Catalyst for preparing methyl glycolate by hydrogenation of dimethyl oxalate as well as preparation method and application of catalyst
Through the displacement reaction of the copper-silver bimetallic catalyst, a copper-silver core-shell structure is formed, which solves the problems of low selectivity and poor stability of the existing catalysts, and achieves high catalytic activity and low-cost production of methyl glycolate.
Patent Information
- Application Number
- CN202410740703.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-10
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-10
AI Technical Summary
Among existing catalysts for the hydrogenation of dimethyl oxalate to prepare methyl glycolate, the copper-based catalyst has low selectivity, while the silver-based catalyst has a high silver loading and poor stability, resulting in high costs and reduced activity.
A copper-silver bimetallic catalyst is used to replace the surface of copper particles with a single layer of uniform silver species through a displacement reaction to form a copper-silver core-shell structure. The carrier is silicon oxide, and the silver species accounts for 1-10wt.% of the total mass to improve Catalyst selectivity and stability.
A copper-silver bimetallic catalyst with high catalytic activity, selectivity and stability is achieved, the silver loading is reduced, and the industrial application prospects and economic benefits of the catalyst are improved.
Smart Images

Figure CN118847144A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalysts and relates to a catalyst for preparing methyl glycolate by hydrogenating dimethyl oxalate, and more specifically to a catalyst for preparing methyl glycolate by hydrogenating dimethyl oxalate, and a preparation method and application thereof. Background Art
[0002] Methyl glycolate is an important chemical raw material intermediate, which can be used to synthesize high value-added chemicals such as medicines, cosmetics, fragrances, pesticides, etc., and has broad application prospects. Polyglycolic acid has strong environmental degradation and can be degraded into carbon dioxide and water in nature within 1-3 months. The demand is huge, so large-scale production of methyl glycolate, the raw material for synthesizing polyglycolic acid, is crucial. However, the traditional methyl glycolate production process has serious pollution and harsh reaction conditions, and it is impossible to produce methyl glycolate on a large scale. In recent years, the coal-based route to produce methyl glycolate through selective hydrogenation of dimethyl oxalate (DMO) has become one of the most promising coal chemical technologies in my country. It is expected to achieve high-value-added degradable materials from coal by regulating the distribution of hydrogenation reaction products. The process has high atomic utilization and is environmentally friendly, which is of great significance to promoting the high-end, diversified and low-carbon development of my country's coal chemical industry.
[0003] At present, the commonly used catalysts for preparing methyl glycolate by hydrogenation of dimethyl oxalate are copper-based catalysts and silver-based catalysts. Compared with copper-based catalysts, silver-based catalysts have weaker hydrogenation ability and weaker adsorption effect on methyl glycolate. Therefore, they can catalyze the highly selective hydrogenation of dimethyl oxalate to methyl glycolate, inhibit its deep hydrogenation, and show a higher yield of methyl glycolate, which can reach more than 85%. However, silver catalysts still have the following problems: 1. In order to ensure that the silver species exists in the form of metallic silver and shows good catalytic activity, the silver loading of the catalyst is generally high, often greater than 10wt.%, which is expensive and costly; 2. The Tamman temperature of silver is low, and the reaction temperature easily leads to the agglomeration and sintering of silver particles, resulting in poor catalyst stability. If a carrier with strong interaction with the silver species is selected, the silver loses electrons, causing its activity to drop significantly, and the acid-base sites on the surface of the carrier easily promote side reactions, reducing selectivity. Summary of the invention
[0004] The present invention aims to overcome the shortcomings of the prior art. Aiming at the problems of low selectivity of copper-based catalysts in the technology of hydrogenating dimethyl oxalate to prepare methyl glycolate and high silver loading and poor stability of silver-based catalysts, a copper-silver bimetallic catalyst is proposed, that is, copper nanoparticles that strongly interact with carrier silicon oxide are used as catalyst precursors. Through a replacement reaction, the metal on the surface of the copper particles is replaced with a single-layer, uniform silver species, thereby reducing the silver loading and promoting its stability without reducing the metallic properties and activity of silver.
[0005] The present invention successfully prepares a copper-silver bimetallic catalyst with a copper-silver core-shell structure by a replacement method. When used for the reaction of preparing methyl glycolate (MG) by hydrogenation of dimethyl oxalate, the catalyst has the characteristics of simple preparation, high catalytic activity, high selectivity and high stability.
[0006] The technical solution adopted by the present invention is:
[0007] A preparation method and application of a catalyst for preparing methyl glycolate by hydrogenating dimethyl oxalate. The catalyst is a copper-silver bimetallic catalyst, comprising a carrier and an active component, wherein the active component is a copper species and a silver species, and the carrier is silicon dioxide. The structure of the copper-silver bimetallic catalyst is as follows: the silver species uniformly covers the surface of the copper species in the form of a shell layer to form a core-shell structure, and the core-shell structure is located on the carrier silicon dioxide in the form of particles, wherein copper and silicon oxide form a strong interaction.
