A regenerated asphalt sand and its design method and carbon emission accounting method

By calculating the blending ratio and asphalt film thickness of old asphalt mixture, tailings sand and rock asphalt, the asphalt consumption is accurately determined, and the problems of high carbon emissions and high performance variability in asphalt sand design in the existing technology are solved, and regeneration is achieved The high stability performance and low carbon emissions of asphalt sand ensure the crack resistance of the pavement and the environmentally friendly utilization of resources.

CN118692610BActive Publication Date: 2024-11-26ANHUI TRANSPORT CONSULTING & DESIGN INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411156959.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-26
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The existing asphalt sand fails to effectively consider the adsorption effect of aggregates of different particle sizes on asphalt during material design, resulting in high carbon emissions and large performance variability, making it difficult to ensure the durability and environmental protection of the road surface.

Method used

By calculating the blending ratio of old asphalt mixture, tailings sand and rock asphalt, combined with Marshall test and asphalt film thickness calculation, the asphalt usage is accurately determined, the optimal asphalt film formation state is formed, the durability of regenerated asphalt sand is improved, and the durability of regenerated asphalt sand is provided. Carbon emission accounting methods to reduce carbon emissions.

Benefits of technology

The high stability performance and low carbon emissions of recycled asphalt sand are achieved, the waste of blindly adding asphalt is avoided, and the road surface crack resistance and environmentally friendly utilization of resources are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure QLYQS_3
    Figure QLYQS_3
Patent Text Reader

Abstract

The present invention belongs to the technical field of road engineering, in particular to a regenerated asphalt sand and its design method and its carbon emission accounting method. The design method of the regenerated asphalt sand of the present invention has the following steps: S1, calculating the blending ratio of old asphalt mixture, tailings sand, rock asphalt and SBS modified asphalt; S2, confirming the thickness of the asphalt film, dividing and numbering the aggregates with a particle size of 4.75 mm or less according to the size of the sieve hole, and then calculating the amount of asphalt wrapped in the i-th grade old aggregate, the amount of asphalt wrapped in the i-th grade tailings sand, and the amount of asphalt wrapped in the i-th grade ash according to the thickness of the asphalt film; S3, combining step S1 and step S2 to obtain the final amount ratio of each raw material of the regenerated asphalt sand. The present invention calculates the optimal asphalt dosage of the regenerated asphalt sand according to the asphalt film-forming characteristics, and considers the difference in the film thickness of the asphalt on the surface of aggregates with different particle sizes, so as to accurately determine the asphalt dosage and give full play to the best effect of asphalt, which can not only save costs, but also have a good emission reduction effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of road engineering, and in particular relates to a regenerated asphalt sand and a design method thereof and a carbon emission accounting method thereof. Background Art

[0002] During the long-term use of asphalt pavement, it is inevitable that there will be varying degrees of damage such as rutting, cracks, potholes, looseness, etc., among which pavement cracking accounts for more than 60% of all damage, which is mainly due to reflective cracks in the semi-rigid base layer and fatigue cracking caused by insufficient fatigue resistance of the pavement material. Once the pavement cracks, rainwater intrusion accelerates its destruction, causing more serious damage, seriously affecting the service level of the pavement, and shortening its expected service life.

[0003] Pavement maintenance and renovation and expansion will generate a large amount of waste materials, and industrial production will also generate a large amount of tailings sand. These solid wastes accumulate and occupy land, pollute the environment, and need to be dealt with urgently. Pavement recycling technology is to process waste pavement materials and industrial solid waste into materials that meet the requirements of pavement use through certain technical means, and pave them on the pavement to achieve better results. It is an important measure to solve the problem of pavement waste materials and tailings sand storage.

[0004] Asphalt sand has a high oil content, and its asphalt content is basically more than 7%. The mixture particles are fine, and the interface connection between the particles is relatively uniform. The structural asphalt film forms a large bonding force and interface energy, which can resist large shear stress and tensile stress. Its fatigue life is more than 100 times that of ordinary asphalt mixtures, which can improve the durability of road use. Regenerated asphalt sand is prepared from road waste materials and tailings sand, and paved on the road surface. The flexibility and large deformation absorption capacity of asphalt sand are used to improve the crack resistance of the road surface, and it can also solve the problem of solid waste accumulation polluting the environment and occupying land.

