A method for preparing conductive silicon-carbon negative electrode material

By using graphitic phase carbon nitride formed in situ as a thermal reducing agent and pore-forming agent, it solves the problems of high preparation cost and volume expansion of silicon-carbon negative electrode materials, improves the conductivity and anti-expansion performance, and realizes low-cost and efficient silicon-carbon anode materials. Preparation of carbon anode materials.

CN118702107BActive Publication Date: 2024-10-25TIANJIN VOCATIONAL INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411186917.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-10-25
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

Silicon-carbon negative electrode materials have high preparation costs and suffer from excessive volume expansion and poor conductivity during charging and discharging.

Method used

Using graphitic phase carbon nitride formed in situ as the thermal reducing agent of nano-silica and the pore-forming agent of carrier activated carbon, the g-C3N4-C composite material coated by the nano-indium tin oxide-silica composite conductive film is used in Thermal reduction at 560-800℃ forms conductive nano-silicon carbon negative electrode material.

Benefits of technology

The thermal reduction temperature is reduced, the cost of raw materials is reduced, and the conductivity and anti-expansion properties are improved without affecting the electrochemical properties of the material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for preparing a conductive silicon-carbon negative electrode material, wherein graphite phase carbon nitride formed in situ is used as a reducing agent for thermal reduction of nano silicon dioxide to nano silicon and a pore-forming agent for carrier activated carbon, and a g-C3N4-C composite material coated with an indium tin oxide-silicon dioxide composite conductive film is thermally reduced at 560-800°C to form a conductive nano silicon-carbon negative electrode material, wherein the indium tin oxide-doped silicon dioxide composite conductive film is formed by sintering its gel film at a high temperature of 550°C; and the g-C3N4-C composite material is formed by calcining a phenol formaldehyde-melamine formaldehyde copolymer coated with a composite conductive film at 400-550°C. In the present invention, the g-C3N4 reducing agent reduces the temperature of thermal reduction of nano silicon dioxide to nano silicon to 560-800°C, greatly reducing energy consumption; and at the same time, the defects of high preparation cost of silicon-carbon negative electrode materials, excessive volume expansion during charging, and poor conductivity are overcome, and the invention has industrial application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a conductive silicon-carbon negative electrode material, and belongs to the technical field of energy storage materials. Background Art

[0002] Lithium-ion batteries have the advantages of high operating voltage, high specific energy, and stable discharge, and are widely used in portable electronic devices, electric vehicles, aviation and other fields. As an important component of lithium-ion batteries, negative electrode materials have a very important impact on the cycle life, energy density and safety performance of lithium-ion batteries. The gram capacity of graphite negative electrode materials currently used in commercialization is close to its limit value, which cannot meet the requirements of high power density, high energy density and stable cycle performance of lithium-ion batteries. Therefore, the development of high specific capacity negative electrode materials has become an important direction of lithium-ion battery research.

[0003] Silicon and lithium can form alloys in various forms, with a theoretical lithium storage capacity of up to 4200mAh / g, a low lithium insertion potential, and abundant reserves in nature. It is the most promising negative electrode material for the next generation of lithium-ion batteries to replace graphite. However, silicon has the following defects as a negative electrode material: (1) The technical and economic efficiency of silicon negative electrode materials is not as good as that of traditional graphite negative electrode materials, which affects its industrial application; (2) During the charge and discharge process of silicon negative electrode materials, alloying and dealloying will cause a volume change of 3-4 times, which will cause the solid electrolyte film on the surface of the material to be continuously generated and broken, and continuously consume active lithium, resulting in a decrease in coulombic efficiency as the charge and discharge cycle proceeds; (3) The rupture and pulverization of silicon particles lead to separation between silicon particles and between silicon particles and current collectors, and then lose electrical contact, resulting in capacity decay and a sharp decline in cycle performance; (4) Silicon negative electrode materials also have the problem of poor electronic conductivity, which makes their rate performance poor, and conductive components need to be added to improve the conductivity of the negative electrode material.

[0004] Improving the economic efficiency of silicon anode material preparation and improving the performance of silicon anode material are also research hotspots. The silicon source for preparing pure silicon is generally silicon dioxide, fluorosilicate, halosilanes and their derivatives. In industry, industrial silicon is usually prepared from silicon dioxide, and further purification treatment is performed to obtain high-purity silicon.

[0005] The main methods for preparing pure silicon using silicon dioxide as a silicon source include metal thermal reduction, non-metal thermal reduction, hydrogen reduction, metal-non-metal coupled reduction, and molten salt electrolysis. However, there are still the following deficiencies: (1) Although the reaction temperature of the metal thermal reduction method of magnesium, calcium, aluminum, or zinc is lower than 500°C, the metal powder cost is high and the consumption is too large, resulting in poor economic benefits and making it difficult to promote and apply it industrially; (2) The temperature of carbon thermal reduction is above 1300°C, which is too high for the thermal reduction reaction and consumes too much energy, resulting in a lack of technical and economic feasibility; (3) The coupled reduction of aluminum and sulfur has the problem of high environmental treatment costs.