[0008] The core-shell structure here means that the silver species is evenly dispersed on the surface of the copper particles like a shell, ensuring that there is a shell layer composed of silver atoms coating the outside of the copper particles. At the same time, the silver shell is also uniform and dense, and can ensure the uniform dispersion of the Cu@Ag particles.
[0009] The silver species accounts for 1-10wt.% of the total mass of the copper-silver bimetallic catalyst, and the copper species accounts for 1-10wt.% of the total mass of the copper-silver bimetallic catalyst. The reason why the mass of the copper-silver bimetallic catalyst needs to be limited to the above range is that: 1. High silver content will make the distribution of the silver shell layer on the surface of the particles uneven, resulting in uneven particle size, which will lead to decreased activity; 2. Increased silver content may also cause part of the silver to not participate in the formation of the core-shell structure, and form silver flocs that grow freely outside the particles, causing some particles to agglomerate. 3. High copper content will cause the particles to be too large and the activity to decrease; 4. Increased copper content may also make the outer layer of copper unable to be completely covered by silver, and the exposed copper is easy to catalyze the deep hydrogenation of methyl glycolate to produce ethylene glycol, resulting in decreased selectivity.
[0010] The copper-silver bimetallic catalyst has a specific surface area of 50-300 m 2 / g, average pore volume is 0.4-1.7cm 3 / g, and the average pore size is 5-30nm. The particle size of the copper-silver bimetal is 1.0-10nm, and the thickness of the silver shell is 0.2-2nm; further, the particle size of the copper-silver bimetal is 1.0-8nm, and the thickness of the silver shell is 0.2-1nm.
[0011] Another object of the present invention is to provide a method for preparing a copper-silver bimetallic catalyst for preparing methyl glycolate by hydrogenating dimethyl oxalate using a replacement process, comprising the following steps:
[0012] Dissolve copper nitrate in deionized water and add ammonia;
[0013] The two solutions obtained above are mixed and mechanically stirred, and a certain amount of silica sol is dropped into the mixture at a certain rate;
[0014] The solution obtained above is subjected to aging treatment, and then heated to evaporate ammonia, and after completion, filtered and washed;
[0015] The washed product is placed in an oven for drying, and then calcined at high temperature to obtain a catalyst precursor, and the catalyst precursor is subjected to a reduction treatment;
[0016] The reduced catalyst precursor is mixed with silver nitrate and ethanol, and ultrasonic treatment and mechanical stirring are performed during the process;
[0017] The obtained solution is centrifuged to extract the Cu@Ag particles, which are then washed with ethanol and deionized water and dried to obtain a finished catalyst product.
[0018] The copper nitrate solution and ammonia water are mixed and stirred for 30 minutes. The aging treatment time is 4 hours. The temperature of ammonia evaporation is 80°C. The drying conditions of the washed product are: temperature 80-130°C, time 12-24 hours. Any one of H2, NaBH4 or N2H4 is used for reduction treatment. The drying after washing with ethanol and deionized water is vacuum drying, the drying temperature is 80-130°C, and the drying time is 12-24 hours.
[0019] The catalyst precursor is mixed with silver nitrate and ethanol at room temperature (20-30°C) or low temperature (-50 to -110°C). The amount of silver nitrate added needs to ensure that the mass ratio of copper to silver is any one of 7:5, 1:1 and 5:7.
[0020] Another object of the present invention is to provide an application of a copper-silver bimetallic catalyst for preparing methyl glycolate by hydrogenating dimethyl oxalate synthesized by a displacement method, wherein the catalyst is used to catalyze the selective hydrogenation of dimethyl oxalate to produce methyl glycolate; specifically, the mixed gasified dimethyl oxalate and hydrogen are introduced into a reactor encapsulated with the copper-silver bimetallic catalyst for reaction; the reaction pressure is 0.5-3.5 MPa; the reaction temperature is 180-240° C.; the mass space velocity of dimethyl oxalate is 0.1-4.0 h -1 ; The hydrogen ester molar ratio is 60-150.
[0021] Or:
[0022] The invention discloses an application of a catalyst prepared by a preparation method of a copper-silver bimetallic catalyst for preparing methyl glycolate by hydrogenating dimethyl oxalate synthesized by a displacement method, wherein the catalyst is used to catalyze the selective hydrogenation of dimethyl oxalate to produce methyl glycolate; specifically, the mixed gasified dimethyl oxalate and hydrogen are introduced into a reactor encapsulated with the copper-silver bimetallic catalyst for reaction; the reaction pressure is 0.5-3.5MPa; the reaction temperature is 180-240°C; the mass space velocity of dimethyl oxalate is 0.1-4.0h -1 ; The hydrogen ester molar ratio is 60-150.
