent are added for ball milling modification to prepare a mixture of modified red mud and carbon nanotubes.
[0066] in:
[0067] The chemical composition of the sintered red mud in step ① is as follows in terms of mass percentage: Fe 2 O 3 11.05%, Al 2 O 3 7.59%, SiO 2 21.78%, CaO 41.59%, Na 2 O 3.01%, TiO 2 3.24%, K 2O 0.35%, MgO 1.65%, loss on ignition 9.74%.
[0068] In step ①, the drying is performed at 110° C. for 5.5 h.
[0069] In step ②, the mass ratio of the mixture of red mud raw material and carbon nanotubes to distilled water is 1:3.5.
[0070] In step ②, the mass of KH550 silane coupling agent accounts for 6.0% of the mass of the mixture of red mud raw material and carbon nanotubes.
[0071] During the ball milling modification in step ②, the rotation speed of the ball mill is 600 r / min, and the ball milling time is 3.2 h.
[0072] The method for preparing the rubber powder modified asphalt described in this embodiment 2 is composed of the following steps:
[0073] (1) Melting petroleum asphalt at 163°C, adding rubber powder to the petroleum asphalt and stirring evenly, then adding a mixture of modified red mud and carbon nanotubes, dodecylbenzene sulfonic acid and stabilizer, keeping the mixture at 185°C for 30 minutes, and then shearing;
[0074] (2) After the shearing is completed, swelling is carried out to prepare rubber powder modified asphalt.
[0075] in:
[0076] In step (1), the shearing speed is 5000 r / min and the shearing time is 40 min.
[0077] In step (2), the swelling temperature is 185° C. and the swelling time is 75 min.
[0078] Example 3
[0079] The rubber powder modified asphalt described in this Example 3 is composed of the following raw materials, in parts by weight: 100 parts of petroleum asphalt, 25 parts of rubber powder, 6 parts of a mixture of modified red mud and carbon nanotubes, 4.7 parts of dodecylbenzene sulfonic acid and 7 parts of a stabilizer, wherein the stabilizer is a mixture of bio-oil, oxidized polyethylene wax and cycloalkane oil.
[0080] in:
[0081] The mass ratio of bio-oil, oxidized polyethylene wax and cycloalkane oil in the stabilizer is 1.2:2.3:1.0.
[0082] Rubber powder is prepared by crushing waste tires, and the particle size is 0.300mm.
[0083] The bio-oil is castor oil, and the manufacturer is Guyun Chemical (Changzhou) Co., Ltd.
[0084] The cycloparaffin oil is NAP1004, and the manufacturer is Karamay Petrochemical Company.
[0085] The preparation method of the mixture of modified red mud and carbon nanotubes consists of the following steps:
[0086] ① Add sintered red mud into water, then add dilute sulfuric acid to adjust the pH value of the system to 10.5, sieve with a 60-mesh sieve, take the sieve and dry it to prepare the red mud raw material;
[0087] ② The red mud raw material and carbon nanotubes prepared in step ① are placed in a ball mill, and distilled water and KH550 silane coupling agent are added for ball milling modification to prepare a mixture of modified red mud and carbon nanotubes.
[0088] in:
[0089] The chemical composition of the sintered red mud in step ① is as follows in terms of mass percentage: Fe 2 O 3 11.05%, Al 2 O 3 7.59%, SiO 2 21.78%, CaO 41.59%, Na 2 O 3.01%, TiO 2 3.24%, K 2 O 0.35%, MgO 1.65%, loss on ignition 9.74%.
[0090] The drying in step ① is performed at 105° C. for 5 h.
[0091] In step ②, the mass ratio of the mixture of red mud raw material and carbon nanotubes to distilled water is 1:3.
[0092] In step ②, the mass of KH550 silane coupling agent accounts for 5.5% of the mass of the mixture of red mud raw material and carbon nanotubes.
[0093] During the ball milling modification in step ②, the rotation speed of the ball mill is 500 r / min, and the ball milling time is 3 h.
[0094] The method for preparing the rubber powder modified asphalt described in this embodiment 3 is composed of the following steps:
[0095] (1) Melting petroleum asphalt at 165°C, adding rubber powder to the petroleum asphalt and stirring evenly, then adding a mixture of modified red mud and carbon nanotubes, dodecylbenzene sulfonic acid and stabilizer, keeping the mixture at 180°C for 35 minutes, and then shearing;
[0096] (2) After the shearing is completed, swelling is carried out to prepare rubber powder modified asphalt.
[0097] in:
[0098] In step (1), the shearing speed is 7000 r / min and the shearing time is 50 min.
[0099] In step (2), the swelling temperature is 180° C. and the swelling time is 70 min.
[0100] Comparative Example 1
[0101] The preparation method of the rubber powder modified asphalt described in this comparative example 1 is the same as that of Example 1, the only difference being that the mixture of modified red mud and carbon nanotubes is no longer added to the raw materials.
[0102] Comparative Example 2
[0103] The preparation method of the rubber powder modified asphalt described in this comparative example 2 is the same as that of Example 1, the only difference being that dodecylbenzene sulfonic acid is no longer added to the raw materials.
[0104] Comparative Example 3
[0105] The preparation method of the rubber powder modified asphalt described in this comparative example 3 is the same as that of Example 1, the only difference being that no stabilizer is added to the raw materials.