[0006] Patent CN101777651B discloses a silicon negative electrode material and a preparation method thereof, and a lithium battery using the material, comprising an active substance and a volume buffer, wherein the active substance is coated or partially coated on the surface of particles of the volume buffer, the active substance is silicon, and the volume buffer is silicon dioxide. The present invention also provides a preparation method of the negative electrode material, wherein the pretreated silicon dioxide powder and the carbon reducing agent powder are vacuum-sintered at high temperature; the negative electrode material provided by the present invention has good cycle performance and high specific capacity.

[0007] Patent CN107195904B discloses a method for preparing a silicon electrode material with a core-shell structure, wherein a reducing alloy is used as a carrier, organic silicon is hydrolyzed to deposit silicon dioxide, and then mixed with a low melting point salt, thermally reduced, coated with a polymer, and calcined at high temperature to obtain a silicon / carbon / conductive metal composite electrode material; the reducing alloy is one or more of magnesium copper, aluminum copper, zinc copper, magnesium nickel, aluminum nickel, zinc nickel, magnesium silver, aluminum silver, zinc silver, magnesium tin, aluminum tin, and zinc tin; the low melting point salt is one or more of chloride, bromide, and fluoride salts of gallium, germanium, tin, aluminum, and magnesium; the polymer is one or more of polyaniline, polypyrrole, polythiophene, and derivatives of the above polymers; the molar ratio of silicon: reducing alloy: low melting point salt is 1:(2-5):(1-20); the molar ratio of silicon to polymer precursor is (1-20):1. The negative electrode material has good electrochemical properties and has good application prospects in the field of lithium-ion batteries.

[0008] Patent CN106410139B discloses a high-stability silicon / carbon nitride / carbon composite nanomaterial for lithium-ion battery electrodes, which is composed of porous silicon, carbon nitride and amorphous carbon, and the carbon nitride and amorphous carbon are directly grown on the surface of porous silicon; when the composite nanomaterial is used as a negative electrode material for a lithium-ion battery, charge and discharge experiments show that its first reversible capacity is 3032-3190mAh / g, and the reversible capacity after 100 cycles is 1415-1590mAh / g.

[0009] Patent CN109473628B discloses a silicon-carbon nitride composite negative electrode material and its preparation and application, wherein elemental silicon is mixed with a carbon nitrogen precursor to obtain a uniformly dispersed silicon / carbon nitrogen precursor; dried in a vacuum drying oven; and then calcined in a tubular furnace to obtain a silicon-carbon nitride composite material. The preparation method has a variety of carbon nitrogen precursors, a simple process, low cost, and a variety of product structures, which effectively alleviates the volume expansion of silicon negative electrode materials and improves the cycle stability of silicon-based lithium batteries.

[0010] Patent CN110739454B discloses a negative electrode material and a preparation method thereof, wherein the negative electrode material comprises a three-dimensional porous skeleton and simple silicon loaded on the three-dimensional porous skeleton, wherein the three-dimensional porous skeleton is a composite skeleton comprising metal and carbon, wherein the metal and carbon in the three-dimensional porous skeleton are both present in simple form; the metal is selected from any one or more of copper, iron, manganese, cobalt, tin, nickel, magnesium, titanium, aluminum or zinc. The composite skeleton composed of metal and carbon in the negative electrode material has excellent toughness and an ordered pore structure, which can buffer the volume effect of silicon during the insertion and extraction of lithium ions, enhance the structural stability of the negative electrode material, and improve the cycle stability of the negative electrode; and the metal and carbon have excellent electrical conductivity, and the composite with silicon effectively improves the electrochemical performance of the negative electrode material.

[0011] Patent CN112086629B discloses a Si@C / ZnNb 2 O 6 The invention relates to the technical field of negative electrode materials for lithium ion batteries, and comprises the following steps: electrostatic spinning with a spinning solution containing a pore-forming agent, high-temperature calcination in an inert protective atmosphere, and washing to obtain porous carbon fibers; mixing a soft template, nano-silicon, a niobium source, a zinc source, and porous carbon fibers, and adding the mixture to anhydrous ethanol to perform a solvent thermal reaction to obtain Si@C / ZnNb 2 O 6 Composite material. Si@C / ZnNb prepared by the present invention 2 O 6 The negative electrode composite material effectively combines the advantages of metal oxides and carbon materials, which not only improves the conductivity of nano-silicon, but also increases the active sites of the material, and can effectively improve the problem of silicon expansion during charging and discharging.