[0023] The present invention has the following beneficial effects:
[0024] 1. The present invention successfully prepares a bimetallic catalyst with a copper-silver core-shell structure. The core-shell structure here means that the silver species is evenly dispersed on the surface of the copper particles like a shell layer, ensuring that there is a shell layer composed of silver atoms coating the outside of the copper particles. At the same time, the silver shell layer is also uniform and dense, and can ensure the uniform dispersion of Cu@Ag particles.
[0025] 2. The copper-silver bimetallic catalyst of the present invention has high stability when used in the heterogeneous hydrogenation reaction of dimethyl oxalate. The reason is that: layered copper silicate is used as a precursor, and copper metal nanoparticles with strong interaction with silicon oxide are formed after reduction, and the Ag species are located on the surface of the copper species. The interaction between copper and silicon oxide provides a basis for anchoring the silver species, which can prevent the sintering of silver particles and ensure that there is no problem of silver particle growth during long-term use, thereby improving its stability and greatly reducing the cost of catalyst replacement in industry.
[0026] 3. The copper-silver bimetallic catalyst of the present invention has the characteristics of low silver loading and high catalytic activity when used for heterogeneous hydrogenation of dimethyl oxalate. Compared with the silver loading of more than 10wt.% in the prior art, the silver species loading in the present invention is only 4-7wt.%, and the MG yield can reach more than 90%. The low silver loading greatly improves the utilization efficiency and greatly saves the catalyst production cost.
[0027] 4. The preparation process of the copper-silver bimetallic catalyst of the present invention changes the copper-silver mass ratio and the replacement reaction synthesis temperature. The change in the mass ratio changes the size of the core-shell structure copper particles and the thickness of the silver shell. The change in the replacement reaction synthesis temperature changes the uniformity of the core-shell structure silver shell, and finally a copper-silver bimetallic catalyst with a copper-silver bimetallic particle size of 1.0-10nm and a silver shell size of 0.2-2nm is obtained, thereby changing the catalytic activity of the catalyst.
[0028] 5. The present invention changes the particle size of the copper-silver bimetallic particles and the formation of the core-shell structure by adjusting the reduction conditions during the synthesis process.
[0029] 6. When the copper-silver bimetallic catalyst obtained by the present invention is used for the heterogeneous hydrogenation reaction of dimethyl oxalate, the raw materials for catalyst preparation are easily available, the reaction conditions are mild, the process is simple and controllable, the structure is stable, the operability is strong, and it has good industrial application prospects and the like. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a high-resolution TEM image of the Cu@Ag structure of the copper-silver bimetallic catalyst of the present invention;
[0031] Figure 2 The XRD diagram of the catalyst after reduction under different reduction conditions in the present invention is
[0032] Figure 3 This is a stability test of the catalysts in the comparative examples and embodiments of the present invention. DETAILED DESCRIPTION
[0033] The present invention is further described below by way of examples, which are not limited to the examples. Experimental methods without specific conditions specified in the examples are generally carried out under conventional conditions and conditions described in the manual, or under conditions recommended by the manufacturer. The general equipment, materials, reagents, etc. used are all commercially available unless otherwise specified.
[0034] The methods for online reduction of the catalyst and evaluation of the catalytic effect in this embodiment and comparative example are as follows:
[0035] In the present invention, the hydrogenation reaction of dimethyl oxalate is carried out in a fixed bed reactor. 0.5 g of catalyst is loaded, reduced at 300° C., maintained for 4 hours, cooled to the reaction temperature, the dimethyl oxalate solution is gasified and mixed with hydrogen before entering the reaction system, the hydrogen-ester ratio is 80, and the hydrogenation reaction is carried out at 2.5 MPa and 225° C. The products after the reaction are analyzed by gas chromatography, and the conversion rate of dimethyl oxalate and the selectivity and yield of methyl glycolate are calculated. Since the hydrogenation reaction of dimethyl oxalate is a series reaction and methyl glycolate is an intermediate hydrogenation product, the difference in the selectivity of the intermediate product can only be reflected when the conversion rate is not 100%; in the process of stability evaluation, in order to make full use of all active sites to participate in the reaction and prevent the occurrence of catalyst deactivation while the conversion rate is still 100%, it is necessary to carry out stability evaluation under the condition that the conversion rate is not 100%; in order to characterize the thermal stability of the catalyst, the atmosphere is switched during the reaction, and the high-temperature heat treatment of nitrogen at 350° C. is carried out for 20 hours, and then the catalyst performance is continued to be fed to test.
[0036] The specific experimental conditions of the comparative examples and catalysts of each embodiment are shown in Table 1 below, and the activity data are shown in Table 2.