[0005] When designing materials for conventional asphalt sand, the determination of the oil-stone ratio and grading is completely dependent on the Marshall test, and the effect of asphalt coating on aggregates of different particle sizes is not considered. In order to ensure good deformation capacity and higher fatigue life, too much asphalt is added, and the amount of free asphalt after coating is large, resulting in a large waste. The carbon emissions during the asphalt processing are high, and it is difficult to obtain a good emission reduction effect. At the same time, the design results are mostly dependent on the final void ratio, and it is difficult to ensure that the performance is in the best state. The performance variability is large, which affects the durability of the mixture.

[0006] Therefore, there is an urgent need for a regenerated asphalt sand and its design method and its carbon emission accounting method to solve the above problems. Summary of the invention

[0007] In order to overcome the defects in the above-mentioned prior art, the present invention provides a regenerated asphalt sand and its design method and its carbon emission accounting method. The present invention strengthens the parameter control in the volume filling process of the regenerated asphalt sand, and considers the asphalt adsorption effect of aggregates with different particle sizes, so that the asphalt is in the best film-forming state, and improves the durability of the regenerated asphalt sand.

[0008] To achieve one of the above purposes, the present invention adopts the following technical solution:

[0009] A design method for regenerating asphalt sand, the method steps are as follows:

[0010] S1. Calculate the blending ratio of old asphalt mixture, tailings sand, rock asphalt and SBS modified asphalt. The calculation formula is:

[0011] ;

[0012] ;

[0013] ;

[0014] In the formula: G represents the content of old asphalt mixture, the unit is %; g represents the content of rock asphalt, the unit is %; Indicates the content of tailings sand, unit is %; Indicates the content of SBS modified asphalt, unit is %; Indicates the compaction density of old asphalt mixture, in g / cm 3 ; VCA represents the skeleton void ratio of the old asphalt mixture constituting the skeleton voids, the unit is %; VMA represents the mineral void ratio of the mineral voids formed after the tailings sand and rock asphalt are filled in the skeleton voids, the unit is %; VV represents the void ratio of the regenerated asphalt sand, the unit is %; Indicates the density of rock asphalt in g / cm 3 ; Indicates the density of tailings sand in g / cm 3 ; Indicates the density of SBS modified asphalt in g / cm 3 ;

[0015] S2. Confirm the thickness of the asphalt film, and classify and number the aggregates with a particle size of 4.75 mm or less according to the size of the sieve hole. Then calculate the amount of asphalt wrapped in the i-th grade of old aggregate, the amount of asphalt wrapped in the i-th grade of tailings sand, and the amount of asphalt wrapped in the i-th grade of ash according to the thickness of the asphalt film. The calculation formula is as follows:

[0016] ;

[0017] ;

[0018] ;

[0019] G;

[0020] Where: P G It indicates the amount of asphalt wrapped in old aggregate, in units of %; P f It indicates the amount of asphalt attached to the tailings sand, in units of %; P g It indicates the amount of asphalt wrapped by ash in rock asphalt, the unit is %;d Gi It indicates the passing rate of old aggregate in the i-th size sieve, in units of %; d fi It indicates the passing rate of tailings sand in the i-th size sieve, in units of %; d gi It indicates the ash content passing rate at the sieve size of the i-th grade, in units of %; P ag Indicates the amount of asphalt in rock asphalt, unit is %; SAJ i Indicates the specific surface area coefficient corresponding to the i-th size sieve hole, in m 2 / kg; P aG It indicates the amount of old asphalt in the old asphalt mixture, in units of %; It indicates the asphalt film thickness corresponding to the aggregate with a sieve size of 4.75 mm, in μm; Indicates the thickness of the asphalt film wrapped around the i-th aggregate 3 ;

[0021] S3. Combining step S1 and step S2, the final usage ratio of each raw material of the regenerated asphalt sand is obtained.