[0012] Patent CN113461015B discloses a method for preparing nitrogen-doped carbon-coated porous silicon, including: using silicon-magnesium alloy as a precursor, mixing it with carbon nitride, and then performing a first heat treatment under an inert atmosphere or vacuum conditions, and then continuing to heat up, and performing a second heat treatment under an inert atmosphere or vacuum conditions; or using silicon-magnesium alloy as a precursor, mixing it with carbon nitride, and then performing a heat treatment under an inert atmosphere or vacuum conditions, and then treating the intermediate product in acid, and drying to obtain nitrogen-doped carbon-coated porous silicon. This method can effectively improve the bonding force between the carbon coating layer and silicon, and improve the electrochemical stability of porous silicon negative electrode materials.

[0013] Patent CN113690417B discloses a negative electrode composite material and its preparation method and application. The preparation method comprises the following steps: (1) mixing and dissolving a carbon source and a dispersant, and spray drying the mixture to obtain carbon balls; (2) mixing a tin source, a zinc source and a solvent, coating the tin source and the zinc source on the carbon balls by liquid phase coating, and oxidizing and sintering the mixture to obtain a hollow spherical tin oxide / zinc oxide composite material; (3) mixing and dissolving a carbon source and a dispersant, and coating the carbon layer on the surface of the tin oxide / zinc oxide composite material by liquid phase coating, and reducing and sintering the mixture to obtain a precursor material; (4) introducing a silicon source, and depositing silicon inside the precursor obtained in step (3) to obtain the negative electrode composite material. The present invention dopes zinc and tin into the silicon-based negative electrode material, thereby improving the conductivity of the silicon-based material. The coated carbon shell has pores, which is conducive to the infiltration of the electrolyte, thereby enhancing the rate performance of the composite material.

[0014] Patent CN113428865B discloses a pomegranate-like silicon-based negative electrode material and a preparation method thereof, wherein the material has a pomegranate-like structure. The method comprises the following steps: (1) activating the nano silicon oxide raw material with concentrated sulfuric acid and hydrogen peroxide; (2) adding melamine to ionized water, stirring and dissolving, adding silicon oxide to the solution for ultrasonic dispersion, and then heating and stirring; (3) lowering the temperature to precipitate melamine on the surface of silicon oxide, and then centrifugally drying and calcining to obtain a precursor; (4) calcining the precursor in an argon atmosphere by a magnesium metal thermal reduction method, performing in-situ compounding, and then soaking it in acid, centrifugally washing it, and obtaining a pomegranate-like silicon-based negative electrode material. The pomegranate-like silicon-based negative electrode material for lithium-ion batteries prepared by the metal thermal reduction method of the present invention has low energy consumption, low cost, short cycle, and is conducive to industrial production. At the same time, the present invention makes full use of the pomegranate-like silicon-based negative electrode material prepared by defective carbon nitride material, and has excellent electrochemical properties.

[0015] Patent CN110739454B discloses a negative electrode material and a preparation method thereof, wherein the negative electrode material comprises a three-dimensional porous skeleton and simple silicon loaded on the three-dimensional porous skeleton, wherein the three-dimensional porous skeleton is a composite skeleton comprising metal and carbon, wherein the metal and carbon in the three-dimensional porous skeleton are both present in simple form; wherein the metal is selected from any one or more of copper, iron, manganese, cobalt, tin, nickel, magnesium, titanium, aluminum or zinc. In the negative electrode material, the composite skeleton composed of metal and carbon has excellent toughness and an ordered pore structure, which can buffer the volume effect of silicon during the insertion and extraction of lithium ions, enhance the structural stability of the negative electrode material, and improve the cycle stability of the negative electrode; and the metal and carbon have excellent electrical conductivity, and the composite with silicon effectively improves the electrochemical performance of the negative electrode material.

[0016] Patent CN113314702B discloses a carbon-silicon-coated tin dioxide composite and its preparation method and application as a negative electrode material for lithium-ion batteries. The ground biomass and ionic liquid are mixed and carbonized to obtain biochar; silicon powder and SnO 2 The nanoparticles are mixed and ball-milled to obtain silicon-oxygen compound-coated tin dioxide nanoparticles; biocarbon is added to the silicon-oxygen compound-coated tin dioxide nanoparticles, and ball-milling is continued to obtain a biocarbon-silicon-coated tin dioxide composite; and finally the biocarbon-silicon-coated tin dioxide composite is sieved. The present invention uses a ball-milling method to simply and conveniently prepare the desired carbon-silicon-coated tin dioxide composite negative electrode material, which has a high reversible specific capacity, good conductivity, and good cycle performance.

[0017] Patent CN112993223B discloses a double-layer coated lithium-ion battery negative electrode material and a preparation method thereof, wherein the material is a Si@AZO@C single-core double-layer coated structure, wherein from the inside to the outside, the core is a silicon matrix, the first coating layer is an AZO (aluminum-doped zinc oxide) conductive film layer, and the second coating layer is a porous carbon matrix layer. The lithium-ion battery negative electrode material of the present invention has a single-core double-layer coated structure, Si is used as the core, and an AZO layer and a carbonized MOF layer are sequentially coated on its surface. The AZO flexible film can shrink and expand repeatedly without breaking, which helps to release the volume strain of silicon during the charging and discharging process, thereby extending the service life of the composite material. Secondly, the outer layer is compounded with Co-based MOF, which is conducive to the transmission of ions and electrons, greatly improving the overall conductivity of the material, and can simultaneously solve the problems of low specific capacity, poor conductivity and poor cycle performance of Si / SiC composite materials, and also improve the problem of poor characteristics caused by the volume change of the silicon-based negative electrode material during the charging and discharging process.