[0037] Comparative Example 1
[0038] Preparation of copper-silver bimetallic catalyst (synthesized at 25°C, co-impregnation method, copper-silver mass ratio 1:1)
[0039] This comparative example is the preparation of copper-silver bimetallic catalyst comparative sample 1 synthesized by impregnation method at 25°C, as follows:
[0040] Dissolve a certain amount of silver nitrate (AgNO3) and copper nitrate (Cu(NO3)2·3H2O) in 150 mL of deionized water, stir at room temperature, and avoid light. Then slowly add the corresponding amount of dried fumed silica and stir vigorously for 20 hours in the dark. Rotary evaporate the mixture at 40°C to remove excess water. Dry the obtained solid in an oven at 110°C for 15 hours and calcine it at 400°C in a muffle furnace for 4 hours. Reduce the obtained catalyst at 300°C in H2 for 4 hours before use. The catalyst in this comparative example was reduced at 1.4 h according to the above-mentioned online reduction conditions and catalyst evaluation method. -1 The catalyst remained stable within 250 h. After 20 h of high-temperature heat treatment, the yield decreased by 9.6%, and during the period from 270 h to 500 h, the yield decreased from 32.8% to 6.7%.
[0041] Comparative Example 2
[0042] Preparation of copper-silver bimetallic catalyst (synthesized at 25°C, impregnation method, copper-silver mass ratio 1:1)
[0043] This comparative example is the preparation of copper-silver bimetallic catalyst comparative sample 2 synthesized by impregnation method at 25°C, as follows:
[0044] Preparation of catalyst precursor by ammonia evaporation method:
[0045] Weigh a certain amount of Cu(NO3)2·H2O and dissolve it in 150mL of deionized water, and mix it with a certain volume of ammonia water (25wt.%) to form a copper ammonia solution. After stirring for 30 minutes, a certain amount of silica sol is dripped into the copper ammonia solution at a certain rate and aged for 4 hours, then the solution is heated to 80°C to start ammonia evaporation, and the ammonia evaporation is completed when the pH of the solution drops to 6-7. The mixed solution is filtered and washed with deionized water. The obtained sample is placed in a 110°C oven and dried for 12 hours, and a catalyst precursor with a Cu loading of 10wt.% is obtained after calcining at 400°C in a muffle furnace for 4 hours.
[0046] Preparation of copper-silver bimetallic catalyst:
[0047] Weigh an appropriate amount of catalyst precursor prepared by ammonia evaporation and mix it with a certain amount of deionized water. After vigorous stirring, add a certain amount of AgNO3 and stir for 12 hours at room temperature. Avoid light. Rotary evaporate the mixture at 45°C to remove excess water. Dry the obtained solid in an oven at 110°C for 12 hours, and then calcine it in a muffle furnace at 400°C for 4 hours to obtain the catalyst.
[0048] The catalyst of this comparative example was subjected to the above-mentioned online reduction conditions and catalyst evaluation method in 1.4 h. -1 The catalyst remained stable within 250 h. After 20 h of high-temperature heat treatment, the yield decreased by 8.7%, and during the period from 270 h to 500 h, the yield decreased from 39.2% to 12.0%.
[0049] Example 1
[0050] Preparation of copper-silver bimetallic catalyst (synthesized at -80℃, displacement method, copper-silver mass ratio 7:5, H2 reduction)
[0051] This comparative example is to use H2 to reduce the catalyst precursor at -80°C, and to prepare the copper-silver bimetallic catalyst sample 1 synthesized by the replacement method, as follows:
[0052] Preparation of catalyst precursor by ammonia evaporation method:
[0053] Weigh 6.8g of Cu(NO3)2·H2O and dissolve it in 150mL of deionized water, and mix it with 27.3mL of ammonia water (ammonia water concentration is 25wt.%) to form a copper ammonia solution. After stirring for 30min, 44.5mL of silica sol is dripped into the copper ammonia solution at a certain rate (slowly dripped, such as: 1 drop per second, etc.) and aged for 4h, then the solution is heated to 80℃ to start ammonia evaporation, and the ammonia evaporation is completed when the pH of the solution drops to 6-7. The mixed solution is filtered and washed with deionized water (using a Buchner funnel). The obtained sample is placed in a 110℃ oven and dried for 12h, and calcined in a muffle furnace at 400℃ for 4h to obtain a catalyst precursor with a Cu loading of 10wt.%.
[0054] Preparation of copper-silver bimetallic catalyst:
[0055] The catalyst precursor obtained by the ammonia evaporation method was placed in a H2 atmosphere at 300°C for reduction for 4 hours. Then 0.2 g of AgNO3 was weighed and dissolved in a small amount of deionized water to obtain a mixed solution for later use.