[0022] Preferably, the calculation method of the skeleton void fraction VCA of the skeleton voids formed by the old asphalt mixture is as follows:

[0023] The old asphalt mixture was heated to 120°C and compacted 75 times on both sides by the Marshall test method to measure its compaction density and calculate its skeleton void fraction VCA. The calculation formula is:

[0024] ×100%;

[0025] Where: Indicates the density of old asphalt mixture in g / m 3 ; Indicates the compaction density of old asphalt mixture, in g / cm 3 .

[0026] Preferably, the specific steps of the method for confirming the thickness of the asphalt film are as follows:

[0027] (1) Take the aggregate of the i-th mesh size and immerse it in water. After soaking for 24 hours, filter it and the mass of the aggregate shall be ≥100g;

[0028] (2) Pour the filtered aggregate into an iron cup, place absorbent paper at the bottom of the cup and filter paper at the top, and place it in a centrifuge and rotate for 2-3 minutes;

[0029] (3) Weigh the total mass m of the aggregate with the i-th sieve size after rotation i1 ;

[0030] (4) Place the aggregate of the i-th mesh size into an oven for drying, and then weigh its total mass m i2 ;

[0031] (5) Water film thickness of aggregate with the i-th mesh size The calculation formula is as follows:

[0032] ;

[0033] Where: m i1 It represents the total mass of the aggregate of the i-th sieve size after centrifugal rotation, in g; m i2 It represents the drying mass of aggregate with the sieve size of the i-th gear, in g; SA i Represents the specific surface area of ​​aggregate with the sieve size of the i-th grade, in m 2 / kg;h i It represents the water film thickness of the aggregate with the sieve size of the i-th gear, in μm; ρ represents the density of water, in g / cm 3 ;

[0034] (6) The calculation formula for the asphalt film thickness of aggregates with a sieve size of 4.75 mm or less is as follows:

[0035] ;

[0036] Where: It represents the thickness of asphalt film wrapped around aggregate of the sieve size of the i-th gear, in μm; It represents the average asphalt film thickness of regenerated asphalt sand, in μm; h i It represents the water film thickness of aggregate with the sieve size of the i-th grade, in μm.

[0037] Preferably, aggregates with a sieve size of 4.75 mm or less are divided into 8 grades according to the sieve size, namely 4.75 mm, 2.36 mm, 1.18 mm, 0.6 mm, 0.3 mm, 0.15 mm, 0.075 mm and less than 0.075 mm.

[0038] Preferably, the porosity VV of the regenerated asphalt sand is 1-2.5%.

[0039] Preferably, the average asphalt film thickness of the regenerated asphalt sand is It is 15-18um.

[0040] Preferably, the mineral gap ratio VMA formed by filling the gaps in the skeleton with tailings sand and rock asphalt is 9-13%.

[0041] To achieve the second purpose above, the present invention provides a regenerated asphalt sand, which includes an old asphalt mixture forming a skeleton structure, the skeleton gaps of the old asphalt mixture are filled with tailings sand and rock asphalt to form mineral gaps; the mineral gaps are filled with SBS modified asphalt; the particle size of the old asphalt mixture is 3-5mm, the old asphalt mixture is composed of old aggregate and old asphalt; the rock asphalt is composed of asphalt and ash, the old asphalt, asphalt and SBS modified asphalt are mixed and fused to form a fused material, and the fused material forms an asphalt film on the surface of the old aggregate, the surface of the tailings sand and the surface of the ash.

[0042] Preferably, the tailings sand is fine-grained tailings sand with a particle size of ≤2.36 mm, wherein the pass rate of a 0.075 mm sieve hole is greater than 50%; the proportion of asphalt in rock asphalt is 25-40%, and the proportion of old asphalt in old asphalt mixture is 2-6%.