[0018] In summary, the measures in the prior art for improving the anti-expansion performance of silicon negative electrode materials and reducing the volume change of silicon negative electrode materials during charging and discharging mainly include: (1) reducing the particle size of silicon negative electrode materials to nanometer level and using the gaps between nanoparticles as buffer space; (2) compounding silicon negative electrode materials with porous carbon materials, carbon nanotubes, graphite and graphene to form a buffer; (3) compounding single silicon negative electrode materials with metal skeleton materials to form a buffer; (4) compounding single silicon negative electrode materials with graphite phase carbon nitride materials to improve their electrochemical performance; (5) compounding single silicon negative electrode materials with conductive carrier materials to form a buffer; (6) compounding silicon negative electrode materials with a combination of conductive materials and porous materials to improve their electrochemical performance.

[0019] The main measures in the prior art to improve the conductivity of silicon negative electrode materials include: (1) doping or compounding conductive metal materials into silicon negative electrode materials to improve conductivity and resistance to volume expansion; (2) doping or compounding conductive carbon materials, carbon nanotubes, graphite, graphene, and conductive plastics into silicon negative electrode materials to improve conductivity and resistance to volume expansion; (3) doping or compounding metal oxides and their compositions into silicon negative electrode materials to improve conductivity and resistance to volume expansion; (4) doping or compounding non-metals, metals, and their oxide compositions into silicon negative electrode materials to improve conductivity and resistance to volume expansion. Summary of the invention

[0020] The purpose of the present invention is to provide a method for preparing a conductive silicon-carbon negative electrode material to overcome the defects of high preparation cost of the silicon-carbon negative electrode material, excessive volume expansion during charging, and poor conductivity.

[0021] In order to achieve the above object, the present invention is realized by the following technical scheme: a method for preparing a conductive silicon-carbon negative electrode material, using in-situ formed graphite phase carbon nitride as a reducing agent for thermal reduction of nano-silicon to nano-silicon and a pore-forming agent for carrier activated carbon, thermally reducing gC coated with an indium tin oxide-silicon dioxide composite conductive film at 560-800°C 3 N 4 -C composite material is a conductive nano silicon carbon negative electrode material, comprising the following steps:

[0022] S1: Preparation of nano-indium tin oxide-silicon dioxide composite hydrosol;

[0023] S2: Preparation of phenol formaldehyde-melamine formaldehyde copolymer;

[0024] S3: adding the phenol formaldehyde-melamine formaldehyde copolymer obtained in step S2 to the nano indium tin oxide-silicon dioxide composite hydrosol obtained in step S1 to obtain a phenol formaldehyde-melamine formaldehyde copolymer xerogel coated with the composite conductive film hydrosol;

[0025] S4: high temperature treatment of the phenol formaldehyde-melamine formaldehyde copolymer dry gel coated with the composite conductive film obtained in step S3 to obtain gC 3 N 4 -C composite materials;

[0026] S5: gC coated with the composite conductive film obtained in step S4 3 N 4 The -C composite material is further treated at high temperature to obtain a conductive nano-silicon-carbon negative electrode material.

[0027] Preferably, step S1 specifically comprises:

[0028] S1.1: dissolving tetraethyl orthosilicate in a 70% by mass ethanol aqueous solution, adding hydrochloric acid as a catalyst, and performing a hydrolysis reaction at room temperature for 8-12 hours to obtain a nano-silica hydrosol;

[0029] S1.2: dissolving indium chloride and tin chloride in an ethanol aqueous solution with a mass fraction of 70%, adding ethanolamine or diethanolamine stabilizer, controlling the feed molar ratio of In:Sn:stabilizer=1:0.01-0.1:0.5-5, and performing a hydrolysis reaction at room temperature for 1-3h to obtain nano indium tin oxide hydrosol;

[0030] S1.3: Mix the nano-silicon dioxide hydrosol and the nano-indium tin oxide hydrosol at a molar ratio of Si:In=1:0.05-0.2, and stir the mixture at room temperature for 0.5-1h to obtain a nano-indium tin oxide-silicon dioxide composite hydrosol.