[0056] A certain volume of ethanol was added to a three-necked flask, and the flask was connected to a Schlenk line and flushed with nitrogen at room temperature to remove the air in the system. Then 2 g of the reduced catalyst precursor was added, and the temperature of the mixed solution was lowered to -80°C by liquid nitrogen and isopropanol, and a certain volume of AgNO3 solution (the above-prepared solution, mass ratio Cu: Ag = 7: 5) was added, and attention was paid to avoiding light. After stirring and mixing for 90 minutes, the mixed solution was filtered and washed with deionized water, and finally the obtained sample was placed in a 110°C oven for 12 hours (vacuum drying) to obtain the catalyst.
[0057] The catalyst in this embodiment was subjected to the above-mentioned online reduction conditions and catalyst evaluation method in 1.4 h. -1 The catalyst remained stable within 250 h. After 20 h of high-temperature heat treatment, the yield decreased by 8.7% and remained basically stable at 70.1% from 270 h to 500 h.
[0058] Example 2
[0059] Preparation of copper-silver bimetallic catalyst (synthesized at -80℃, displacement method, copper-silver mass ratio 1:1, H2 reduction)
[0060] This comparative example is the preparation of copper-silver bimetallic catalyst sample 2 synthesized by replacement method at -80°C. The difference between this comparative example and the preparation of copper-silver bimetallic catalyst sample 1 in Example 1 is that the copper-silver mass ratio of the copper-silver bimetallic catalyst prepared in this example is 1:1 during the preparation process, as follows:
[0061] The catalyst precursor obtained by the ammonia evaporation method was placed in a H2 atmosphere at 300°C for reduction for 4 hours. Then a certain amount of AgNO3 was weighed and dissolved in a small amount of deionized water to obtain a mixed solution for later use.
[0062] A certain volume of ethanol was added to a three-necked flask, and the flask was connected to a Schlenk line and flushed with nitrogen at room temperature to remove the air in the system. Then a certain amount of reduced catalyst precursor was added, the temperature of the mixed solution was lowered to -80°C by liquid nitrogen and isopropanol, and a certain volume of AgNO3 solution (the above-prepared AgNO3 solution, mass ratio Cu: Ag = 1:1) was added, and attention was paid to avoiding light. After stirring and mixing for 90 minutes, the mixed solution was filtered and washed with deionized water, and finally the obtained sample was placed in a 110°C oven to dry for 12 hours to obtain the catalyst.
[0063] The catalyst of this example was subjected to the above-mentioned online reduction conditions and catalyst evaluation method in 1.4 h. -1 The catalyst remained stable within 250 h. After 20 h of high-temperature heat treatment, the yield decreased by 8.2% and remained basically stable at 82.5% from 270 h to 500 h.
[0064] Example 3
[0065] Preparation of copper-silver bimetallic catalyst (synthesized at 25°C, displacement method, copper-silver mass ratio 1:1, H2 reduction)
[0066] This example is the preparation of copper-silver bimetallic catalyst sample 3, which is different from the preparation of copper-silver bimetallic catalyst sample 2 in Example 2 in that the copper-silver bimetallic catalyst prepared in this example is synthesized at 25° C. The preparation process is as follows:
[0067] The catalyst precursor obtained by the ammonia evaporation method was placed in a H2 atmosphere at 300°C for reduction for 4 hours. Then a certain amount of AgNO3 was weighed and dissolved in a small amount of deionized water to obtain a mixed solution for later use.
[0068] A certain volume of ethanol was added to a three-necked flask, and the flask was connected to a Schlenk line and flushed with nitrogen at room temperature to remove the air in the system. Then a certain amount of reduced catalyst precursor was added, and then a certain volume of AgNO3 solution (the above-prepared AgNO3 solution, mass ratio Cu: Ag = 1:1) was added, and attention was paid to avoiding light. After stirring and mixing for 90 minutes, the mixed solution was filtered and washed with deionized water, and finally the obtained sample was placed in a 110°C oven to dry for 12 hours to obtain a catalyst.
[0069] The catalyst of this example was subjected to the above-mentioned online reduction conditions and catalyst evaluation method in 1.4 h. -1 The reaction was carried out under the conditions of 100 % NH 2 O and 10 % NH 2 O. The catalyst yield values are shown in Table 2.
[0070] Example 4
[0071] Preparation of copper-silver bimetallic catalyst (synthesized at -80℃, displacement method, copper-silver mass ratio 5:7, H2 reduction)
[0072] This example is the preparation of copper-silver bimetallic catalyst sample 4, which is different from the preparation of copper-silver bimetallic catalyst sample 3 in Example 3 in that the copper-silver bimetallic catalyst prepared in this example is synthesized at -80°C, and the mass ratio of copper to silver is 5:7 during the preparation process. The preparation process is as follows:
[0073] The catalyst precursor obtained by the ammonia evaporation method was placed in a H2 atmosphere at 300°C for reduction for 4 hours. Then a certain amount of AgNO3 was weighed and dissolved in a small amount of deionized water to obtain a mixed solution for later use.