[0043] To achieve the third purpose above, the present invention provides a method for calculating carbon emissions from regenerated asphalt sands. The calculation formula for carbon emissions from 1 ton of regenerated asphalt sands is as follows:

[0044] ;

[0045] Where: C represents the carbon emission of 1 ton of recycled asphalt sand, in kgCO2; G represents the content of old asphalt mixture, in %; It represents the carbon emission factor of old asphalt mixture, in kgCO2; Indicates the content of tailings sand, unit is %; represents the carbon emission factor of tailings sand, the unit is kgCO2; g represents the content of rock asphalt, the unit is %; represents the carbon emission factor of rock asphalt, in kgCO2; Indicates the content of SBS modified asphalt, unit is %; Indicates the carbon emission factor of SBS modified asphalt, in kgCO 2。

[0046] The advantages of the present invention are:

[0047] (1) The present invention transfers asphalt in rock asphalt, SBS modified asphalt and old asphalt to each other, and finally wraps them on the surface of old aggregate, the surface of rock asphalt ash and the surface of tailings sand. According to the film-forming characteristics of asphalt, the optimal asphalt dosage of regenerated asphalt sand mixed with tailings sand is calculated, and the difference in film thickness of asphalt on the surface of aggregates with different particle sizes is taken into consideration, so as to accurately determine the asphalt dosage and exert the best effect of asphalt, thereby avoiding blind addition of asphalt, which affects the quality and cost of regenerated asphalt sand.

[0048] (2) The present invention combines the composition mechanism of the mixture, controls the quality of the regenerated asphalt sand according to the changes in volume parameters of the old asphalt mixture, rock asphalt, tailings sand, and SBS modified asphalt during the space filling process, considers the influence of the components in the old asphalt mixture and rock asphalt on the filling effect, and provides a theoretical calculation method for the composition ratio of raw materials to ensure that the regenerated asphalt sand has highly stable performance.

[0049] (3) The present invention uses industrial waste tailings and old asphalt mixtures discarded from roads as raw materials for asphalt sands, and provides a carbon emission accounting method for the asphalt sands, making full use of rock asphalt and asphalt in old asphalt mixtures to maximize their value, and accurately controlling the amount of new asphalt added, thereby effectively reducing carbon emissions during the use of asphalt sands, and realizing waste resource utilization, resource conservation, and high efficiency and environmental protection. DETAILED DESCRIPTION

[0050] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in combination with embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.

[0051] Example 1

[0052] A regenerated asphalt sand comprises fine-grained tailings sand, SBS modified asphalt, rock asphalt and old asphalt mixture with a particle size of 3-5 mm. The old asphalt mixture with a particle size of 3-5 mm consists of two parts: old aggregate and old asphalt, and the rock asphalt consists of two parts: asphalt and ash. The rock asphalt and the old asphalt mixture are extracted, and the asphalt content in the rock asphalt is measured to be 30%, and the old asphalt content in the old asphalt mixture is measured to be 4.0%.

[0053] A design method for regenerating asphalt sand, the specific steps are as follows:

[0054] S1. Screening of tailings sand, ash in rock asphalt, and old aggregate in old asphalt mixture, the results are shown in Table 1-2 below:

[0055] Table 1 Raw material screening results

[0056] ;

[0057] Table 2 Density of raw materials

[0058] ;

[0059] S2. The old asphalt mixture was heated to 120°C and compacted 75 times on both sides using the Marshall test method. The compacted density was determined to be 1.92 g / cm 3 , and calculate its skeleton void fraction VCA as:

[0060] = 28.9%;

[0061] Tailings sand and rock asphalt are filled in the gaps of the skeleton, and the gaps formed are the gaps between the mineral materials. The gap ratio VMA of the mineral materials is 9%. SBS modified asphalt is filled in the gaps between the mineral materials. The remaining gaps after filling are the gaps between the regenerated asphalt sands. The gap ratio VV of the regenerated asphalt sands is 1%. The blending ratios of tailings sand, SBS modified asphalt, rock asphalt and old asphalt mixture are calculated according to the following formulas:

[0062] ;

[0063] ;

[0064] ;

[0065] S3. The thickness of the asphalt film on the aggregate surface of each mesh size is determined as follows:

[0066] (1) Take the residual aggregates with sieve sizes of 4.75 mm, 2.36 mm, 1.18 mm, 0.6 mm, 0.3 mm, 0.15 mm, 0.075 mm and <0.075 mm. The aggregate masses are shown in Table 3 below. Soak in water for 24 hours and then filter.