[0031] By adopting the above technical scheme, indium chloride and tin chloride ethanol aqueous solution can form indium tin hydroxide coprecipitation under alkaline conditions, and alkaline ethanolamine or diethanolamine is selected as a stabilizer, and the indium chloride and tin chloride ethanol aqueous solution is slowly hydrolyzed into nano indium tin oxide hydrosol, rather than coprecipitation of indium tin hydroxide. This is because ethanolamine or diethanolamine has a coordination effect with transition metals, has a stabilizing effect on the nano indium tin oxide hydrosol, and inhibits the generation of indium tin hydroxide coprecipitation. Nano silica hydrosol and nano indium tin oxide hydrosol can be mutually dissolved to form nano indium tin oxide-nano silica composite hydrosol, which can polymerize to form a composite hydrogel during the aging process.

[0032] Preferably, step S2 specifically comprises: heating and stirring phenol, melamine and formaldehyde in an acidic aqueous solution for 2-4 hours, controlling the feeding molar ratio of phenol: melamine: formaldehyde = 1: 0.2-2: 1.2-5, reacting to generate a precipitate of phenol formaldehyde-melamine formaldehyde copolymer, filtering the precipitate, drying and crushing the precipitate to obtain a powder of phenol formaldehyde-melamine formaldehyde copolymer.

[0033] The above technical scheme is adopted to synthesize phenol formaldehyde-melamine formaldehyde copolymer with phenol, melamine and formaldehyde as raw materials. The composition and structure of the copolymer are relatively complex, mainly phenol formaldehyde-melamine formaldehyde block copolymer, and also includes some phenol formaldehyde-melamine formaldehyde alternating copolymer. The phenol formaldehyde-melamine formaldehyde copolymer is coated with nano-indium tin oxide-nano-silicon dioxide composite hydrosol to form a composite hydrogel with a core-shell structure.

[0034] The ethyl orthosilicate in the present invention is easily soluble in ethanol aqueous solution, and undergoes hydrolysis reaction under acidic conditions to form nano-silicon dioxide hydrosol, which has good film-forming and coating effects. If necessary, other organic silicon coupling agents can be added to improve its performance.

[0035] Preferably, step S3 is specifically as follows: adding the powder of the phenol formaldehyde-melamine formaldehyde copolymer obtained in step S2 to the nano indium tin oxide-silicon dioxide composite hydrosol obtained in step S1, shaking for 12-24 hours to form a hydrogel of the mixture, and drying the hydrogel at 110-150° C. to obtain a phenol formaldehyde-melamine formaldehyde copolymer xerogel coated with a composite conductive film.

[0036] Preferably, step S4 is specifically as follows: the phenol formaldehyde-melamine formaldehyde copolymer xerogel coated with the composite conductive film obtained in step S3 is placed in a crucible, placed in a high-temperature furnace protected by inert gas, and slowly heated to 550° C. at a rate of 3-5° C. / min, and kept warm for 1-3 hours to obtain gC coated with the composite conductive film. 3 N 4 -C composite material.

[0037] Preferably, step S5 specifically comprises: 3 N 4 The C composite material is further heated to 560-800°C in a high-temperature furnace protected by inert gas and kept at this temperature for 3-9 hours. 3 N 4 gC in C-composite materials 3 N 4 Thermal reduction of nano-silicon dioxide to nano-silicon, gC 3 N 4 The decomposition of the copolymer activated carbon leaves a large number of micropores, and the nano-silicon is loaded on the copolymer activated carbon to generate a conductive nano-silicon carbon negative electrode material, the mass composition of which is Si 30%-60%, C 20%-50%, O 5%-15%, In5%-15%, Sn 0.5%-5%; its specific surface area is 600-900m 2 / g; the specific capacity retention rate after 100 charge and discharge cycles is 83%-93%.

[0038] By adopting the above technical scheme, when the phenol formaldehyde-melamine formaldehyde copolymer dry gel coated with nano-indium tin oxide-nano-silicon dioxide is sintered at 550° C., the experiment found that the nano-indium tin oxide-nano-silicon dioxide in the outer shell is sintered to form a surface film with good conductivity; the phenol formaldehyde-melamine formaldehyde copolymer powder in the inner core undergoes a thermochemical reaction, the phenol formaldehyde component in the copolymer is mainly converted into activated carbon, the melamine formaldehyde component in the copolymer is mainly converted into graphite phase carbon nitride with good stability, and the copolymer also has some oxidative degradation.

[0039] Experimental discovery of gC 3 N 4The melting point and boiling point of gC are very high, and the chemical properties are also very stable. It begins to oxidatively decompose at 560°C. The present invention creatively uses it as a thermal reducing agent and a pore-forming agent at the same time. 3 N 4 It can capture oxygen from nano-silicon dioxide molecules and convert them into nano-silicon. 3 N 4 It is oxidized and decomposed into nitrogen and carbon dioxide. The chemical reaction formula is: 3SiO 2 +gC 3 N 4 →3Si+3CO 2 ↑+2N 2 ↑.