[0074] A certain volume of ethanol was added to a three-necked flask, and the flask was connected to a Schlenk line and flushed with nitrogen at room temperature to remove the air in the system. Then a certain amount of reduced catalyst precursor was added, the temperature of the mixed solution was lowered to -80°C by liquid nitrogen and isopropanol, and a certain volume of AgNO3 solution (the above-prepared AgNO3 solution, mass ratio Cu: Ag = 5:7) was added, and attention was paid to avoiding light. After stirring and mixing for 90 minutes, the mixed solution was filtered and washed with deionized water, and finally the obtained sample was placed in a 110°C oven to dry for 12 hours to obtain the catalyst.
[0075] The catalyst of this example was subjected to the above-mentioned online reduction conditions and catalyst evaluation method in 1.4 h. -1 The reaction was carried out under the conditions of 100 % NH 2 O and 10 % NH 2 O. The catalyst yield values are shown in Table 2.
[0076] Example 5
[0077] Preparation of copper-silver bimetallic catalyst (synthesized at -80℃, displacement method, copper-silver mass ratio 7:5, NaBH4 reduction)
[0078] This example is the preparation of copper-silver bimetallic catalyst sample 5, which is different from the preparation of copper-silver bimetallic catalyst sample 4 in Example 4 in that the copper-silver bimetallic catalyst prepared in this example is prepared by reducing the catalyst precursor with NaBH4 during the preparation process. The preparation process is as follows:
[0079] The catalyst precursor obtained by the ammonia evaporation method was placed in excess NaBH4 for reduction for 4 hours. Then a certain amount of AgNO3 was weighed and dissolved in a small amount of deionized water to obtain a mixed solution for later use.
[0080] A certain volume of ethanol was added to a three-necked flask, and the flask was connected to a Schlenk line and flushed with nitrogen at room temperature to remove the air in the system. Then a certain amount of reduced catalyst precursor was added, the temperature of the mixed solution was lowered to -80°C by liquid nitrogen and isopropanol, and a certain volume of AgNO3 solution (the above-prepared AgNO3 solution, mass ratio Cu: Ag = 7:5) was added, and attention was paid to avoiding light. After stirring and mixing for 90 minutes, the mixed solution was filtered and washed with deionized water, and finally the obtained sample was placed in a 110°C oven to dry for 12 hours to obtain the catalyst.
[0081] The catalyst of this example was subjected to the above-mentioned online reduction conditions and catalyst evaluation method in 1.4 h. -1 The reaction was carried out under the conditions of 100 % NH 2 O and 10 % NH 2 O. The catalyst yield values are shown in Table 2.
[0082] Example 6
[0083] Preparation of copper-silver bimetallic catalyst (synthesized at -80℃, displacement method, copper-silver mass ratio 7:5, N2H4 reduction)
[0084] This example is the preparation of copper-silver bimetallic catalyst sample 6, which is different from the preparation of copper-silver bimetallic catalyst sample 5 in Example 5 in that the copper-silver bimetallic catalyst prepared in this example is prepared by reducing the catalyst precursor with N2H4 during the preparation process. The preparation process is as follows:
[0085] The catalyst precursor obtained by the ammonia evaporation method was placed in excess N2H4 for reduction for 4 hours. Then a certain amount of AgNO3 was weighed and dissolved in a small amount of deionized water to obtain a mixed solution for later use.
[0086] A certain volume of ethanol was added to a three-necked flask, and the flask was connected to a Schlenk line and flushed with nitrogen at room temperature to remove the air in the system. Then a certain amount of reduced catalyst precursor was added, the temperature of the mixed solution was lowered to -80°C by liquid nitrogen and isopropanol, and a certain volume of AgNO3 solution (the above-prepared AgNO3 solution, mass ratio Cu: Ag = 7:5) was added, and attention was paid to avoiding light. After stirring and mixing for 90 minutes, the mixed solution was filtered and washed with deionized water, and finally the obtained sample was placed in a 110°C oven to dry for 12 hours to obtain the catalyst.
[0087] The catalyst of this example was subjected to the above-mentioned online reduction conditions and catalyst evaluation method in 1.4 h. -1 The reaction was carried out under the conditions of 100 % NH 2 O and 10 % NH 2 O. The catalyst yield values are shown in Table 2.
[0088] It can be seen from Comparative Examples 1, 2 and Example 3 that the catalyst in Comparative Example 1 is synthesized by co-impregnation method, and the catalyst activity is very low, the selectivity is only 46.4%, and the yield is only 42.4%. The catalyst in Comparative Example 2 is synthesized by impregnation method, and the catalyst activity is low, the selectivity is 48.7%, and the yield is only 47.9%. In Example 2, the copper-silver bimetallic catalyst is synthesized by replacement method, so that the catalyst activity is increased, the selectivity is increased to 71.4%, the MG yield is increased to 68.6%, and the space-time yield is increased from 6.1 g·g cat -1 ·h -1 Increased to 9.9 g·g cat -1 ·h -1 Therefore, the replacement method is used in the preparation process of the copper-silver bimetallic catalyst, which can better anchor the copper species and the silver species through strong interactions, enhance the catalyst activity, improve the directional selectivity of methyl glycolate, enhance the stability of the catalyst, and reduce the cost of catalyst replacement in industrial applications.