[0067] Table 3 Aggregate quality

[0068] ;

[0069] (2) Pour the aggregates after soaking and filtering with different mesh sizes into an iron cup, pad the bottom of the iron cup with absorbent paper, separate the top with filter paper, and put it into a centrifuge for rotation for 2-3 minutes;

[0070] (3) The total mass of aggregates of each mesh size after rotation is weighed as shown in Table 4 below;

[0071] Table 4 Total mass of aggregate after centrifugal rotation

[0072] ;

[0073] (4) After the aggregates of various mesh sizes are placed in an oven for drying, their total mass is weighed as shown in Table 5 below;

[0074] Table 5 Aggregate drying quality

[0075] ;

[0076] (5) Calculate the water film thickness of aggregates at each mesh size using the following formula , as shown in Table 6 below, the density of water is 1g / cm 3 ;

[0077] ;

[0078] Among them, SA i 0.41+0.0041a+0.0082b+0.0164c+0.0287d+0.0614e+0.1229x+0.3277y;

[0079] In the formula, SA i Indicates the specific surface area of ​​aggregate of the i-th sieve size, m 2 / kg; a, b, c, d, e, x, and y are the passing rates of each sieve hole below 4.75 mm.

[0080] Table 6 Calculation results of water film thickness on aggregate surface

[0081] ;

[0082] (6) Average asphalt film thickness of regenerated asphalt sand Take 15um and calculate the asphalt film thickness of aggregates of various mesh sizes according to the following formula: , the results are shown in Table 7 below:

[0083] ;

[0084] Table 7 Calculation results of asphalt film thickness on aggregate surface

[0085] ;

[0086] S4, the amount of asphalt wrapped in old aggregate, tailings sand, and rock asphalt ash is calculated according to the following formula, and the specific surface area coefficient is taken according to the standard method, as shown in Table 8 below:

[0087] =0.0386G;

[0088] =0.306f;

[0089] =0.279g;

[0090] ;

[0091] Table 8 Surface area coefficient of tailings sand, ash and old aggregate

[0092] ;

[0093] Combining all the above formulas, it is calculated that the proportion of tailings sand in recycled asphalt sand is 12.4%, the proportion of SBS modified asphalt is 3.54%, the proportion of rock asphalt is 6.63%, and the proportion of old asphalt mixture is 80.97%.

[0094] A carbon emission accounting method for regenerated asphalt sands is as follows:

[0095] Calculate the carbon emission of 1 ton of recycled asphalt sand mixed with tailings and the carbon emission factor of old asphalt mixture Take 1.09kgCO2 / t, the carbon emission factor of tailings sand Taking 1.25kgCO2 / t, the carbon emission factor of SBS modified asphalt is Take 295.91kgCO2 / t, the carbon emission factor of rock asphalt Take 2.51kgCO2 / t and calculate according to the following formula:

[0096] =11.67kgCO2;

[0097] The road performance verification was carried out, and the performance results of the recycled asphalt sand are shown in Table 9 below:

[0098] Table 9 Road performance of recycled asphalt sand mixed with tailings sand

[0099] ;

[0100] It can be seen from Table 9 that the regenerated asphalt sand designed in Example 1 meets the requirements of the rutting test, satisfies the freeze-thaw splitting test, and has excellent bending failure strain performance.

[0101] Example 2

[0102] A regenerated asphalt sand comprises fine-grained tailings sand, SBS modified asphalt, rock asphalt, and old asphalt mixture with a particle size of 3-5 mm. The old asphalt mixture consists of two parts: old aggregate and old asphalt, and the rock asphalt consists of two parts: asphalt and ash. The rock asphalt and the old asphalt mixture are extracted, and the asphalt content in the rock asphalt is measured to be 30%, and the asphalt content in the old asphalt mixture is measured to be 4.0%.