[0040] Because gC 3 N 4 The reducibility of metal is stronger than that of activated carbon materials. The minimum temperature required for thermal reduction of nano-silicon dioxide to nano-silicon is 560°C, while the minimum temperature required for thermal reduction of nano-silicon dioxide to nano-silicon by activated carbon materials is above 1000°C. Although the reaction temperature required for thermal reduction of nano-silicon dioxide to nano-silicon by metal is below 500°C, due to the excessive consumption of metal powder, the high cost of raw materials, and the troublesome removal of the generated metal oxides, this method lacks technical and economic feasibility.

[0041] When the nano-indium tin oxide-silicon dioxide composite conductive film is coated with gC 3 N 4 When the C-composite material is further heated to 560-800℃ in a high temperature furnace protected by inert gas, gC 3 N 4 gC in C-composite materials 3 N 4 The component has stronger reducing property than the activated carbon component, and preferentially undergoes thermal reduction reaction with nano-silicon dioxide, which reduces nano-silicon dioxide to nano-silicon and loads it on the carrier activated carbon; on the other hand, gC 3 N 4 After decomposition, a large number of micropores are left in the activated carbon, which increases the specific surface area of ​​the carrier activated carbon, which is equivalent to the role of a pore-forming agent.

[0042] C 3 N 4 The carbon dioxide gas produced by thermal reduction of nano-silicon dioxide at high temperature also has a certain activation effect on the activated carbon material, leaving more micropores in the carrier activated carbon and increasing the specific surface area of ​​the carrier activated carbon. The chemical reaction formula is: C+CO 2 →2CO↑.

[0043] In the present invention, gC 3 N 4The new technology of thermally reducing nano-silicon dioxide to nano-silicon at high temperature has greatly reduced the thermal reduction temperature compared with the existing technology of thermally reducing nano-silicon dioxide to nano-silicon using activated carbon materials; compared with the existing technology of thermally reducing nano-silicon dioxide to nano-silicon using metals, it not only greatly reduces the cost of raw materials, but also does not require the subsequent complicated process of processing metal oxides, and the residual gC 3 N 4 It also has no adverse effect on the performance of silicon-carbon negative electrode materials.

[0044] The nano-indium tin oxide conductive film used in the present invention not only has better conductivity than the tin antimony oxide conductive film and the zinc aluminum oxide conductive film, but also has a specific catalytic thermal reduction function of nano-silicon dioxide to nano-silicon. This is because at a high temperature above 560°C, indium oxide can be reduced to metallic indium by activated carbon, which reduces the conductivity of the nano-indium tin oxide conductive film. The chemical reaction formula is expressed as: In 2 O 3 +C→In+CO 2 ↑; Under high temperature, metallic indium can also capture oxygen from nano-silicon dioxide molecules, converting them into nano-silicon, and then being oxidized and decomposed into indium oxide. Nano-indium oxide plays the role of a catalyst for the thermal reduction reaction of silicon dioxide. The chemical reaction formula is: 3SiO 2 +4In→3Si+2In 2 O 3 .

[0045] Compared with the prior art, the preparation method of the conductive silicon-carbon negative electrode material of the present invention has many substantial features and significant technical advances: (1) the gC generated in situ 3 N 4 It can also be used as a thermal reducing agent for the preparation of nano-silicon and a pore-forming agent for the carrier activated carbon; (2) Indium tin oxide conductive film is not only an excellent conductive material, but also a catalyst for the preparation of nano-silicon; (3) The carrier activated carbon formed by in-situ activation of phenol formaldehyde-melamine formaldehyde copolymer has a large specific surface area, and the silicon-carbon negative electrode material formed by loading nano-silicon and conductive film has good anti-expansion performance; (4) gC 3 N 4 When used as a thermal reducing agent for nano-silicon dioxide, the reaction temperature is low, the raw material cost is low, and it has technical and economic benefits.

[0046] Beneficial effects of the present invention:

[0047] (1) In the present invention, the graphite phase carbon nitride formed in situ is used as a thermal reducing agent and a pore-forming agent at the same time, which can thermally reduce nano-silicon dioxide to nano-silicon, and can convert gC 3 N 4 -C composite material is activated into a carrier activated carbon with high specific surface area.

[0048] (2) The activated carbon in situ formed by the phenol formaldehyde-melamine formaldehyde copolymer in the present invention has a large specific surface area, and the conductive silicon-carbon negative electrode material formed by loading nano-silicon and a conductive film has good anti-expansion performance.

[0049] (3) The indium tin oxide conductive film coated with the nano-silicon carbon material in the present invention has good conductivity, which not only improves the electrochemical performance of the silicon-carbon negative electrode material, but also has a catalytic effect on the thermal reduction reaction of nano-silicon dioxide to nano-silicon. DETAILED DESCRIPTION

[0050] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.