[0089] It can be seen from Examples 1, 2, and 4 that Examples 1, 2, and 4 are catalysts synthesized by changing the copper-silver mass ratio during the preparation process. Under different copper-silver mass ratios, the catalyst selectivity and MG yield have changed, so different copper-silver mass ratios have different effects on the synthesis of copper-silver bimetallic catalysts.
[0090] It can be seen from Examples 1, 5 and 6 that the reduction conditions of the catalyst precursor were changed during the preparation process. Under different reduction conditions, the catalyst selectivity and MG yield also changed, indicating that the reduction conditions also have a certain influence on the preparation process.
[0091] It can be seen from Examples 2 and 3 that the replacement reaction synthesis temperature of the copper-silver bimetallic catalyst in Examples 2 and 3 changed during the preparation process, and the MG yield and space-time yield of the prepared catalysts under the reaction conditions were also different, indicating that the synthesis temperature has an effect on the preparation of the copper-silver bimetallic catalyst.
[0092] Table 1 Preparation conditions and particle size of each catalyst
[0093]
[0094] Table 2 Activity data of various catalysts for heterogeneous hydrogenation of dimethyl oxalate
[0095]
[0096] By comparative examples 1, 2 and embodiment 3 in Table 1-2 and Figure 1 It can be seen that the replacement method is the best synthesis method. This is because when the co-impregnation method is used, there is no strong interaction between the Cu species and the catalyst carrier, and it cannot be completely anchored on the catalyst surface. When the impregnation method is used to load Ag, the Ag species is randomly located on the surface of the catalyst precursor and is not completely anchored to the copper species. The combination between the two metals is poor. Figure 1 It can be seen that the replacement method anchors Ag on the surface of Cu, and copper and silver form a core-shell structure, which synergistically catalyzes the hydrogenation of DMO.
[0097] It can be seen from Examples 1, 2, and 4 in Table 1-2 that during the preparation process, Cu:Ag=1:1 has the best effect. This is because when the Ag content is low, all the metal Cu species cannot be coated with Ag, resulting in a low catalytic selectivity of the catalyst, while when the Ag content is high, the Ag species agglomerate during the replacement process, the Ag nanoparticles grow, and Cu cannot be coated with Ag, so Cu:Ag=1:1 has the best effect.
[0098] By Examples 1, 5, 6 and Figure 2It can be seen that the catalyst precursor has the best effect when it is reduced by H2. Because in the process of catalyst precursor reduction, N2H4 as a reducing agent will cause the agglomeration of copper particles and reduce the catalyst activity. Although NaBH4 as a reducing agent will not cause large agglomeration of copper particles, it will introduce B elements and may affect the subsequent preparation of copper-silver bimetallic catalysts. When reduced by H2, copper particles will not agglomerate and no new elements will be introduced. Therefore, the catalyst precursor has the best effect when it is reduced by H2.
[0099] By Examples 2, 3 and Figure 3 It can be seen that low-temperature synthesis has the best effect in the preparation process. Because the temperature decreases, the replacement reaction rate decreases, the replacement between the two metals becomes milder, the particle size of the obtained bimetallic particles decreases, and the degree of dispersion increases. Therefore, low-temperature synthesis has the best effect in the preparation process, and Figure 3 It can be seen that low temperature synthesis makes the catalyst more stable.
[0100] The present invention synthesizes the copper-silver bimetallic catalyst by replacement method, which has the characteristics of mild conditions, simple preparation process, easy raw materials, low cost, excellent catalytic performance, etc. When actually applied to industry, it can be used alone for the production of methyl glycolate with high economic value and high demand, and can still maintain a methyl glycolate yield of more than 90% at a higher space velocity. In addition, the stability of the catalyst is greatly improved, the life of the catalyst is greatly increased, the loss caused by industrial catalyst replacement is reduced, and its industrialization cost is reduced.
Claims
1. A catalyst for preparing methyl glycolate by hydrogenating dimethyl oxalate, the catalyst being a copper-silver bimetallic catalyst, characterized in that: The catalyst comprises a carrier and active components. The active components are copper species and silver species. The carrier is silicon dioxide. The silver species accounts for 1-10 wt. % of the total mass of the catalyst, and the copper species accounts for 1-10 wt. % of the total mass of the catalyst.
2. The catalyst for preparing methyl glycolate by hydrogenating dimethyl oxalate according to claim 1, characterized in that: The specific surface area of the catalyst is 50-300m 2 / g, average pore volume is 0.4-1.7cm 3 / g, and the average pore size is 5-30nm.