[0103] A design method for regenerating asphalt sand, the specific steps are as follows:

[0104] S1. Screening of tailings sand, ash in rock asphalt, and old aggregate in old asphalt mixture, the results are shown in Table 10-11 below:

[0105] Table 10 Raw material screening results

[0106] ;

[0107] Table 11 Density of raw materials

[0108] ;

[0109] S2. The old asphalt mixture was heated to 120°C and compacted 75 times on both sides using the Marshall test method. The compacted density was determined to be 1.92 g / cm 3 , and calculate its framework void fraction VCA:

[0110] = 28.9%;

[0111] Tailings sand and rock asphalt are filled in VCA, and the gaps formed are the gaps between mineral materials. The gap ratio VMA of the mineral materials is 13%. SBS modified asphalt is filled in the gaps between mineral materials. The remaining gaps after filling are the gaps of regenerated asphalt sand. The gap ratio VV of regenerated asphalt sand is 2.5%. The blending ratio of tailings sand, SBS modified asphalt, rock asphalt and old asphalt mixture is calculated according to the following formula:

[0112] ;

[0113] ;

[0114] ;

[0115] S3. The thickness of the asphalt film on the aggregate surface of each mesh size is determined as follows:

[0116] (1) Take the aggregates with sieve hole sizes of 0.075mm, 0.15mm, 0.3mm, 0.6mm, 1.18mm, 2.36mm, 4.75mm and <0.075mm. The aggregate masses are shown in Table 12 below. Soak in water for 24 hours and then filter;

[0117] Table 12 Aggregate quality

[0118] ;

[0119] (2) Pour the aggregates after soaking and filtering with different sieve hole sizes into an iron cup, pad the bottom of the iron cup with absorbent paper, separate the top with filter paper, and put it into a centrifuge for rotation for 2-3 minutes;

[0120] (3) Weigh the total mass of aggregates of each sieve size after rotation as shown in Table 13 below;

[0121] Table 13 Total mass of aggregate after centrifugal rotation

[0122] ;

[0123] (4) After the aggregates of various mesh sizes are placed in an oven for drying, their total mass is weighed as shown in the following table;

[0124] Table 14 Aggregate drying quality

[0125] ;

[0126] (5) Calculate the water film thickness of aggregates at each mesh size using the following formula As shown in Table 15 below, the density of water is 1 g / cm 3 ;

[0127] ;

[0128] Among them, SA i 0.41+0.0041a+0.0082b+0.0164c+0.0287d+0.0614e+0.1229x+0.3277y;

[0129] In the formula, SA i —Specific surface area of ​​aggregate with the sieve size of the i-th gear, m 2 / kg; a, b, c, d, e, x, and y are the passing rates of each sieve hole below 4.75 mm.

[0130] Table 15 Calculation results of water film thickness on aggregate surface

[0131] ;

[0132] (6) The average asphalt film thickness of regenerated asphalt sand is 18 μm, and the asphalt film thickness of aggregates of different mesh sizes is calculated. , the results are shown in Table 16 below:

[0133] ;

[0134] Table 16 Calculation results of asphalt film thickness on aggregate surface

[0135] ;

[0136] S4, the amount of asphalt used for wrapping old aggregate, tailings sand, and rock asphalt ash is calculated according to the following formula, and the specific surface area coefficient is taken according to the standard method, as shown in Table 17 below:

[0137] =0.0464G;

[0138] =0.368f;

[0139] =0.335g;

[0140] 0.04;

[0141] Table 17 Surface area coefficient of tailings sand, ash and old aggregate

[0142] ;

[0143] Combining all the above formulas, it is calculated that the proportion of fine-grained tailings sand in the recycled asphalt sand is 11.3%, the proportion of SBS modified asphalt is 4.8%, the proportion of rock asphalt is 5.0%, and the proportion of old asphalt mixture is 83.7%.