[0051] Embodiment 1: 210g (1mol) of tetraethyl orthosilicate was dissolved in 800mL of 70% ethanol aqueous solution by mass fraction, and then 20mL (0.25mol) of concentrated hydrochloric acid catalyst was added, and hydrolysis reaction was carried out at room temperature for 12h to obtain nano silicon dioxide hydrosol; 18.g (0.1mol) of indium chloride and 1.9g (0.01mol) of stannous chloride were dissolved in 100mL of 70% ethanol aqueous solution by mass fraction, and then 24.4g (0.4mol) of ethanolamine stabilizer was added, and hydrolysis reaction was carried out at room temperature for 2h to obtain nano indium tin oxide hydrosol; the above nano silicon dioxide hydrosol was mixed with nano indium tin oxide hydrosol, and stirred for reaction at room temperature for 0.5h to obtain 925g of nano indium tin oxide-silicon dioxide composite hydrosol.

[0052] 19.8 g (0.2 mol) of phenol, 25.2 g (0.2 mol) of melamine and 64.8 g (0.8 mol) of a 37% formaldehyde aqueous solution were stirred in a hydrochloric acid aqueous solution with a pH of 1-2 at 60° C. for 2 h to react to generate a precipitate of a phenol formaldehyde-melamine formaldehyde copolymer. The precipitate was filtered, dried and crushed to obtain 29.6 g of a powder of a phenol formaldehyde-melamine formaldehyde copolymer.

[0053] The above phenol formaldehyde-melamine formaldehyde copolymer powder was added to the above nano indium tin oxide-silicon dioxide composite hydrosol, and the mixture was shaken for 24 hours to form a hydrogel. The hydrogel was dried at 110-150° C. to obtain 105 g of phenol formaldehyde-melamine formaldehyde copolymer xerogel coated with a composite conductive film.

[0054] The dry gel of phenol formaldehyde-melamine formaldehyde copolymer coated with the composite conductive film was placed in a crucible, placed in a high-temperature furnace protected by nitrogen, and slowly heated to 550°C at a rate of 3-5°C / min and kept warm for 3h to obtain gC coated with the composite conductive film. 3 N 4-C composite material 95g.

[0055] The gC coated with the above composite conductive film 3 N 4 The -C composite material was further heated to 560°C in a high-temperature furnace protected by nitrogen and kept warm for 9 hours to produce 70g of conductive nano-silicon-carbon negative electrode material, with a mass composition of Si 50.9%, C 21.8%, O11.6%, In 13.5%, Sn 2.2%; its specific surface area was 600m 2 / g; the specific capacity retention rate after 100 charge and discharge cycles is 83%.

[0056] Embodiment 2: 210g (1mol) of tetraethyl orthosilicate was dissolved in 800mL of 70% ethanol aqueous solution by mass fraction, and then 8.3mL (0.1mol) of concentrated hydrochloric acid catalyst was added, and hydrolysis reaction was carried out at room temperature for 12h to obtain nano silicon dioxide hydrosol; 18.g (0.1mol) of indium chloride and 1.0g (0.005mol) of stannous chloride were dissolved in 100mL of 70% ethanol aqueous solution by mass fraction, and then 21g (0.2mol) of diethanolamine stabilizer was added, and hydrolysis reaction was carried out at room temperature for 2h to obtain nano indium tin oxide hydrosol; the above nano silicon dioxide hydrosol was mixed with nano indium tin oxide hydrosol, and stirred for reaction at room temperature for 1h to obtain 680g of nano indium tin oxide-silicon dioxide composite hydrosol.

[0057] 47 g (0.5 mol) of phenol, 25.2 g (0.2 mol) of melamine and 89 g (1.1 mol) of a 37% formaldehyde aqueous solution were stirred in a hydrochloric acid aqueous solution with a pH of 1-2 at 60° C. for 2 h to react to generate a precipitate of a phenol formaldehyde-melamine formaldehyde copolymer. The precipitate was filtered, dried and crushed to obtain 85.4 g of a powder of a phenol formaldehyde-melamine formaldehyde copolymer.

[0058] Add the above phenol formaldehyde-melamine formaldehyde copolymer powder to the above nano indium tin oxide-silicon dioxide composite hydrosol, shake for 24 hours to form a hydrogel of the mixture, and dry the hydrogel at 110-150° C. to obtain 125 g of phenol formaldehyde-melamine formaldehyde copolymer xerogel coated with a composite conductive film.

[0059] The dry gel of phenol formaldehyde-melamine formaldehyde copolymer coated with the composite conductive film was placed in a crucible, placed in a high-temperature furnace protected by nitrogen, and slowly heated to 550°C at a rate of 3-5°C / min and kept warm for 3h to obtain gC coated with the composite conductive film. 3 N 4 -C composite material 87.5g.

[0060] The gC coated with the above composite conductive film3 N 4 The -C composite material was further heated to 800°C in a high-temperature furnace protected by nitrogen and kept warm for 3 hours to produce 70g of conductive nano-silicon-carbon negative electrode material, with a mass composition of Si 39.9%, C 41.9%, O 6.8%, In 10.5%, Sn 0.9%; its specific surface area was 900m 2 / g; the specific capacity retention rate after 100 charge and discharge cycles is 93%.