3. The catalyst for preparing methyl glycolate by hydrogenating dimethyl oxalate according to claim 2, characterized in that: The structure of the catalyst is that the silver species covers the surface of the copper species in the form of a shell layer to form a core-shell structure. The preferred solution is: The core-shell structure is deposited on the carrier silica in the form of particles, wherein copper forms a strong interaction with silica.
4. The catalyst for preparing methyl glycolate by hydrogenating dimethyl oxalate according to claim 3, characterized in that: The particle size of the copper-silver bimetal is 1.0-10 nm, and the thickness of the silver shell layer is 0.2-2 nm. The preferred solution is: The particle size of the copper-silver bimetal is 1.0-8 nm, and the thickness of the silver shell is 0.2-1 nm.
5. A method for preparing a catalyst for preparing methyl glycolate by hydrogenating dimethyl oxalate as claimed in claim 1, 2, 3 or 4, characterized in that: It includes the following steps: Dissolve copper salt in water, add ammonia water, stir evenly and then drop silica sol; After aging treatment, the temperature is raised to evaporate ammonia, and after completion, it is filtered and washed; The washed product is dried and then calcined to obtain a catalyst precursor, which is then subjected to reduction treatment; The catalyst precursor is mixed with silver nitrate and ethanol, and the copper and silver particles are extracted after centrifugation. The finished catalyst product is obtained after washing and drying.
6. The method for preparing a catalyst for preparing methyl glycolate by hydrogenating dimethyl oxalate according to claim 5, characterized in that: The aging treatment time is 4 hours, and the temperature of the ammonia evaporation is 80 degrees Celsius.
7. The method for preparing a catalyst for preparing methyl glycolate by hydrogenating dimethyl oxalate according to claim 5, characterized in that: The drying conditions of the washed product are: temperature of 80-130 degrees Celsius, and drying time of 12-24 hours.
8. The method for preparing a catalyst for preparing methyl glycolate by hydrogenating dimethyl oxalate according to claim 5, characterized in that: For the reduction treatment, any one of H2, NaBH4 or N2H4 is used.
9. The method for preparing a catalyst for preparing methyl glycolate by hydrogenating dimethyl oxalate according to claim 5, 6, 7 or 8, characterized in that: The temperature of the catalyst precursor after mixing with silver nitrate and ethanol is room temperature or -50 to -110 degrees Celsius. The preferred solution is: The copper salt is copper nitrate. The preferred solution is: The mass ratio of copper to silver is any one of 7:5, 1:1 or 5:
7.
10. Use of the catalyst for hydrogenating dimethyl oxalate to methyl glycolate as claimed in claim 1, 2, 3 or 4, characterized in that: The catalyst is used for catalyzing the selective hydrogenation of dimethyl oxalate to produce methyl glycolate; Specifically, the mixed gasified dimethyl oxalate and hydrogen are introduced into a reactor encapsulated with the copper-silver bimetallic catalyst to react; The reaction pressure is 0.5-3.5MPa; the reaction temperature is 180-240℃; the mass space velocity of dimethyl oxalate is 0.1-4.0h -1 ; The hydrogen ester molar ratio is 60-150. The preferred solution is: An application of a catalyst prepared by the method for preparing a catalyst for hydrogenating dimethyl oxalate to methyl glycolate as claimed in claim 9, characterized in that: The catalyst is used for catalyzing the selective hydrogenation of dimethyl oxalate to produce methyl glycolate; Specifically, the mixed gasified dimethyl oxalate and hydrogen are introduced into a reactor encapsulated with the copper-silver bimetallic catalyst to react; The reaction pressure is 0.5-3.5MPa; the reaction temperature is 180-240℃; the mass space velocity of dimethyl oxalate is 0.1-4.0h -1 ; The hydrogen ester molar ratio is 60-150.
Citation Information
Patent Citations
Preparation method and application of copper-silver bimetallic catalyst
CN113856700A
Dimethyl oxalate hydrogenation catalyst as well as preparation method and application thereof
CN114054041A
Preparation method of catalyst for preparing methyl glycolate through selective hydrogenation of dimethyl oxalate
CN114849705A
Preparation method and application of dimethyl oxalate selective hydrogenation catalyst
CN115007172A
Copper-based catalyst for catalytic hydrogenation of dimethyl oxalate as well as preparation method and application of copper-based catalyst
CN116078399A
Cited By
Catalyst and preparation method thereof, and preparation method of methyl glycolate
CN120771891A
Catalyst, process for its preparation and process for the preparation of methyl glycolate
CN120771891B
Selective hydrogenation reaction Ag-based catalyst and preparation method thereof
CN121372399A
Copper-gallium bimetallic silicon-based carrier catalyst and preparation method and application thereof
CN121892149A