[0144] A method for calculating carbon emissions from recycled asphalt sands is as follows:

[0145] Calculate the carbon emission of 1 ton of recycled asphalt sand and the carbon emission factor of old asphalt mixture Take 1.09 kgCO2 / t, the carbon emission factor of tailings sand Taking 1.25kgCO2 / t, the carbon emission factor of SBS modified asphalt is Take 295.91kgCO2 / t, the carbon emission factor of rock asphalt Take 2.51kgCO2 / t and calculate according to the following formula:

[0146] =15.38kgCO2;

[0147] The road performance of the regenerated asphalt sand was verified, and the performance results of the regenerated asphalt sand are shown in Table 18:

[0148] Table 18 Road performance of recycled asphalt sand mixed with tailings sand

[0149] ;

[0150] It can be seen from Table 18 that the regenerated asphalt sand designed in Example 2 meets the requirements of the rutting test, satisfies the freeze-thaw splitting test, and has excellent bending failure strain performance.

[0151] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A design method for regenerating asphalt sand, characterized in that: The method is as follows: S1. Calculate the blending ratio of old asphalt mixture, tailings sand, rock asphalt and SBS modified asphalt. The calculation formula is: ; ; ; In the formula: G represents the content of old asphalt mixture, the unit is %; g represents the content of rock asphalt, the unit is %; Indicates the content of tailings sand, unit is %; Indicates the content of SBS modified asphalt, unit is %; Indicates the compaction density of old asphalt mixture, in g / cm 3 ; VCA represents the skeleton void ratio of the old asphalt mixture constituting the skeleton voids, the unit is %; VMA represents the mineral void ratio of the mineral voids formed after the tailings sand and rock asphalt are filled in the skeleton voids, the unit is %; VV represents the void ratio of the regenerated asphalt sand, the unit is %; Indicates the density of rock asphalt in g / cm 3 ; Indicates the density of tailings sand in g / cm 3 ; Indicates the density of SBS modified asphalt in g / cm 3 ; S2. Confirm the thickness of the asphalt film, and classify and number the aggregates with a particle size of 4.75 mm or less according to the size of the sieve hole. Then calculate the amount of asphalt wrapped in the i-th grade of old aggregate, the amount of asphalt wrapped in the i-th grade of tailings sand, and the amount of asphalt wrapped in the i-th grade of ash according to the thickness of the asphalt film. The calculation formula is as follows: ; ; ; G; Where: P G It indicates the amount of asphalt wrapped in old aggregate, in units of %; P f It indicates the amount of asphalt attached to the tailings sand, in units of %; P g It indicates the amount of asphalt wrapped in ash in rock asphalt, in %; d Gi It indicates the passing rate of old aggregate in the i-th size sieve, in units of %; d fi It indicates the passing rate of tailings sand at the i-th size sieve, in units of %; d gi It indicates the ash content passing rate at the sieve size of the i-th grade, in units of %; P ag Indicates the amount of asphalt in rock asphalt, unit is %; SAJ i Indicates the specific surface area coefficient corresponding to the i-th size sieve hole, in m 2 / kg; P aG It indicates the amount of old asphalt in the old asphalt mixture, in units of %; It indicates the asphalt film thickness corresponding to the aggregate with a sieve size of 4.75 mm, in μm; It represents the thickness of asphalt film wrapped around the i-th aggregate; S3, combining step S1 and step S2 to obtain the final usage ratio of each raw material of the regenerated asphalt sand; The specific steps of the method for confirming the thickness of the asphalt film are as follows: (1) Take the aggregate of the i-th mesh size and immerse it in water. After soaking for 24 hours, filter it and the mass of the aggregate shall be ≥100g; (2) Pour the filtered aggregate into an iron cup, place absorbent paper at the bottom of the cup and filter paper at the top, and place it in a centrifuge and rotate for 2-3 minutes; (3) Weigh the total mass m of the aggregate with the i-th sieve size after rotation i1 ; (4) Place the aggregate of the i-th mesh size into an oven for drying, and then weigh its total mass m i2 ; (5) Water film thickness of aggregate with the i-th mesh size The calculation formula is as follows: ; Where: m i1 It represents the total mass of the aggregate of the i-th sieve size after centrifugal rotation, in g; m i2 It represents the drying mass of aggregate with the sieve size of the i-th gear, in g; SA i Represents the specific surface area of ​​aggregate with the sieve size of the i-th grade, in m 2 / kg;h i It represents the water film thickness of the aggregate with the sieve size of the i-th gear, in μm; ρ represents the density of water, in g / cm 3 ; (6) The calculation formula for the asphalt film thickness of aggregates with a sieve size of 4.75 mm or less is as follows: ; Where: It represents the thickness of asphalt film wrapped around aggregate of the sieve size of the i-th gear, in μm; It represents the average asphalt film thickness of reclaimed asphalt sand, in μm.