[0061] Comparative Example 1: Silicon negative electrode material was prepared according to the method of patent CN101777651B, 36 grams of pretreated silicon dioxide powder and 12 grams of carbon reducing agent were mixed, stirred for 12 hours to make them evenly mixed, and then sent to 1000°C vacuum environment for reaction, kept warm for 3 hours, and then cooled to room temperature to obtain negative electrode material. After 150 charge and discharge cycles, the specific capacity retention rate was 69%.

[0062] Comparative Example 2: Silicon negative electrode material was prepared according to the method of patent CN 107195904B, and the alloy reduction to prepare nano-silicon was completed at 500°C. The obtained silicon-based material contained a three-dimensional porous structure of conductive metal / silicon / carbon. When used for the negative electrode of lithium-ion batteries, after 100 charge and discharge cycles, the specific capacity retention rate was 77%.

[0063] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention.

[0064] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for preparing a conductive silicon-carbon negative electrode material, It is characterized in that The following steps are involved: S1: Preparation of nano-indium tin oxide-silicon dioxide composite hydrosol; S2: Preparation of phenol formaldehyde-melamine formaldehyde copolymer; S3: adding the phenol formaldehyde-melamine formaldehyde copolymer obtained in step S2 to the nano indium tin oxide-silicon dioxide composite hydrosol obtained in step S1 to obtain a phenol formaldehyde-melamine formaldehyde copolymer xerogel coated with the composite conductive film hydrosol; S4: high temperature treatment of the phenol formaldehyde-melamine formaldehyde copolymer dry gel coated with the composite conductive film obtained in step S3 to obtain gC 3 N 4 -C composite materials; S5: gC coated with the composite conductive film obtained in step S4 3 N 4 The -C composite material is further treated at high temperature to obtain a conductive nano-silicon-carbon negative electrode material.

2. A method for preparing a conductive silicon-carbon negative electrode material as claimed in claim 1, Features: Step S1 is specifically as follows: S1.1: dissolving tetraethyl orthosilicate in 70% by mass ethanol aqueous solution, adding hydrochloric acid catalyst, and hydrolyzing at room temperature for 8-12 hours to obtain nano-silica hydrosol; S1.2: dissolving indium chloride and tin chloride in an ethanol aqueous solution with a mass fraction of 70%, adding ethanolamine or diethanolamine stabilizer, controlling the feed molar ratio of In:Sn:stabilizer to be 1:0.01-0.1:0.5-5, and hydrolyzing the reaction at room temperature for 1-3h to obtain nano indium tin oxide hydrosol; S1.3: Mix the nano-silicon dioxide hydrosol and the nano-indium tin oxide hydrosol at a molar ratio of Si:In=1:0.05-0.2, and stir the mixture at room temperature for 0.5-1h to obtain a nano-indium tin oxide-silicon dioxide composite hydrosol.

3. A method for preparing a conductive silicon-carbon negative electrode material according to claim 1, Features: Step S2 specifically comprises: heating and stirring phenol, melamine and formaldehyde in an acidic aqueous solution for 2-4 hours, controlling the molar ratio of phenol: melamine: formaldehyde to be 1: 0.2-2: 1.2-5, reacting to generate a precipitate of a phenol formaldehyde-melamine formaldehyde copolymer, filtering the precipitate, air-drying and crushing the precipitate to obtain a powder of the phenol formaldehyde-melamine formaldehyde copolymer.

4. A method for preparing a conductive silicon-carbon negative electrode material according to claim 1, Features: Step S3 is specifically as follows: adding the powder of the phenol formaldehyde-melamine formaldehyde copolymer obtained in step S2 to the nano indium tin oxide-silicon dioxide composite hydrosol obtained in step S1, shaking for 12-24 hours to form a hydrogel of the mixture, and drying the hydrogel at 110-150° C. to obtain a phenol formaldehyde-melamine formaldehyde copolymer xerogel coated with a composite conductive film.

5. A method for preparing a conductive silicon-carbon negative electrode material according to claim 1, Features: Step S4 is specifically as follows: the phenol formaldehyde-melamine formaldehyde copolymer xerogel coated with the composite conductive film obtained in step S3 is placed in a crucible, placed in a high-temperature furnace protected by inert gas, and slowly heated to 550°C at a rate of 3-5°C / min, and kept at this temperature for 1-3h to obtain gC coated with the composite conductive film. 3 N 4 -C composite material.

6. A method for preparing a conductive silicon-carbon negative electrode material according to claim 1, Features: Step S5 specifically comprises: 3 N 4 The -C composite material is further heated to 560-800°C in a high-temperature furnace protected by inert gas and kept warm for 3-9 hours to obtain a conductive nano-silicon-carbon negative electrode material with a mass composition of Si 30%-60%, C 20%-50%, O5%-15%, In 5%-15%, and Sn 0.5%-5%; its specific surface area is 600-900m 2 / g; the specific capacity retention rate after 100 charge and discharge cycles is 83%-93%.