[0106] The performance tests were performed on the rubber powder modified asphalt prepared in Examples 1-3 and Comparative Examples 1-3. The results are shown in Table 1 below:
[0107] Table 1 Performance test results of rubber powder modified asphalt prepared in Examples 1-3 and Comparative Examples 1-3
[0108]
[0109] As shown in Table 1, the performance of the rubber powder modified asphalt prepared in Examples 1-3 is much better than that of Comparative Examples 1-3. The raw materials of Comparative Example 1 no longer add the mixture of modified red mud and carbon nanotubes, the raw materials of Comparative Example 2 no longer add dodecylbenzene sulfonic acid, and the raw materials of Comparative Example 3 no longer add stabilizers, which all lead to an increase in the needle penetration of the prepared rubber powder modified asphalt (an increase in needle penetration means that the high temperature performance of the rubber powder modified asphalt deteriorates), a decrease in 5°C ductility (a decrease in ductility means that the plasticity of the rubber powder modified asphalt decreases), an increase in the separation softening point difference (an increase in the separation softening point difference means that the stability of the rubber powder modified asphalt deteriorates), and a decrease in 25°C elastic recovery. It can be seen that the mixture of modified red mud and carbon nanotubes, dodecylbenzene sulfonic acid, and stabilizer in the raw materials used in the rubber powder modified asphalt have a synergistic effect.
Claims
1. A rubber powder modified asphalt, characterized in that: The method comprises the following raw materials in parts by weight: 100 parts of petroleum asphalt, 23-25 parts of rubber powder, 6-8 parts of a mixture of modified red mud and carbon nanotubes, 3.3-4.7 parts of dodecylbenzene sulfonic acid and 5-7 parts of a stabilizer, wherein the stabilizer is a mixture of bio-oil, oxidized polyethylene wax and cycloparaffin oil, and the bio-oil is castor oil. The method for preparing the mixture of modified red mud and carbon nanotubes comprises the following steps: ① Add sintered red mud into water, then add dilute sulfuric acid to adjust the pH value of the system to 10.5, sieve with a 60-mesh sieve, take the sieve and dry it to prepare the red mud raw material; ② The red mud raw material and carbon nanotubes prepared in step ① are placed in a ball mill, and distilled water and KH550 silane coupling agent are added for ball milling modification to prepare a mixture of modified red mud and carbon nanotubes.
2. The rubber powder modified asphalt according to claim 1, characterized in that: The invention is composed of the following raw materials in parts by weight: 100 parts of petroleum asphalt, 24 parts of rubber powder, 7 parts of a mixture of modified red mud and carbon nanotubes, 4 parts of dodecylbenzene sulfonic acid and 6 parts of a stabilizer, wherein the stabilizer is a mixture of bio-oil, oxidized polyethylene wax and cycloalkane oil.
3. The rubber powder modified asphalt according to claim 1, characterized in that: The mass ratio of the bio-oil, the oxidized polyethylene wax and the cycloalkane oil in the stabilizer is 1.2-1.4: 2.1-2.3: 0.8-1.
0.
4. The rubber powder modified asphalt according to claim 1, characterized in that: Rubber powder is prepared by crushing waste tires, and the particle size is 0.212-0.300mm.
5. The rubber powder modified asphalt according to claim 1, characterized in that: The cycloparaffin oil was NAP1004.
6. The rubber powder modified asphalt according to claim 1, characterized in that: In step ①, the chemical composition of the sintered red mud is as follows, in terms of mass percentage: Fe2O3 11.05%, Al2O3 7.59%, SiO2 21.78%, CaO 41.59%, Na2O3.01%, TiO2 3.24%, K2O 0.35%, MgO 1.65%, and loss on ignition 9.74%; In step ①, the drying is performed at 105-110° C. for 5-5.5 hours.
7. The rubber powder modified asphalt according to claim 1, characterized in that: In step ②, the mass ratio of the mixture of red mud raw material and carbon nanotubes to distilled water is 1:3-3.5; In step ②, the mass of KH550 silane coupling agent accounts for 5.5-6.0% of the mass of the mixture of red mud raw material and carbon nanotubes; During the ball milling modification in step ②, the rotation speed of the ball mill is 500-600 r / min, and the ball milling time is 3-3.2 h.
8. A method for preparing rubber powder modified asphalt according to claim 1, characterized in that: It consists of the following steps: (1) Melting petroleum asphalt at 163-165°C, adding rubber powder to the petroleum asphalt and stirring evenly, then adding a mixture of modified red mud and carbon nanotubes, dodecylbenzene sulfonic acid and a stabilizer, keeping the mixture at 180-185°C for 30-35 minutes, and then shearing; (2) After the shearing is completed, swelling is carried out to prepare rubber powder modified asphalt.
9. The method for preparing rubber powder modified asphalt according to claim 8, characterized in that: In step (1), the shearing speed is 5000-7000 r / min, and the shearing time is 40-50 min; In step (2), the swelling temperature is 180-185° C. and the swelling time is 70-75 min.
Citation Information
Patent Citations
Rubber powder modified asphalt and preparation method thereof
CN111393863A
Polymer-based carbon nanotube master batch and rubber powder modified asphalt and preparation method thereof
CN115109424A