2. The design method of regenerated asphalt sand according to claim 1, characterized in that: The calculation method of the skeleton void fraction VCA of the skeleton voids of the old asphalt mixture is as follows: The old asphalt mixture was heated to 120°C and compacted 75 times on both sides by the Marshall test method to measure its compaction density and calculate its skeleton void fraction VCA. The calculation formula is: ×100%; Where: Indicates the density of old asphalt mixture in g / m 3 ; Indicates the compaction density of old asphalt mixture, in g / cm 3 .

3. The design method of regenerated asphalt sand according to claim 1, characterized in that: Aggregates with sieve sizes of 4.75mm and below are divided into 8 grades according to the sieve size, namely 4.75mm, 2.36mm, 1.18mm, 0.6mm, 0.3mm, 0.15mm, 0.075mm and less than 0.075mm.

4. The design method of regenerated asphalt sand according to claim 1, characterized in that: The porosity VV of the regenerated asphalt sand is 1-2.5%.

5. The design method of regenerated asphalt sand according to claim 1, characterized in that: The average asphalt film thickness of the reclaimed asphalt sand It is 15-18um.

6. The design method of regenerated asphalt sand according to claim 1, characterized in that: The mineral gap ratio VMA of the mineral gap formed by filling the skeleton gap with the tailings sand and the rock asphalt is 9-13%.

7. A regenerated asphalt sand obtained by the design method according to any one of claims 1 to 6, characterized in that: The regenerated asphalt sand comprises an old asphalt mixture forming a skeleton structure, the skeleton gaps of the old asphalt mixture are filled with tailings sand and rock asphalt, and mineral gaps are formed; the mineral gaps are filled with SBS modified asphalt; the particle size of the old asphalt mixture is 3-5mm, the old asphalt mixture is composed of old aggregate and old asphalt; the rock asphalt is composed of asphalt and ash, the old asphalt, asphalt and SBS modified asphalt are mixed and fused to form a fused material, and the fused material forms an asphalt film on the surface of the old aggregate, the surface of the tailings sand and the surface of the ash.

8. The regenerated asphalt sand according to claim 7, characterized in that: The tailings sand is fine-grained tailings sand with a particle size of ≤2.36mm, wherein the pass rate of a 0.075mm sieve hole is greater than 50%; the proportion of asphalt in the rock asphalt is 25-40%, and the proportion of old asphalt in the old asphalt mixture is 2-6%.

9. A method for calculating carbon emissions from regenerated asphalt sands as claimed in claim 7, characterized in that: The calculation formula for carbon emissions from 1 ton of recycled asphalt sand is as follows: ; Where: C represents the carbon emission of 1 ton of recycled asphalt sand, in kgCO2; G represents the content of old asphalt mixture, in %; It represents the carbon emission factor of old asphalt mixture, in kgCO2; Indicates the content of tailings sand, unit is %; represents the carbon emission factor of tailings sand, the unit is kgCO2; g represents the content of rock asphalt, the unit is %; represents the carbon emission factor of rock asphalt, in kgCO2; Indicates the content of SBS modified asphalt, unit is %; Indicates the carbon emission factor of SBS modified asphalt, in kgCO 2。